Copper-bismuth catalyst for synthesizing 1, 4-butynediol and preparation method of copper-bismuth catalyst
By first re-adding and then adding precipitation and regulating the aging process, a copper bismuth catalyst with a multi-layer core-shell structure is formed, and the problems of small particle size and poor wear resistance of the unsupported copper bismuth catalyst are solved, thus achieving controllable particle size and particles The distribution is evenly improved, and the activity and life of the catalyst is improved.
Patent Information
- Application Number
- CN202411307720.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-12-06
AI Technical Summary
In the production of existing 1,4-butynylene glycol, the uneven particle size of the copper bismuth catalyst has a small particle size, poor wear resistance, resulting in a short catalyst life and a blockage of the filter cloth, affecting the process efficiency.
The copper bismuth mixed salt solution and alkali solution are prepared by the precipitation method of reverse addition first and then combined addition, and the precipitation reaction conditions and aging process are controlled. The crystal growth is regulated by adding bicarbonate solution to form a copper bismuth catalyst with a multi-layer core-shell structure. Ensure controllable particle size and uniform particle distribution.
The particle size of the copper bismuth catalyst is controlled and the particle distribution is uniform, the mechanical wear resistance and activity of the catalyst is improved, the catalyst life is extended, and the influence of organic matter residues on the reaction is avoided.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalyst preparation, and specifically relates to a copper-bismuth catalyst for synthesizing 1,4-butynediol and a preparation method thereof. Background Art
[0002] At present, there are three main industrialized 1,4-butanediol production process routes, namely, formaldehyde acetylation (Reppe method), maleic anhydride method and bioconversion method. Among them, the formaldehyde acetylation method for producing 1,4-butanediol has the highest market share. Domestic and foreign 1,4-butanediol production units all adopt the improved formaldehyde acetylation production process, among which the representative process technologies are INVISTA process, ISP process, FRONTECH process and Shanxi three-dimensional process. Compared with traditional formaldehyde acetylation, the improved formaldehyde acetylation is carried out in a slurry bed under low pressure of 0.10-0.13MPa and low temperature of 90-100℃, and the catalysts are mainly Cu2(OH)2CO3, CuO / SiO2 and CuO-Bi2O3 / MgSiO3.
[0003] At present, the INVISTA process accounts for the largest proportion of existing formaldehyde acetylene production 1,4-butanediol units, which uses an unsupported basic copper carbonate copper bismuth catalyst. The unsupported basic copper carbonate copper bismuth catalyst has the advantages of good selectivity and high conversion rate, but has poor mechanical wear resistance and is easily damaged to produce small particles, causing filter cloth blockage and thus reducing the catalyst life.
[0004] The main method to improve the mechanical wear resistance of unsupported basic copper carbonate type copper bismuth catalyst is to increase the particle size of the catalyst particles and ensure that the particle size distribution of the catalyst is uniform. In order to improve the particle size and distribution uniformity of the catalyst, some processes add additives during the catalyst preparation process. For example, invention patents CN106669697B, CN106669698B, CN106669688B, etc. all use a variety of organic substances as additives to increase the particle size of the catalyst. However, during the catalyst preparation process, the added additives are likely to remain in the catalyst, affecting the synthesis reaction of 1,4-butynediol, and easily enter the subsequent 1,4-butanediol production process.
[0005] In summary, the unsupported copper-bismuth catalyst for producing 1,4-butynediol in the prior art still has technical problems such as small catalyst particle size, uneven particle size, and poor catalyst wear resistance. Summary of the invention
[0006] The purpose of the present invention is to address the deficiencies of the prior art and provide a copper-bismuth catalyst for synthesizing 1,4-butynediol and a preparation method thereof. The catalyst prepared by the method is a multilayer core-shell copper-bismuth catalyst for synthesizing 1,4-butynediol from formaldehyde and acetylene in a slurry bed, which is a multilayer core-shell copper-bismuth catalyst having the advantages of controllable particle size, uniform particle distribution, good activity, and no organic residue.
