ZnIn2S4 / ZnSn (OH) 6 photocatalyst as well as preparation method and application thereof

By forming a hollow structure in ZnSn(OH)6 photocatalyst and loading ZnIn2S4, the problems of small specific surface area and low light utilization are solved, and efficient electron-hole separation in the visible light band is achieved, which expands the application range and improves the Photocatalytic properties.

CN119076017APending Publication Date: 2024-12-06TIANJIN POLYTECHNIC UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411307902.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing ZnSn(OH)6 photocatalyst has a small specific surface area, low light utilization rate, and no response in the visible light band, and photogenerated electron holes are easy to recombinate, limiting its application range.

Method used

Solid ZnSn(OH)6 crystals were synthesized by co-precipitation method, and hollow ZnSn(OH)6 micronomial material was formed by self-sacrificing template method, followed by in-situ growth of ZnIn2S4 on it to form ZnIn2S4/ZnSn(OH)6 light Catalysts increase the specific surface area and loading point, expand the absorption light band range, and reduce the recombination effect of photogenerated carriers.

Benefits of technology

The photocatalytic performance and light utilization efficiency are significantly improved, so that it can also perform electron-hole separation in the visible light band, expanding the application range.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119076017A_ABST
    Figure CN119076017A_ABST
Patent Text Reader

Abstract

The invention discloses a ZnIn2S4 / ZnSn (OH) 6 photocatalyst as well as a preparation method and application thereof. The preparation method comprises the following steps: 1) synthesizing a solid ZnSn (OH) 6 crystal by adopting a coprecipitation method; (2) eroding the internal structure of the solid ZnSn (OH) 6 crystal by adopting a self-sacrifice template method to form a hollow ZnSn (OH) 6 micro-nano material; and (3) carrying out in-situ growth on ZnIn2S4 on the hollow ZnSn (OH) 6 material, so as to prepare the ZnIn2S4 / ZnSn (OH) 6 photocatalyst. The photocatalytic performance of the photocatalyst is greatly enhanced, the light utilization efficiency is improved, and the application range is expanded.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to, in particular to a ZnIn 2 S 4 / ZnSn(OH) 6 Photocatalyst and its preparation method and application. Background Art

[0002] As the country pays more attention to the control of new pollutants, new antibiotic pollutants have gradually come into people's view. Among them, tetracycline is widely used in infections caused by Gram-positive and Gram-negative bacteria, intracellular mycoplasmas, chlamydia and rickettsia. It is one of the commonly used antibiotics in animal husbandry and aquaculture. The tetracycline-containing wastewater discharged into the environment poses a risk to human health. Clean and efficient photocatalytic technology is an effective way to degrade tetracycline in wastewater.

[0003] New semiconductor photocatalytic material ZnSn(OH) 6 The crystal structure of zinc hydroxystannate is a face-centered cubic perovskite crystal structure. Due to its special crystal structure, its surface is rich in hydroxyl groups. Its unique molecular structure is conducive to reacting with photogenerated carriers during the photocatalytic reaction to form hydroxyl radicals OH, which can become active groups in photocatalytic oxidation reactions. However, the large band gap of zinc hydroxystannate (Eg≈3.7eV) determines that it can only use ultraviolet light, which reduces its light utilization efficiency and narrows its application range. ZnIn 2 S 4 As a visible light photocatalyst, ZnIn has low band gap energy, is stable and easy to prepare, but the problems of poor electron-hole separation efficiency and easy recombination limit the application of ZnIn 2 S 4 For single use. Summary of the invention

[0004] In view of the above defects or deficiencies in the prior art, it is desirable to provide a ZnIn 2 S 4 / ZnSn(OH) 6 Photocatalysts and their preparation methods and applications have greatly enhanced photocatalytic performance, improved light utilization efficiency, and expanded the scope of application.

[0005] The present invention provides a ZnIn 2 S 4 / ZnSn(OH) 6 The method for preparing a photocatalyst comprises the following steps:

[0006] 1) Synthesis of solid ZnSn(OH) by coprecipitation method 6 Crystals;

[0007] 2) Etching the solid ZnSn(OH) using a self-sacrificial template method 6 The internal structure of the crystal forms a hollow ZnSn(OH) 6 Micro-nano materials;

[0008] 3) ZnIn 2 S 4 In the hollow ZnSn(OH) 6 In situ growth was performed on the material to prepare ZnIn 2 S 4 / ZnSn(OH) 6 Photocatalyst.

