Composite-phase molybdenum carbide catalyst as well as preparation method and application thereof

By loading molybdenum salt on Mo2N and carbonizing in a reducing atmosphere, a composite phase molybdenum carbide catalyst containing α-MoC and β-Mo2C was prepared, which solved the problem of high preparation cost and difficult to control in the prior art, and improved the catalysis Activity and selectivity achieve efficient CO2 conversion to CO reaction.

CN119076031AActive Publication Date: 2024-12-06SHAANXI UNIV OF SCI & TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411185176.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-06
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

The existing composite phase molybdenum carbide catalysts are costly to prepare, and the composite phase ratio is difficult to accurately control, resulting in unsatisfactory catalytic activity and selectivity.

Method used

By loading molybdenum salt on Mo2N, carbonizing in a drying and reducing atmosphere by immersion, a composite phase molybdenum carbide catalyst containing α-MoC and β-Mo2C was prepared, and the composite phase ratio was adjusted using the mass ratio of molybdenum salt and Mo2N.

Benefits of technology

The preparation of composite phase molybdenum carbide catalyst with simple steps, easy raw materials and safe operation is achieved, which improves the conversion rate and CO selectivity of CO2 to CO, and the catalyst has excellent stability and high activity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119076031A_ABST
    Figure CN119076031A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of catalysts, and relates to a preparation method of a composite-phase molybdenum carbide catalyst, which comprises the following steps: S1, weighing molybdenum salt, and dissolving in deionized water to obtain a molybdenum solution; mo2N is added into the molybdenum solution, and turbid liquid is obtained; heating and stirring the turbid liquid in a water bath until the turbid liquid is in a gel state, and drying at 50-120 DEG C to prepare a precursor; the precursor is carbonized in a reducing atmosphere, and a composite phase molybdenum carbide material containing alpha-MoC and beta-Mo2C is prepared; the carbonization condition is as follows: the temperature is raised to 500-680 DEG C within 1-5 hours, and the carbonization time is 2-10 hours. Mo2N is loaded with a molybdenum salt solution to obtain a precursor, and the precursor is carbonized at 500-680 DEG C to obtain the proportion-controllable composite-phase molybdenum carbide catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of catalysts, and in particular relates to a composite phase molybdenum carbide catalyst and a preparation method and application thereof. Background Art

[0002] The massive consumption of fossil fuels has resulted in the emission of large amounts of carbon dioxide (CO2), which has induced a serious greenhouse effect. Therefore, CO2 capture, storage, and utilization (CCU) have attracted extensive attention as a potential way to control the greenhouse effect. To date, the catalytic reduction of CO2 to value-added products is widely considered to be a compelling solution to reduce the CO2 concentration in the atmosphere, thereby mitigating global warming and providing a sustainable solution to the energy crisis. The reverse water gas shift reaction (RWGS) is one of the most studied CO2 utilization processes for the production of carbon monoxide (CO), which is one of the most relevant and versatile C1 building blocks for the fine chemical industry, in addition to being a potential sustainable alternative to traditional petrochemical feedstocks. It is a key component of industrial processes such as the Fischer-Tropsch synthesis of hydrocarbons and alcohols, methanol carbonylation for large-scale production of acetic acid, production of polymers, and synthesis of fine chemicals (e.g., olefin and alkyne carbonylation, olefin hydrogenation, carbonylation cross-coupling, and C-H bond carbonylation, to name a few).

[0003] In the reverse water gas shift reaction, the performance of the catalyst plays a key role. Conventional reverse water gas shift catalysts, copper, platinum and other precious metal-based catalysts are known to effectively promote RWGS. The high CO selectivity of copper catalysts, along with the cheaper cost of non-critical elements, make them valuable candidates for the process. Although they have certain activity under certain conditions, they often suffer from problems such as low activity, unsatisfactory selectivity and poor stability.