[0007] In order to achieve the purpose of the present invention, the specific technical scheme of the present invention is as follows:
[0008] A method for preparing a copper-bismuth catalyst for synthesizing 1,4-butynediol comprises the following steps:
[0009] (1) dissolving a soluble copper salt and a soluble bismuth salt in a certain amount of an acidic solution to prepare a copper-bismuth mixed salt solution with a concentration of 0.5 mol / L to 2.0 mol / L;
[0010] (2) dissolving a soluble alkali in a certain amount of pure water to prepare an alkali solution with a concentration of 0.5 mol / L to 2.0 mol / L;
[0011] (3) adding the copper and bismuth mixed solution in step (1) and the alkaline solution in step (2) dropwise into the reaction kettle by a precipitation method of first back-addition and then addition, and performing a precipitation reaction at a reaction temperature of 15° C. to 60° C. and a stirring speed of 250 rpm to 500 rpm;
[0012] (4) After the precipitation is completed, a certain amount of a bicarbonate solution with a concentration of 0.01 mol / L to 0.1 mol / L is added to the reaction kettle in step (3), and then the reaction temperature is increased to 70° C. to 90° C. to start aging for 2 to 6 hours;
[0013] (5) After aging, the solution is filtered, washed, and dried to obtain copper-bismuth precursor I;
[0014] (6) According to steps (1), (2) and (3), secondary feeding and precipitation are carried out. After the precipitation is completed, the copper-bismuth precursor I obtained in step (5) is added into the reaction kettle in a certain mass ratio, and the reaction temperature is increased to 70° C. to 90° C. to start aging, and the aging time is 2 to 6 hours.
[0015] (7) After aging, the solution is filtered and washed to obtain a copper-bismuth precursor II, and the copper-bismuth precursor II is slurried with water in a mass ratio to prepare a slurry;
[0016] (8) The slurry in step (7) is subjected to spray granulation to obtain a copper-bismuth catalyst for synthesizing 1,4-butynediol.
[0017] As a preferred embodiment of the present invention, the soluble copper salt in step (1) is one or more of copper nitrate, copper sulfate, copper acetate, and copper chloride, and more preferably is bismuth nitrate.
[0018] As a preferred embodiment of the present invention, the soluble bismuth salt described in step (1) is one or more of bismuth nitrate, bismuth sulfate, bismuth acetate, and bismuth chloride, more preferably bismuth nitrate.
[0019] As a preferred embodiment of the present invention, the acidic solution in step (1) is one or more of nitric acid, sulfuric acid, and hydrochloric acid, more preferably nitric acid.
[0020] As a preferred embodiment of the present invention, the soluble alkali in step (2) is one or more of sodium carbonate, sodium hydroxide, potassium carbonate, potassium hydroxide, ammonium carbonate, ammonium bicarbonate, ammonia water, and sodium bicarbonate, more preferably sodium carbonate.
[0021] As a better embodiment of the present invention, the precipitation method of first adding back in step (3) is: by volume, first add one quarter to one half of the alkali solution into the reactor, and then add an equal volume of copper and bismuth mixed solution into the reactor. Then continue to add the remaining alkali solution and copper and bismuth mixed solution to the reactor at the same time, and control the pH of the precipitation process to be 6-7. The precipitation method has a great influence on the particle size and distribution uniformity of the copper-bismuth catalyst. The precursor prepared by the precipitation method of adding back has a poor particle size distribution, but the precursor prepared under the same preparation conditions has a good repeatability in particle size and particle size distribution. The precursor prepared by the precipitation method of adding together has a better particle size distribution, but the basic physical property parameters of the precursor prepared under the same conditions have poor repeatability. Therefore, the precursor prepared by the precipitation method of first adding back and then adding together has a good particle size distribution and good continuous production repeatability.
[0022] As a preferred embodiment of the present invention, the bicarbonate in step (4) is one or more of sodium bicarbonate, potassium bicarbonate, and ammonium bicarbonate, more preferably sodium bicarbonate.
[0023] As a preferred embodiment of the present invention, the molar ratio of the bicarbonate in step (4) to the soluble base in step (2) is 1:10 to 1:100 (specifically 1:10, 1:20, 1:30, 1:40, 1:50, 1:60, 1:70, 1:80, 1:90, 1:100, etc.).