[0009] Further, in step 1), first take a beaker and add SnCl 4 Add to ethanol and stir for a while to form solvent 1; take another beaker and add (CH3COO) 2 Zn·2H 2 O and sodium dodecyl sulfate, then add deionized water, and stir for a period of time to form solution 2; mix the solution 1 and solution 2 at room temperature to obtain a mixed solution; add NaOH solution dropwise to the mixed solution, stir for a period of time at room temperature, obtain a white product by centrifugation, wash the white product with deionized water and ethanol, and then dry the white product to obtain the solid ZnSn(OH) 6 Crystal.

[0010] Furthermore, in the step 2), the solid ZnSn(OH) 6 The crystals are added to a NaOH solution, stirred at room temperature for a period of time, and then centrifuged to obtain a product, washed with deionized water and ethanol, and then dried to obtain the ZnSn(OH) 6 Hollow micro-nanomaterials.

[0011] Furthermore, in step 3), the hollow ZnSn(OH) 6 The micro-nano material was added into a three-necked flask, deionized water was added into the three-necked flask, and the mixture was stirred rapidly for a period of time for later use; then ZnCl 2 and InCl 3 ·4H 2 O is dissolved in deionized water and stirred for a period of time to form solution A for use; thioacetamide is dissolved in deionized water to form solution B for use;

[0012] Then, the solution B is added to the three-necked flask and stirred for a period of time, and then the solution A is added to the three-necked flask and stirred for a period of time, and finally, the flask is placed in a constant temperature water bath at 60-80° C. for 2-2.5 hours under continuous stirring, and a yellow product is obtained by centrifugation, and the yellow product is washed with deionized water and ethanol, and then the yellow product is dried to obtain the ZnIn 2 S 4 / ZnSn(OH) 6 Photocatalyst.

[0013] In addition, the present invention also provides a method using the above-mentioned ZnIn 2 S 4 / ZnSn(OH) 6 ZnIn prepared by the method for preparing photocatalyst 2 S 4 / ZnSn(OH) 6 Photocatalyst.

[0014] In addition, the present invention also provides a method using the above-mentioned ZnIn 2 S 4 / ZnSn(OH) 6 Application of photocatalysts in photocatalytic degradation of tetracycline.

[0015] Compared with the prior art, the beneficial effects of the present invention are:

[0016] The present invention aims at the prior art ZnSn(OH) 6 The shortcomings of small specific surface area, low light utilization, no visible light response, and easy recombination of photogenerated electrons and holes were improved by using NaOH solution to 6 The crystal is internally etched to form a hollow ZnSn(OH) 6 Micro-nano materials increase the specific surface area and also provide ZnIn 2 S 4 The ZnIn 2 S 4 Loaded onto hollow ZnSn(OH) 6 On micro-nano materials, ZnIn is formed 2 S 4 / ZnSn(OH) 6 The photocatalytic heterojunction expands the wavelength range of light absorption, making it possible to separate electrons and holes in the visible light band. In addition, due to the special energy band structure, the hollow ZnSn(OH) 6 Micro-nano materials (0.49eV~4.20eV) and ZnIn with a smaller bandgap 2 S 4(-0.98eV~1.4eV) forms a heterojunction, and the photogenerated holes and electrons are transferred to ZnSn(OH) 6 The valence band and ZnIn 2 S 4 The conduction band of the photogenerated carriers is reduced, the recombination effect is reduced, the photocatalytic performance of the photocatalyst is greatly enhanced, the light utilization efficiency is improved, and the application range is expanded.