[0004] Transition metal carbides (TMC) are a special class of abundant and relatively cheap materials with excellent physical properties, such as extremely high hardness, simple crystal structure, electrical and thermal conductivity, and good chemical and thermal stability, and they have shown excellent activity and selectivity in many catalytic reactions. However, pure phase molybdenum carbide also has shortcomings. The surface of β-Mo2C has strong adsorption and dissociation ability for H2, but its selectivity for CO is not high. At present, the preparation of α-MoC and β-Mo2C composite phase molybdenum carbide catalysts is mainly through high-temperature calcination to partially convert the α-Mo2C phase into the α-MoC phase or partially convert the α-MoC phase into the α-Mo2C phase, thereby obtaining composite phase molybdenum carbide. This route has high preparation costs and the ratio of the composite phase is difficult to accurately control. Summary of the invention

[0005] The purpose of the present invention is to provide a composite phase molybdenum carbide catalyst and a preparation method and application thereof, which solves the problems of high preparation cost and difficulty in accurately controlling the ratio of the composite phase of the existing composite phase molybdenum carbide catalyst.

[0006] The present invention is achieved through the following technical solutions:

[0007] A method for preparing a composite phase molybdenum carbide catalyst comprises the following steps:

[0008] S1, weighing a molybdenum salt and dissolving it in deionized water to obtain a molybdenum solution;

[0009] S2, adding Mo2N to the molybdenum solution to obtain a suspension;

[0010] S3, heating and stirring the suspension in a water bath until it reaches a gel state, and drying at 50-120° C. to obtain a precursor;

[0011] S4, carbonizing the precursor under a reducing atmosphere to obtain a composite phase molybdenum carbide material containing α-MoC and β-Mo2C;

[0012] The carbonization conditions are: heating to 500-680° C. in 1-5 hours, and carbonization time of 2-10 hours.

[0013] Further, in S1, the molybdenum salt is one or more of ammonium molybdate, molybdic acid, molybdenum oxide and molybdenum pentachloride.

[0014] Further, in S3, the water bath temperature is 40-90°C.

[0015] Further, in S4, the carbon source used for the carbonization is CH4, urea, sucrose, glucose or aniline.

[0016] Further, in S2, the preparation process of Mo2N is:

[0017] MoO3 is prepared from ammonium molybdate using a template method; MoO3 is nitrided in a flowing nitrogen source to obtain Mo2N.

[0018] Furthermore, the nitriding conditions are: heating to 500-700° C. in 1-3 hours and keeping the temperature for 1-3 hours.

[0019] Furthermore, the nitrogen source is ammonia or carbon nitride.

[0020] The invention discloses a composite phase molybdenum carbide catalyst prepared by the preparation method. The composite phase molybdenum carbide catalyst contains α-MoC and β-Mo2C, and the ratio of α-MoC and β-Mo2C is regulated by the mass ratio of molybdenum salt and Mo2N.

[0021] The invention discloses the application of the composite phase molybdenum carbide catalyst as a reverse water-gas shift catalyst in the reverse water-gas shift reaction.

[0022] Compared with the prior art, the present invention has the following beneficial technical effects:

[0023] The present invention discloses a method for preparing a composite phase molybdenum carbide catalyst, wherein a molybdenum salt is loaded on Mo2N by an impregnation method, and then the composite phase molybdenum carbide catalyst is prepared by drying and carbonization. The preparation method is reported for the first time and has the advantages of simple steps, easy availability of raw materials, and safe operation. The existing composite phase molybdenum carbide is obtained by carbonizing Mo2N at high temperature (≥800°C), and the composite phase ratio is uncontrollable. The present invention first prepares an AM / Mo2N precursor, and Mo2N is carbonized in a reducing atmosphere to obtain α-MoC, and the molybdenum salt provided by the molybdenum solution is carbonized to obtain β-Mo2C. Therefore, a molybdenum salt solution is loaded on Mo2N to obtain a precursor, and carbonization is performed at 500-680°C to obtain a composite phase molybdenum carbide catalyst with a controllable ratio.