[0024] The present invention also protects a copper-bismuth catalyst for synthesizing 1,4-butynediol prepared by any of the above methods or a reasonable combination of method steps.
[0025] The present invention also protects the use of the copper-bismuth catalyst for synthesizing 1,4-butynediol described above in synthesizing 1,4-butynediol from formaldehyde and acetylene in a slurry bed.
[0026] After the copper and bismuth mixed solution is precipitated with the alkaline solution, Cu3(CO3)2(OH)2 precipitate is first generated, and then during the aging process, the Cu3(CO3)2(OH)2 precipitate gradually transforms into a fixed form of Cu2CO3(OH)2, as shown in the following chemical equation:
[0027] 3Na2CO3+3Cu(NO3)2+H2O=Cu3(CO3)2(OH)2↓+6NaNO3+CO2↑
[0028] 2Cu3(CO3)2(OH)2+H2O=3Cu2CO3(OH)2+CO2↑
[0029] The growth of Cu2CO3(OH)2 crystals is mainly controlled by two steps: the nucleation process and the nucleus growth process. In the existing process, the main reason for the small particle size and uneven distribution of copper-bismuth catalysts is that the solution is in an oversaturated state during the aging process, and a large number of Cu2CO3(OH)2 crystals are nucleated, and there is not enough space and time for crystal growth. The chemical equation of the aging process is split into two ionic equations as shown below:
[0030] CO3 2- +H2O=CO2+2(OH) -
[0031] 2Cu3(CO3)2(OH)2+2(OH) - =3Cu2CO3(OH)2+CO3 2-
[0032] According to the ionic equation, it can be found that the carbonate hydrolysis process is the controlling step of the aging process. By adding bicarbonate solution to the precipitation solution, the carbonate hydrolysis process can be slowed down and the solution saturation can be reduced, thereby allowing the Cu2CO3(OH)2 crystals to grow fully, and finally obtaining a copper-bismuth precursor with larger particle size and more uniform distribution.
[0033] As a preferred embodiment of the present invention, the addition ratio of the copper-bismuth precursor I in step (6) is the ratio of the mass of the copper-bismuth precursor I to the theoretical mass of the copper-bismuth precipitate, which ranges from 1:1 to 1:19. Adding the copper-bismuth precursor I to the copper-bismuth precipitate can make the Cu2CO3(OH)2 crystals grow along the surface of the copper-bismuth precursor I to form a multi-layer core-shell structure, further increasing the particle size of the copper-bismuth precursor II. By controlling the ratio of the copper-bismuth precursor I to the theoretical mass of the copper-bismuth precipitate, the particle size of the copper-bismuth precursor II can be controlled.
[0034] As a preferred embodiment of the present invention, in step (7), the mass ratio of the copper-bismuth precursor to water is 1:3 to 11:9 (specifically 1:3, 1:2, 1:1, 11:9, etc.).
[0035] In the method, a feeding method of first back-adding and then adding together is adopted to obtain a copper-bismuth precursor with stable quality, good production repeatability and uniform particle size distribution. Then, a bicarbonate solution is added during the aging process of the copper-bismuth precursor to regulate the crystal growth rate of the copper-bismuth precursor, thereby obtaining a copper-bismuth precursor with a larger particle size and a more uniform distribution. The copper-bismuth precursor is added during the aging process to obtain a multi-layer core-shell copper-bismuth precursor with controllable particle size. Finally, a copper-bismuth catalyst is obtained after spray granulation.
[0036] Compared with the prior art, the present invention has the following beneficial effects:
[0037] (1) The preparation method provided by the present invention can first obtain a copper-bismuth precursor I with stable quality, good production repeatability and uniform particle size distribution by a feeding method of first back-adding and then adding. Then, by adding a bicarbonate solution during the aging process of the copper-bismuth precursor I, the crystal growth rate of the copper-bismuth precursor I is regulated, thereby obtaining a copper-bismuth precursor II with a larger particle size and more uniform distribution. Finally, by adding the copper-bismuth precursor I during the aging process, a copper-bismuth precursor II with controllable particle size is obtained. After spray granulation, the copper-bismuth catalyst obtained has a controllable particle size, uniform particle distribution and good activity.