[0017] It should be understood that the contents described in the summary of the invention are not intended to limit the key or important features of the embodiments of the present invention, nor are they intended to limit the scope of the present invention. Other features of the present invention will become easily understood through the following description. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:

[0019] Figure 1 Solid ZnSn(OH) 6 SEM images of the crystals;

[0020] Figure 2 Solid ZnSn(OH) 6 Transmission electron microscope image of the crystal;

[0021] Figure 3 Hollow ZnSn(OH) 6 Scanning electron microscope images of micro-nano materials;

[0022] Figure 4 Hollow ZnSn(OH) 6 Transmission electron microscopy images of micro-nano materials;

[0023] Figure 5 ZnIn 2 S 4 / ZnSn(OH) 6 Scanning electron microscope image of the photocatalyst;

[0024] Figure 6 ZnIn 2 S 4 / ZnSn(OH) 6 Transmission electron microscopy image of the photocatalyst;

[0025] Figure 7 ZnSn(OH) 6 、ZnIn 2 S 4 and ZnIn 2 S 4 / ZnSn(OH) 6 XRD diffraction pattern of photocatalyst;

[0026] Figure 8 ZnSn(OH) 6 、ZnIn 2 S 4 and different composite ratios of ZnIn 2 S 4 / ZnSn(OH) 6 Schematic diagram of photocatalytic degradation of tetracycline by photocatalyst;

[0027] Fig. 9 ZnIn 2 S 4 / ZnSn(OH) 6 X-ray photoelectron spectrum of

[0028] Fig.10 This is the local high-resolution map of the Zn element;

[0029] Fig.11 This is the local high-resolution spectrum of the In element;

[0030] Fig.12 It is the local high-resolution map of the S element;

[0031] Fig.13 This is the local high-resolution map of Sn element;

[0032] Fig.14 This is a local high-resolution map of the O element. DETAILED DESCRIPTION

[0033] The present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments. It is to be understood that the specific embodiments described herein are only used to explain the relevant invention, rather than to limit the invention. It should also be noted that, for ease of description, only the parts related to the invention are shown in the accompanying drawings.

[0034] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0035] Example 1

[0036] An embodiment of the present invention provides a ZnIn 2 S 4 / ZnSn(OH) 6 The method for preparing a photocatalyst comprises the following steps:

[0037] 1) Synthesis of solid ZnSn(OH) by coprecipitation method 6 Crystals;

[0038] First, take a 25mL beaker and stir SnCl 4 (0.8-1mmol) was added to 4-5mL ethanol and stirred for 8-10min to form solvent 1; then another 25mL beaker was added with (CH3COO) 2 Zn·2H 2 O (0.8-1mmol) and sodium dodecyl sulfonate (0.8-1mmol), then add 10-12mL of deionized water, and stir for 8-10min to form solution 2; mix solution 1 and solution 2 at room temperature to obtain a mixed solution; add NaOH solution (4-5mL, 2M) dropwise to the mixed solution, stir for 30-40min at room temperature, obtain a white product by centrifugation, wash the white product with deionized water and ethanol, and then dry the white product in an oven at 60-70°C to obtain solid ZnSn(OH) 6 Crystals;

[0039] 2) Etching solid ZnSn(OH) using self-sacrificial template method 6 The internal structure of the crystal forms a hollow ZnSn(OH) 6 Micro-nano materials;

[0040] First, 160-170 mg of solid ZnSn(OH) 6 The crystals were added to a NaOH (4-5 mL, 2 M) solution, stirred at room temperature for 5-8 min, and then centrifuged to obtain the product. The product was washed with deionized water and ethanol, and then dried in an oven at 60-70 ° C to obtain ZnSn(OH) 6 Hollow micro-nanomaterials;

[0041] 3) ZnIn 2 S 4 In hollow ZnSn(OH) 6 In situ growth was performed on the material to prepare ZnIn 2 S 4 / ZnSn(OH) 6 Photocatalysts;

[0042] First, 143 mg of hollow ZnSn(OH) 6 The micro-nano material (0.4-0.5 mmol) was added to a 250 mL three-necked flask, 100-120 mL of deionized water was added to the three-necked flask, and the mixture was stirred rapidly for 0.5-0.6 h for later use; then 13.63 mg of ZnCl 2 and 58.65 mg InCl 3 ·4H 2O was dissolved in 20 mL of deionized water and stirred for 8-10 min to form solution A-1 for later use; 90 mg of thioacetamide (TAA) was dissolved in 20 mL of deionized water to form solution B-1 for later use;

[0043] Then, solution B-1 was added to the three-necked flask and stirred for 0.5-0.6h, and then solution A-1 was added to the three-necked flask and stirred for 8-10min. Finally, the flask was placed in a constant temperature water bath at 60-80℃ for 2-2.5h under continuous stirring, and a yellow product was obtained by centrifugation. The yellow product was washed with deionized water and ethanol, and then dried in an oven at 60-70℃ to obtain ZnIn 2 S 4 / ZnSn(OH) 6 Photocatalyst-No.1.