[0024] The present invention also discloses a composite phase molybdenum carbide catalyst, which contains α-MoC and β-Mo2C. The ratio of α-MoC and β-Mo2C in the composite phase can be precisely controlled by regulating the mass ratio of molybdenum salt and Mo2N. The composite phase molybdenum carbide catalyst prepared by the present invention has an improved conversion rate in catalyzing CO2 to CO compared with single phase molybdenum carbide.

[0025] The present invention also discloses the use of the composite phase molybdenum carbide catalyst as a reverse water-gas shift catalyst in a reverse water-gas shift reaction. The catalyst obtained by the present invention has an excellent CO2 conversion rate and a CO selectivity of more than 95%. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The XRD diagram of the composite phase molybdenum carbide catalyst prepared by the present invention;

[0027] Figure 2 This is a detection diagram of the conversion rate of CO2 of the composite phase molybdenum carbide catalyst prepared by the present invention;

[0028] Figure 3 The rate and selectivity detection diagram of the composite phase molybdenum carbide catalyst prepared by the present invention;

[0029] Figure 4 This is a stability test diagram of the composite phase molybdenum carbide catalyst prepared by the present invention;

[0030] Figure 5 The present invention is a flow chart of the preparation method of the composite phase molybdenum carbide catalyst. DETAILED DESCRIPTION

[0031] In order to make the purpose, technical solution and advantages of the present invention more clear, the following is further described in detail with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention, that is, the embodiments described are only part of the embodiments of the present invention, not all embodiments.

[0032] The detailed description of the embodiments of the present invention provided in the following drawings is not intended to limit the scope of the invention claimed for protection, but merely represents a selected embodiment of the present invention. Based on the drawings and embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention.

[0033] The present invention discloses a method for preparing a composite phase molybdenum carbide catalyst, comprising the following steps:

[0034] S1, weighing a molybdenum salt and dissolving it in deionized water to obtain a molybdenum solution;

[0035] S2, adding Mo2N to the molybdenum solution to obtain a suspension;

[0036] S3, heating and stirring the suspension in a water bath until it is in a gel state, and drying at 50-120° C. overnight to obtain a precursor;

[0037] S4. Carbonizing the precursor in a reducing atmosphere to obtain a composite phase molybdenum carbide material containing α-MoC and β-Mo2C.

[0038] Preferably, in S1, the molybdenum salt is one or more of ammonium molybdate tetrahydrate, molybdic acid, molybdenum oxide, and molybdenum pentachloride.

[0039] Preferably, in S3, the water bath temperature is 40-90°C.

[0040] Preferably, in S4, the carbon source used for carbonization is CH4, urea, sucrose, glucose, or aniline.

[0041] The carbonization is specifically as follows: the temperature is raised to 500-680° C. within 1-5 hours, and the carbonization time is 2-10 hours.

[0042] The features and performances of the present invention are further described in detail below in conjunction with the embodiments.

[0043] Example 1

[0044] like Figure 5 As shown, the present invention discloses a method for preparing a composite phase molybdenum carbide catalyst, comprising the following steps:

[0045] S1, weigh 0.045g of ammonium molybdate tetrahydrate and dissolve it in 20mL of deionized water to obtain a molybdenum solution;

[0046] S2, weighing 0.1g of carrier Mo2N and adding it to the molybdenum solution, stirring in a 75°C water bath until it is in a gel state, moving it to a mixing oven and drying it at 80°C for 6h to obtain an AM / Mo2N mixture as a precursor;

[0047] S3. 0.055 g of the precursor was placed in a quartz tube, and a CH4 / H2 mixed gas (CH4:H2=1:3) was introduced with a total flow rate of 60 mL / min. The temperature was then raised to 680°C at a rate of 2°C / min and maintained for 3 h. After natural cooling, a composite molybdenum carbide catalyst was obtained, which was recorded as (75%) MoC / Mo2C.