[0038] (2) The preparation method provided by the present invention does not add an organic solvent during the preparation of the catalyst, and will not cause adverse effects on the synthesis reaction of 1,4-butynediol and downstream processes. DETAILED DESCRIPTION
[0039] All features disclosed in this specification, or steps in all methods or processes disclosed, except mutually exclusive features and / or steps, can be combined in any manner.
[0040] Any feature disclosed in this specification (including claims and abstract), unless otherwise stated, may be replaced by other equivalent or alternative features having similar purposes. That is, unless otherwise stated, each feature is only an example of a series of equivalent or similar features.
[0041] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0042] All the following raw materials are commercially available products; % not otherwise specified indicates the mass percentage, i.e. wt%.
[0043] Embodiment 1:
[0044] This embodiment provides a copper-bismuth catalyst for synthesizing 1,4-butynediol and a preparation method thereof, which specifically comprises the following steps:
[0045] Weigh 11.89kg of copper nitrate trihydrate and 0.39kg of bismuth nitrate pentahydrate, dissolve them in dilute nitric acid to prepare a copper and bismuth mixed salt solution with a concentration of 0.5mol / L. Weigh 7.18kg of anhydrous sodium carbonate and dissolve them in pure water to prepare an alkaline solution with a concentration of 0.68mol / L. First, use the reverse feeding method to add 50L of alkaline solution into the reactor, and add an equal volume of copper and bismuth mixed salt solution at a reaction temperature of 20°C and a stirring speed of 250rpm. Then, use the feeding method of adding and dropping the remaining copper, bismuth mixed salt solution and alkaline solution at the same time, and control the pH to 6-7. After the feed precipitation is completed, add 200L of bicarbonate solution with a concentration of 0.03mol / L into the reactor, and then start aging at 80°C for 3h; after the aging is completed, filter, wash and dry the solution to obtain a green precipitate, i.e., copper-bismuth precursor I.
[0046] Weigh 11.89kg of copper nitrate trihydrate and 0.39g of bismuth nitrate pentahydrate, dissolve them in dilute nitric acid to prepare a copper and bismuth mixed salt solution with a concentration of 0.5mol / L. Weigh 7.18kg of anhydrous sodium carbonate and dissolve them in pure water to prepare an alkaline solution with a concentration of 0.68mol / L. First, use the reverse feeding method to add 50L of alkaline solution into the reactor, and add an equal volume of copper and bismuth mixed salt solution at a reaction temperature of 20°C and a stirring speed of 250rpm. Then, use the feeding method of adding and dropping the remaining copper, bismuth mixed salt solution and alkaline solution at the same time, and control the pH to 6-7. After the feed precipitation is completed, add 4.06kg of green precipitate to the reactor, and then start aging at 80°C for 3h. After the aging is completed, the solution is filtered and washed to obtain a new green precipitate (i.e., copper-bismuth precursor II), which is slurried with water at a mass ratio of 1:3 to prepare a slurry, and spray granulation is performed to obtain a copper-bismuth catalyst.
[0047] The results of the measurement using the LS-POP(9) / 609 laser particle size analyzer showed that the average particle size of the catalyst was D50 = 21.52 μm, and the percentage of particles smaller than 7 μm was less than 1%.
[0048] Example 2
[0049] Weigh 21.42kg of copper nitrate trihydrate and 0.66kg of bismuth nitrate pentahydrate, dissolve them in dilute nitric acid to prepare a copper and bismuth mixed salt solution with a concentration of 1.4mol / L. Weigh 12.16kg of anhydrous sodium carbonate and dissolve them in pure water to prepare an alkaline solution with a concentration of 1.7mol / L. First, use the reverse feeding method to add 25L of alkaline solution into the reactor, and add an equal volume of copper and bismuth mixed salt solution at a reaction temperature of 45°C and a stirring speed of 300rpm. Then, use the feeding method of adding and dropping the remaining copper and bismuth mixed salt solution and alkaline solution at the same time, and control the pH to 6-7. After the feed precipitation is completed, add 150L of bicarbonate solution with a concentration of 0.05mol / L into the reactor, and then start aging at 75°C for 5h; after the aging is completed, filter, wash and dry the solution to obtain a green precipitate (i.e., copper-bismuth precursor I).