[0044] Example 2

[0045] An embodiment of the present invention provides a ZnIn 2 S 4 / ZnSn(OH) 6 The method for preparing a photocatalyst comprises the following steps:

[0046] 1) Synthesis of solid ZnSn(OH) by coprecipitation method 6 Crystals;

[0047] First, take a 25mL beaker and stir SnCl 4 (0.8-1mmol) was added to 4-5mL ethanol and stirred for 8-10min to form solvent 1; then another 25mL beaker was added with (CH3COO) 2 Zn·2H 2 O (0.8-1mmol) and sodium dodecyl sulfonate (0.8-1mmol), then add 10-12mL of deionized water, and stir for 8-10min to form solution 2; mix solution 1 and solution 2 at room temperature to obtain a mixed solution; add NaOH solution (4-5mL, 2M) dropwise to the mixed solution, stir for 30-40min at room temperature, obtain a white product by centrifugation, wash the white product with deionized water and ethanol, and then dry the white product in an oven at 60-70°C to obtain solid ZnSn(OH) 6 Crystals;

[0048] 2) Etching solid ZnSn(OH) using self-sacrificial template method 6 The internal structure of the crystal forms a hollow ZnSn(OH) 6 Micro-nano materials;

[0049] First, 160-170 mg of solid ZnSn(OH) 6The crystals were added to a NaOH (4-5 mL, 2 M) solution, stirred at room temperature for 5-8 min, and then centrifuged to obtain the product. The product was washed with deionized water and ethanol, and then dried in an oven at 60-70 ° C to obtain ZnSn(OH) 6 Hollow micro-nanomaterials;

[0050] 3) ZnIn 2 S 4 In hollow ZnSn(OH) 6 In situ growth was performed on the material to prepare ZnIn 2 S 4 / ZnSn(OH) 6 Photocatalysts;

[0051] First, 143 mg of hollow ZnSn(OH) 6 Add the micro-nano material (0.4-0.5mmol) into a 250mL three-necked flask, add 100-120mL deionized water into the three-necked flask, stir rapidly for 0.5-0.6h, and then add 34.08mg ZnCl 2 and 146.62 mg InCl 3 ·4H 2 O was dissolved in 20 mL of deionized water and stirred for 8-10 min to form solution A-2 for later use; 225 mg of thioacetamide (TAA) was dissolved in 20 mL of deionized water to form solution B-2 for later use;

[0052] Then, solution B-2 was added to the three-necked flask and stirred for 0.5-0.6h, and then solution A-2 was added to the three-necked flask and stirred for 8-10min. Finally, the flask was placed in a constant temperature water bath at 60-80°C for 2-2.5h under continuous stirring, and a yellow product was obtained by centrifugation. The yellow product was washed with deionized water and ethanol, and then dried in an oven at 60-70°C to obtain ZnIn 2 S 4 / ZnSn(OH) 6 Photocatalyst-2.

[0053] Example 3

[0054] An embodiment of the present invention provides a ZnIn 2 S 4 / ZnSn(OH) 6 The method for preparing a photocatalyst comprises the following steps:

[0055] 1) Synthesis of solid ZnSn(OH) by coprecipitation method 6 Crystals;

[0056] First, take a 25mL beaker and stir SnCl4 (0.8-1mmol) was added to 4-5mL ethanol and stirred for 8-10min to form solvent 1; then another 25mL beaker was added with (CH3COO) 2 Zn·2H 2 O (0.8-1mmol) and sodium dodecyl sulfonate (0.8-1mmol), then add 10-12mL of deionized water, and stir for 8-10min to form solution 2; mix solution 1 and solution 2 at room temperature to obtain a mixed solution; add NaOH solution (4-5mL, 2M) dropwise to the mixed solution, stir for 30-40min at room temperature, obtain a white product by centrifugation, wash the white product with deionized water and ethanol, and then dry the white product in an oven at 60-70°C to obtain solid ZnSn(OH) 6 Crystals;