[0048] Example 2

[0049] Refer to Example 1, and the similarities will not be repeated here. Only the differences will be described below: Weigh 0.09 g of ammonium molybdate tetrahydrate to prepare a composite phase molybdenum carbide catalyst, recorded as (50%) MoC / Mo2C.

[0050] Example 3

[0051] Refer to Example 1, and the similarities will not be repeated here. Only the differences will be described below: Weigh 0.135 g of ammonium molybdate tetrahydrate to prepare a composite phase molybdenum carbide catalyst, recorded as (25%) MoC / Mo2C.

[0052] The above 25%, 50%, and 75% represent the proportion of α-MoC in the composite phase molybdenum carbide.

[0053] Example 4

[0054] On the basis of Example 3, ammonium molybdate tetrahydrate was replaced by molybdenum pentachloride, and the carbonization temperature was adjusted to 500° C. to prepare (25%) MoC / Mo2C.

[0055] Example 5

[0056] On the basis of Example 3, ammonium molybdate tetrahydrate was replaced by molybdenum oxide, and the carbonization temperature was adjusted to 600° C. to prepare (25%) MoC / Mo2C.

[0057] Example 6

[0058] On the basis of Example 3, ammonium molybdate tetrahydrate was replaced by molybdic acid, and the carbonization temperature was adjusted to 550° C. to prepare (25%) MoC / Mo2C.

[0059] Comparative Example 1

[0060] 0.1 g of Mo2N precursor was weighed, put into a quartz tube, carbonized at 680 °C for 3 h, and then cooled naturally to obtain the catalyst α-MoC, but no β-Mo2C was obtained.

[0061] Comparative Example 2

[0062] Weigh 0.1 g of MoO3 precursor, put it into a quartz tube, carbonize it at 680°C for 3 h, and then wait for natural cooling to obtain the catalyst β-Mo2C, but no α-MoC.

[0063] In the above embodiments, Mo2N is prepared by a template method, specifically:

[0064] First, 2.0 g of P123 surfactant was dissolved in 30 mL of ethanol and 10 mL of water;

[0065] Subsequently, 1.0 g of ammonium molybdate tetrahydrate was added to the solution;

[0066] Then, 3.0 g of urea was added and stirred for another hour, and the resulting solution was transferred to a 100 mL container with a Teflon line and placed in an oven for hydrothermal treatment at 160 °C for 20 h;

[0067] Afterwards, the formed gel was centrifuged at 5000 rpm for 30 min, washed with pure water three times, and then dried in an oven at 110 °C for 24 h;

[0068] Finally, the dried gel was calcined in a furnace with an air environment at 550 °C for 6 h to obtain the MoO3 material. The specific surface area of ​​the MoO3 material is 113.8 m 2 g -1 , the larger specific surface area can promote CO2 adsorption.

[0069] Weigh 0.5 g of the obtained MoO3 material and add it into a quartz tube. Nitridize it in a tubular furnace with a flowing nitrogen source at 40 mL / min. Wait for it to cool to room temperature and take it out to obtain Mo2N.

[0070] The nitriding temperature is 500-700° C., the heating time is 1-3 hours, and the temperature holding time is 1-3 hours.

[0071] More specifically, the nitrogen source is ammonia or carbon nitride.

[0072] The materials prepared in Examples 1-3 and the two comparative examples were subjected to diffraction analysis to obtain XRD patterns, as shown in FIG. Figure 1 As shown, with the increase of the proportion of α-MoC, the characteristic peak increases significantly, indicating that the composite phase molybdenum carbide is successfully synthesized.

[0073] like Figure 2As shown, the materials prepared in Examples 1-3 and two comparative examples were used as reverse water gas shift catalysts to detect the conversion rate of CO2. As the reaction temperature increases, the composite phase molybdenum carbide catalyst has higher activity than the single phase molybdenum carbide. The carbon monoxide selectivity of Comparative Example 2 is 95%, which is not much different from the embodiment, but the conversion rate is low, only 0.81 times that of Example 3. The selectivity of Comparative Example 2 is only 84%, and the conversion rate is only 0.77 times that of Example 3.