[0050] Weigh 21.42kg of copper nitrate trihydrate and 0.66kg of bismuth nitrate pentahydrate, dissolve them in dilute nitric acid to prepare a copper and bismuth mixed salt solution with a concentration of 1.4mol / L. Weigh 12.16kg of anhydrous sodium carbonate and dissolve them in pure water to prepare an alkaline solution with a concentration of 1.7mol / L. First, use the reverse feeding method to add 25L of alkaline solution into the reactor, and add an equal volume of copper and bismuth mixed salt solution at a reaction temperature of 45°C and a stirring speed of 300rpm. Then use the feeding method of adding and dropping the remaining salt solution and alkaline solution at the same time to control the pH to 6-7. After the feed precipitation is completed, add 5.08kg of green precipitate to the reactor, and then start aging at 75°C for 5h. After the aging is completed, the solution is filtered and washed to obtain a new green precipitate (i.e., copper-bismuth precursor II), which is slurried with water at a mass ratio of 1:1 to prepare a slurry, and spray granulation is performed to obtain a copper-bismuth catalyst.
[0051] The average particle size of the catalyst measured by LS-POP (9) / 609 laser particle size analyzer was D50 = 21.70 μm, and the percentage of particles smaller than 7 μm was less than 1%.
[0052] Example 3
[0053] Weigh 21.37kg of copper nitrate trihydrate and 0.76kg of bismuth nitrate pentahydrate, dissolve them in dilute nitric acid to prepare a copper and bismuth mixed salt solution with a concentration of 1.5mol / L. Weigh 12.91kg of anhydrous sodium carbonate and dissolve it in pure water to prepare an alkaline solution with a concentration of 2.0mol / L. First, use the reverse feeding method to add 15L of alkaline solution into the reactor, and add an equal volume of copper and bismuth mixed salt solution at a reaction temperature of 50°C and a stirring speed of 250rpm. Then, use the feeding method of adding and dropping the remaining copper and bismuth mixed salt solution and alkaline solution at the same time, and control the pH to 6-7. After the feed precipitation is completed, add 120L of bicarbonate solution with a concentration of 0.02mol / L into the reactor, and then start aging at 75°C for 6h; after the aging is completed, filter, wash and dry the solution to obtain a green precipitate (i.e., copper-bismuth precursor I).
[0054] Weigh 21.37kg of copper nitrate trihydrate and 0.76kg of bismuth nitrate pentahydrate, dissolve them in dilute nitric acid to prepare a copper and bismuth mixed salt solution with a concentration of 1.5mol / L. Weigh 12.91kg of anhydrous sodium carbonate and dissolve them in pure water to prepare an alkaline solution with a concentration of 2.0mol / L. First, use the reverse feeding method to add 15L of alkaline solution into the reactor, and add an equal volume of copper and bismuth mixed salt solution at a reaction temperature of 50°C and a stirring speed of 250rpm. Then, use the feeding method of adding and dropping the remaining copper, bismuth mixed salt solution and alkaline solution at the same time, and control the pH to 6-7. After the feed precipitation is completed, add 2.54kg of green precipitate to the reactor, and then start aging at 75°C for 6h. After the aging is completed, the solution is filtered and washed to obtain a new green precipitate (i.e., copper-bismuth precursor II), which is slurried with water at a mass ratio of 11:9 to prepare a slurry, and spray granulation is performed to obtain a copper-bismuth catalyst.
[0055] The average particle size of the catalyst measured by LS-POP(9) / 609 laser particle size analyzer was D50=20.85 μm, and the percentage of particles smaller than 7 μm was less than 1%.