[0057] 2) Etching solid ZnSn(OH) using self-sacrificial template method 6 The internal structure of the crystal forms a hollow ZnSn(OH) 6 Micro-nano materials;

[0058] First, 160-170 mg of solid ZnSn(OH) 6 The crystals were added to a NaOH (4-5 mL, 2 M) solution, stirred at room temperature for 5-8 min, and then centrifuged to obtain the product. The product was washed with deionized water and ethanol, and then dried in an oven at 60-70 ° C to obtain ZnSn(OH) 6 Hollow micro-nanomaterials;

[0059] 3) ZnIn 2 S 4 In hollow ZnSn(OH) 6 In situ growth was performed on the material to prepare ZnIn 2 S 4 / ZnSn(OH) 6 Photocatalysts;

[0060] First, 143 mg of hollow ZnSn(OH) 6 Add the micro-nano material (0.4-0.5mmol) into a 250mL three-necked flask, add 100-120mL deionized water into the three-necked flask, stir rapidly for 0.5-0.6h, and then add 68.15mg ZnCl 2 and 293.24 mg InCl 3 ·4H 2 O was dissolved in 20 mL of deionized water and stirred for 8-10 min to form solution A-3 for later use; 450 mg of thioacetamide (TAA) was dissolved in 20 mL of deionized water to form solution B-3 for later use;

[0061] Then, solution B-3 was added to the three-necked flask and stirred for 0.5-0.6h, and then solution A-3 was added to the three-necked flask and stirred for 8-10min. Finally, the flask was placed in a constant temperature water bath at 60-80℃ for 2-2.5h under continuous stirring, and a yellow product was obtained by centrifugation. The yellow product was washed with deionized water and ethanol, and then dried in an oven at 60-70℃ to obtain ZnIn 2 S 4 / ZnSn(OH) 6 Photocatalyst-No.3.

[0062] Example 4

[0063] Test ZnIn separately 2 S 4 / ZnSn(OH) 6 Photocatalyst-1, ZnIn 2 S 4 / ZnSn(OH) 6 Photocatalyst-2 and ZnIn 2 S 4 / ZnSn(OH) 6 Characterization of photocatalyst-3.

[0064] 1) Electron microscopy characterization experiment

[0065] In this experiment, the Gemini SEM500 thermal field emission scanning electron microscope produced by ZEISS of Germany and the Hitachi H7650 transmission electron microscope produced by HITACHI of Japan were used to observe the microscopic surface and internal structure of the samples.

[0066] like Figure 1 and Figure 2 As shown in the figure, through the coprecipitation reaction, the uniformly dispersed solid ZnSn(OH) with smooth edges and corners and a particle size of about 500nm-2μm was successfully obtained. 6 Crystal.

[0067] like Figure 3 and Figure 4 As shown, NaOH solution has an effect on solid ZnSn(OH) 6 After the crystal is internally etched, a hollow ZnSn(OH) 6 Micro-nano materials.

[0068] like Figure 5 and Figure 6 As shown, the flaky ZnIn 2 S 4 Successfully loaded onto the hollow ZnSn(OH) 6 A composite material, ZnIn2 S 4 / ZnSn(OH) 6 Photocatalyst.

[0069] 2) XRD characterization experiment

[0070] In order to verify the physical phase of the product, in this experiment, the physical phase was characterized by using a DMAX-2500 X-ray diffractometer (XRD) of Rigaku Corporation, Japan, and the XRD pattern of the prepared sample was obtained to infer the crystal structure. Cu-Kα radiation was used, the scanning range was 2θ=3.0°-70.0°, the tube current was set to 40 mA, and the tube voltage was set to 40 kV.

[0071] like Figure 7 As shown, XRD results show that the product ZnIn 2 S 4 / ZnSn(OH) 6 The diffraction peaks of the photocatalyst at 19.6°, 22.7°, 32.4°, 36.4°, 38.3°, 40.0°, 43.4°, 46.5°, 52.4° and 57.8° correspond to the hollow ZnSn(OH) 6 The (111), (200), (220), (013), (311), (222), (321), (400), (420) and (422) crystal planes of the micro-nanomaterials; the diffraction peaks at 27.6° and 47.3° correspond to ZnIn 2 S 4 The (102) and (110) crystal planes of ZnIn 2 S 4 With hollow ZnSn(OH) 6 After the micro-nano material is composited, it can be clearly seen that its peak position and peak shape are similar to those of pure ZnIn 2 S 4 and hollow ZnSn(OH) 6 The characteristic peaks of micro-nano materials remain consistent. This shows that the ZnIn 2 S 4 Maintains a stable crystal structure and is not affected by ZnSn(OH) 6 The effect of the introduction, the hollow ZnSn(OH) after the reaction 6 The crystal structure of the micro-nano materials is not destroyed either.

[0072] 3) XPS characterization experiment

[0073] like Figures 9 to 14 As shown by Fig. 9 The XPS full peak spectrum of the sample shows that ZnIn 2 S 4 / ZnSn(OH)6 The photocatalyst is mainly composed of Sn, Zn, In, S and O elements; Fig.10 , 11 , 12, 13, and 14 show the local high-resolution spectra of Zn, In, S, Sn, and O, respectively. The weak C1s peak (284.6 eV) in the spectrum comes from hydrocarbon contamination of the XPS instrument itself, and no other impurity elements are detected. From the XPS spectrum of this sample, ZnIn 2 S 4 Successfully loaded on hollow ZnSn(OH) 6 The micro-nano material is pure ZnIn 2 S 4 / ZnSn(OH) 6 Photocatalyst.

[0074] 4) Experimental characterization of the photocatalytic activity of tetracycline

[0075] In this experiment, tetracycline was used as the target for degrading pollutants to test the photocatalytic performance of the prepared photocatalyst. In the experiment, a 500W xenon lamp was used as the light source. The specific experimental steps are as follows:

[0076] 20 mg ZnIn 2 S 4 / ZnSn(OH) 6 The photocatalyst was added into 40 mL of tetracycline solution (50 mg / L) and stirred for 30 min in dark conditions to reach adsorption-desorption equilibrium; then the light source was turned on to carry out the photocatalytic reaction, and samples were taken every 30 min. After centrifugation, the absorbance value at the maximum absorption wavelength (nm) of the supernatant was determined by a UV-visible spectrophotometer, and the change of tetracycline concentration in the reaction solution with the illumination time t was detected, and its degradation rate (D) was calculated according to the following formula.

[0077] D(%)=[(C 0 -C) / C 0 ]×100%;

[0078] Among them, C 0 and C represent the initial concentration and concentration of tetracycline solution at time t, respectively.

[0079] like Figure 8 As shown, ZnIn 2 S 4 / ZnSn(OH) 6 -Photocatalyst No. 1, ZnIn 2 S 4 / ZnSn(OH) 6 -Photocatalyst No. 2, ZnIn 2 S4 / ZnSn(OH) 6 -Photocatalyst No. 3, hollow ZnSn(OH) 6 Micro-nano materials and pure ZnIn 2 S 4 The tetracycline degradation rates were 36.2%, 92.9%, 87.5%, 29.9% and 81.3% respectively.

[0080] The present invention aims at the prior art ZnSn(OH) 6 The shortcomings of small specific surface area, low light utilization, no visible light response, and easy recombination of photogenerated electrons and holes were improved by using NaOH solution to 6 The crystal is internally etched to form a hollow ZnSn(OH) 6 Micro-nano materials increase the specific surface area and also provide ZnIn 2 S 4 The ZnIn 2 S 4 Loaded onto hollow ZnSn(OH) 6 On micro-nano materials, ZnIn is formed 2 S 4 / ZnSn(OH) 6 The photocatalytic heterojunction expands the wavelength range of light absorption, making it possible to separate electrons and holes in the visible light band. In addition, due to the special energy band structure, the hollow ZnSn(OH) 6 Micro-nano materials (0.49eV~4.20eV) and ZnIn with a smaller bandgap 2 S 4 (-0.98eV~1.4eV) forms a heterojunction, and the photogenerated holes and electrons are transferred to ZnSn(OH) 6 The valence band and ZnIn 2 S 4 The conduction band of the photogenerated carriers is reduced, the recombination effect is reduced, the photocatalytic performance of the photocatalyst is greatly enhanced, the light utilization efficiency is improved, and the application range is expanded.