[0056] Example 4
[0057] Weigh 21.41kg of copper nitrate trihydrate and 0.69kg of bismuth nitrate pentahydrate, dissolve them in dilute nitric acid to prepare a copper and bismuth mixed salt solution with a concentration of 1.2mol / L. Weigh 12.24kg of anhydrous sodium carbonate and dissolve them in pure water to prepare an alkaline solution with a concentration of 1.54mol / L. First, use the reverse feeding method to add 25L of alkaline solution into the reactor, and add an equal volume of copper and bismuth mixed salt solution at a reaction temperature of 30°C and a stirring speed of 500rpm. Then, use the feeding method of adding and dropping the remaining copper and bismuth mixed salt solution and alkaline solution at the same time, and control the pH to 6-7. After the feed precipitation is completed, add 150L of bicarbonate solution with a concentration of 0.04mol / L into the reactor, and then start aging at 90°C for 2h; after the aging is completed, filter, wash and dry the solution to obtain a green precipitate (i.e., copper-bismuth precursor I).
[0058] Weigh 21.41kg of copper nitrate trihydrate and 0.69kg of bismuth nitrate pentahydrate, dissolve them in dilute nitric acid to prepare a copper and bismuth mixed salt solution with a concentration of 1.2mol / L. Weigh 12.24kg of anhydrous sodium carbonate and dissolve them in pure water to prepare an alkaline solution with a concentration of 1.54mol / L. First, use the reverse feeding method to add 25L of alkaline solution into the reactor, and add an equal volume of copper and bismuth mixed salt solution at a reaction temperature of 30°C and a stirring speed of 500rpm. Then, use the feeding method of adding and dropping the remaining copper, bismuth mixed salt solution and alkaline solution at the same time, and control the pH to 6-7. After the feed precipitation is completed, add 2.10kg of green precipitate to the reactor, and then start aging at 90°C for 2h. After the aging is completed, the solution is filtered and washed to obtain a new green precipitate (i.e., copper-bismuth precursor II), which is slurried with water at a mass ratio of 2:3 to prepare a slurry, and spray granulation is performed to obtain a copper-bismuth catalyst.
[0059] The average particle size of the catalyst measured by LS-POP (9) / 609 laser particle size analyzer was D50 = 20.51 μm, and the percentage of particles smaller than 7 μm was less than 1%.
[0060] Example 5
[0061] Weigh 21.48kg of copper nitrate trihydrate and 0.51kg of bismuth nitrate pentahydrate, dissolve them in dilute nitric acid to prepare a copper and bismuth mixed salt solution with a concentration of 0.9mol / L. Weigh 12.88kg of anhydrous sodium carbonate and dissolve them in pure water to prepare an alkaline solution with a concentration of 1.22mol / L. First, use the reverse feeding method to add 50L of alkaline solution into the reactor, and add an equal volume of copper and bismuth mixed salt solution at a reaction temperature of 15°C and a stirring speed of 300rpm. Then, use the feeding method of adding and dropping the remaining copper, bismuth mixed salt solution and alkaline solution at the same time, and control the pH to 6-7. After the feed precipitation is completed, add 300L of bicarbonate solution with a concentration of 0.01mol / L into the reactor, and then start aging at 85°C for 3h; after the aging is completed, filter, wash and dry the solution to obtain a green precipitate (i.e., copper-bismuth precursor I).
[0062] Weigh 21.48kg of copper nitrate trihydrate and 0.51kg of bismuth nitrate pentahydrate, dissolve them in dilute nitric acid to prepare a copper and bismuth mixed salt solution with a concentration of 0.9mol / L. Weigh 12.88kg of anhydrous sodium carbonate and dissolve them in pure water to prepare an alkaline solution with a concentration of 1.22mol / L. First, use the reverse feeding method to add 50L of alkaline solution into the reactor, and add an equal volume of copper and bismuth mixed salt solution at a reaction temperature of 15°C and a stirring speed of 300rpm. Then, use the feeding method of adding and dropping the remaining copper, bismuth mixed salt solution and alkaline solution at the same time, and control the pH to 6-7. After the feed precipitation is completed, add 20.30kg of green precipitate to the reactor, and then start aging at 85°C for 3h. After the aging is completed, the solution is filtered and washed to obtain a new green precipitate (i.e., copper-bismuth precursor II), which is slurried with water at a mass ratio of 3:7 to prepare a slurry, and spray granulation is performed to obtain a copper-bismuth catalyst.
[0063] The average particle size of the catalyst measured by LS-POP (9) / 609 laser particle size analyzer was D50 = 22.33 μm, and the percentage of particles smaller than 7 μm was less than 1%.
[0064] Example 6
[0065] Weigh 21.42kg of copper nitrate trihydrate and 0.66kg of bismuth nitrate pentahydrate, dissolve them in dilute nitric acid to prepare a copper and bismuth mixed salt solution with a concentration of 1.4mol / L. Weigh 12.16kg of anhydrous sodium carbonate and dissolve them in pure water to prepare an alkaline solution with a concentration of 1.7mol / L. First, use the reverse feeding method to add 25L of alkaline solution into the reactor, and add an equal volume of copper and bismuth mixed salt solution at a reaction temperature of 45°C and a stirring speed of 300rpm. Then, use the feeding method of adding and dropping the remaining copper and bismuth mixed salt solution and alkaline solution at the same time, and control the pH to 6-7. After the feed precipitation is completed, aging begins at 75°C for 5h; after the aging is completed, the solution is filtered, washed, and dried to obtain a green precipitate (i.e., copper-bismuth precursor I), which is slurried with water at a mass ratio of 1:1 to prepare a slurry, and spray granulation is performed to obtain a copper-bismuth catalyst.
[0066] The average particle size of the catalyst measured by LS-POP(9) / 609 laser particle size analyzer was D50=25.38 μm, and the percentage of particles smaller than 7 μm was less than 1%.
[0067] Example 7
[0068] Weigh 21.41kg of copper nitrate trihydrate and 0.69kg of bismuth nitrate pentahydrate, dissolve them in dilute nitric acid to prepare a copper and bismuth mixed salt solution with a concentration of 1.2mol / L. Weigh 12.24kg of anhydrous sodium carbonate and dissolve them in pure water to prepare an alkaline solution with a concentration of 1.54mol / L. Adopt a feeding method of adding and dropping the copper and bismuth mixed salt solution and the alkaline solution at the same time, and control the pH = 6-7. After the feed precipitation is completed, add 150L of bicarbonate solution with a concentration of 0.04mol / L into the reactor, and then start aging at 90℃ for 2h; after the aging is completed, filter, wash and dry the solution to obtain a green precipitate (i.e., copper-bismuth precursor I), and mix it with water at a mass ratio of 2:3 to prepare a slurry, spray granulate, and obtain a copper-bismuth catalyst.
[0069] The average particle size of the catalyst measured by LS-POP (9) / 609 laser particle size analyzer was D50 = 14.38 μm, and the percentage of particles smaller than 7 μm was less than 6.5%.
[0070] Experimental example
[0071] The performance of the copper-bismuth catalyst samples prepared in Examples 1-5 was tested. The test results are shown in Table 1.
[0072] Catalyst evaluation conditions:
[0073] 800 ml of 37% formaldehyde aqueous solution was added to a 2L slurry bed reactor, and then 50 g of the prepared copper bismuth catalyst was slurried with 100 g of water and added into the slurry bed reactor and stirring was started. An appropriate amount of sodium bicarbonate was added to adjust the solution pH to 7. At 80°C, acetylene and nitrogen were introduced at flow rates of 14 L / h and 6 L / h, respectively, to activate the catalyst for 9 hours, and then the acetylation reaction was carried out for 7 hours. The product composition was analyzed online using an Agilent 8890 gas chromatograph.
[0074] Table 1 Performance evaluation of copper bismuth catalyst samples for the synthesis of 1,4-butynediol
[0075] sample Formaldehyde conversion rate (%) 1,4-Butynediol selectivity (%) Example 1 97.2 98.1 Example 2 96.7 97.3 Example 3 96.8 97.5 Example 4 97.0 97.8 Example 5 97.5 98.3 Example 6 91.2 94.0 Example 7 95.5 96.2
[0076] The above-mentioned embodiments only express the specific implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the protection scope of the present application. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the technical solution concept of the present application, and these all belong to the protection scope of the present application.
[0077] This background section is provided to generally present the context of the invention, and the work of the presently named inventors, the work to the extent described in this background section, and aspects of this section that did not constitute prior art at the time of application are neither explicitly nor implicitly admitted to be prior art to the present invention.