[0081] Example 5

[0082] The embodiment of the present invention also provides a method using the above-mentioned ZnIn 2 S 4 / ZnSn(OH) 6 ZnIn prepared by the method for preparing photocatalyst 2 S 4 / ZnSn(OH) 6 Photocatalyst.

[0083] Example 6

[0084] The embodiment of the present invention also provides a method using the above-mentioned ZnIn 2 S 4 / ZnSn(OH) 6 Application of photocatalysts in photocatalytic degradation of tetracycline.

[0085] In the description of this specification, the description of the terms "one embodiment", "some embodiments", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0086] The above are only preferred embodiments of the present application and are not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

Claims

1. A method for preparing a ZnIn2S4 / ZnSn(OH)6 photocatalyst, characterized in that: The steps include: 1) Solid ZnSn(OH)6 crystals were synthesized by coprecipitation method; 2) using a self-sacrificial template method to erode the internal structure of the solid ZnSn(OH)6 crystal to form a hollow ZnSn(OH)6 micro-nano material; 3) In-situ growth of ZnIn2S4 on the hollow ZnSn(OH)6 material to prepare a ZnIn2S4 / ZnSn(OH)6 photocatalyst.

2. The method for preparing the ZnIn2S4 / ZnSn(OH)6 photocatalyst according to claim 1, characterized in that: In the step 1), first, take a beaker, add SnCl4 to ethanol under constant stirring and stir for a period of time to form solvent one; then take another beaker, add (CH3COO)2Zn·2H2O and sodium dodecyl sulfate, then add deionized water, and stir for a period of time to form solution two; mix solution one and solution two at room temperature to obtain a mixed solution; add NaOH solution dropwise to the mixed solution, stir for a period of time at room temperature, obtain a white product by centrifugation, wash the white product with deionized water and ethanol, and then dry the white product to obtain the solid ZnSn(OH)6 crystal.

3. The method for preparing the ZnIn2S4 / ZnSn(OH)6 photocatalyst according to claim 1, characterized in that: In the step 2), the solid ZnSn(OH)6 crystals are first added to a NaOH solution, stirred at room temperature for a period of time, and then centrifuged to obtain a product. The product is washed with deionized water and ethanol, and then dried to obtain the ZnSn(OH)6 hollow micro-nano material.

4. The method for preparing the ZnIn2S4 / ZnSn(OH)6 photocatalyst according to claim 1, characterized in that: In the step 3), firstly, the hollow ZnSn(OH)6 micro-nano material is added to a three-necked flask, deionized water is added to the three-necked flask, and the mixture is rapidly stirred for a period of time for later use; then, ZnCl2 and InCl3·4H2O are dissolved in deionized water, and stirred for a period of time to form a solution A for later use; and thioacetamide is dissolved in deionized water to form a solution B for later use; Then, the solution B is added to the three-necked flask and stirred for a period of time, and then the solution A is added to the three-necked flask and stirred for a period of time. Finally, the flask is placed in a constant temperature water bath at 60-80°C for 2-2.5 hours under continuous stirring, and a yellow product is obtained by centrifugation. The yellow product is washed with deionized water and ethanol, and then the yellow product is dried to obtain the ZnIn2S4 / ZnSn(OH)6 photocatalyst.

5. A ZnIn2S4 / ZnSn(OH)6 photocatalyst prepared by the preparation method of the ZnIn2S4 / ZnSn(OH)6 photocatalyst described in any one of claims 1 to 4.

6. Use of the ZnIn2S4 / ZnSn(OH)6 photocatalyst according to claim 5 in photocatalytic degradation of tetracycline.

Citation Information

Patent Citations

  • Preparation method of CdIn2S4 / ZnSn (OH) 6 composite micron block

    CN118416913A