Claims
1. A method for preparing a copper-bismuth catalyst for synthesizing 1,4-butynediol, It is characterized in that The following steps are involved: (1) dissolving a soluble copper salt and a soluble bismuth salt in a certain amount of an acidic solution to prepare a copper-bismuth mixed salt solution with a concentration of 0.5 mol / L to 2.0 mol / L; (2) dissolving a soluble alkali in a certain amount of pure water to prepare an alkali solution with a concentration of 0.5 mol / L to 2.0 mol / L; (3) adding the copper-bismuth mixed salt solution in step (1) and the alkaline solution in step (2) dropwise into the reaction kettle by a precipitation method of first back-addition and then combined addition, and performing a precipitation reaction at a reaction temperature of 15° C. to 60° C. and a stirring speed of 250 rpm to 500 rpm; (4) After the precipitation reaction is completed, a certain amount of a bicarbonate solution with a concentration of 0.01 mol / L to 0.1 mol / L is added to the reaction kettle in step (3), and then the reaction temperature is increased to 70° C. to 90° C. to start aging for 2 to 6 hours; (5) After aging, the solution is filtered, washed, and dried to obtain copper-bismuth precursor I; (6) performing secondary feeding and precipitation according to steps (1), (2) and (3); after the precipitation, adding the copper-bismuth precursor I obtained in step (5) into the reaction kettle in a certain mass ratio, raising the reaction temperature to 70° C. to 90° C. to start aging, and the aging time is 2 to 6 hours; (7) After aging, the solution is filtered and washed to obtain a copper-bismuth precursor II; the copper-bismuth precursor II is then slurried with water in a mass ratio to prepare a slurry; (8) The slurry in step (7) is subjected to spray granulation to obtain a copper-bismuth catalyst for synthesizing 1,4-butynediol.
2. The preparation method according to claim 1, It is characterized in that The soluble copper salt is one or more of copper nitrate, copper sulfate, copper acetate, and copper chloride; the soluble bismuth salt is one or more of bismuth nitrate, bismuth sulfate, bismuth acetate, and bismuth chloride; and the acidic solution is one or more of nitric acid, sulfuric acid, and hydrochloric acid.
3. The preparation method according to claim 1, It is characterized in that The soluble alkali is one or more of sodium carbonate, sodium hydroxide, potassium carbonate, potassium hydroxide, ammonium carbonate, ammonium bicarbonate, ammonia water, and sodium bicarbonate.
4. The preparation method according to claim 1, It is characterized in that The precipitation method of first back-adding and then adding together is: first adding one quarter to one half of the alkali solution by volume into the reactor, then dropping an equal volume of the copper and bismuth mixed solution into the reactor, and then using the precipitation method of adding together to continue to drop the remaining alkali solution and the copper and bismuth mixed solution into the reactor at the same time after the back-adding, and controlling the pH value of the precipitation process to be 6-7.
5. The preparation method according to claim 1, It is characterized in that The bicarbonate is one or more of sodium bicarbonate, potassium bicarbonate, and ammonium bicarbonate; the molar ratio of the bicarbonate to the soluble alkali in step (2) is 1:10 to 1:
100.
6. The preparation method according to claim 1, It is characterized in that The addition ratio of the copper-bismuth precursor I is the ratio of the mass of the copper-bismuth precursor I to the theoretical mass of the copper-bismuth precipitate, and the range is 1:1 to 1:
19.
7. The preparation method according to claim 1, It is characterized in that The mass ratio of the copper-bismuth precursor II to water is 1:3 to 11:
9.
8. The preparation method according to claim 1, It is characterized in that The soluble copper salt is bismuth nitrate; the soluble bismuth salt is bismuth nitrate; the acidic solution is nitric acid; the soluble alkali is sodium carbonate; and the bicarbonate is sodium bicarbonate.
9. A copper-bismuth catalyst for synthesizing 1,4-butynediol prepared according to any one of claims 1 to 8.
10. Use of the copper-bismuth catalyst for synthesizing 1,4-butynediol according to claim 9 in synthesizing 1,4-butynediol from formaldehyde and acetylene in a slurry bed.