[0074] The process of application as reverse water gas shift catalyst is:

[0075] After the catalyst was crushed into 40-80 mesh, 0.05-1 g was taken and filled into a quartz tube, which was placed in a fixed bed reactor for reaction evaluation.

[0076] Carbon dioxide and hydrogen are used as the reaction raw materials, the molar ratio is CO2:H2=(1:1, 1:2, 1:3, 1:4) and the gas space velocity GHSV is 1000-200000mL·g -1 ·h -1 ,

[0077] The reaction pressure is normal pressure or near normal pressure, and the reaction temperature is 200°C-400°C.

[0078] like Figure 3 As shown, the rate and selectivity of the reverse water gas shift catalyst prepared in the embodiment of the present invention and the comparative example are tested. As the α-MoC ratio increases, the selectivity of the catalyst to CO gradually increases, while the α-MoC in comparative example 1 has a weak ability to dissociate hydrogen, and the conversion rate decreases; the dissociation ability to hydrogen in comparative example 2 is strong, but the selectivity to CO is not high. The catalytic rate of the composite phase molybdenum carbide catalyst is superior to that of the single phase molybdenum carbide, and the CO selectivity increases as the α-MoC ratio increases.

[0079] like Figure 4 As shown, the reverse water gas shift catalysts prepared in the embodiments of the present invention and the comparative examples were tested for stability. During the 30-hour stability test, there was no deactivation, so the composite phase molybdenum carbide has good stability.

[0080] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present invention can still be modified or replaced by equivalents. Any modification or equivalent replacement that does not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.

Claims

1. A method for preparing a composite phase molybdenum carbide catalyst, characterized in that: The following steps are involved: S1, weighing a molybdenum salt and dissolving it in deionized water to obtain a molybdenum solution; S2, adding Mo2N to the molybdenum solution to obtain a suspension; S3, heating and stirring the suspension in a water bath until it reaches a gel state, and drying at 50-120° C. to obtain a precursor; S4, carbonizing the precursor under a reducing atmosphere to obtain a composite phase molybdenum carbide material containing α-MoC and β-Mo2C; The carbonization conditions are: heating to 500-680° C. in 1-5 hours, and carbonization time of 2-10 hours.

2. The method for preparing a composite phase molybdenum carbide catalyst according to claim 1, characterized in that: In S1, the molybdenum salt is one or more of ammonium molybdate, molybdic acid, molybdenum oxide and molybdenum pentachloride.

3. The method for preparing a composite phase molybdenum carbide catalyst according to claim 1, characterized in that: In S3, the water bath temperature is 40-90°C.

4. The method for preparing a composite phase molybdenum carbide catalyst according to claim 1, characterized in that: In S4, the carbon source used for carbonization is CH4, urea, sucrose, glucose or aniline.

5. The method for preparing a composite phase molybdenum carbide catalyst according to claim 1, characterized in that: In S2, the preparation process of Mo2N is: MoO3 is prepared from ammonium molybdate using a template method; MoO3 is nitrided in a flowing nitrogen source to obtain Mo2N.

6. The method for preparing a composite phase molybdenum carbide catalyst according to claim 5, characterized in that: The nitriding conditions are: heating to 500-700° C. in 1-3 hours and keeping the temperature for 1-3 hours.

7. The method for preparing a composite phase molybdenum carbide catalyst according to claim 5, characterized in that: The nitrogen source is ammonia or carbon nitride.

8. A composite phase molybdenum carbide catalyst prepared by the method for preparing a composite phase molybdenum carbide catalyst according to any one of claims 1 to 7, characterized in that: The composite phase molybdenum carbide catalyst contains α-MoC and β-Mo2C, and the ratio of α-MoC to β-Mo2C is regulated by the mass ratio of molybdenum salt and Mo2N.

9. Use of the composite phase molybdenum carbide catalyst according to claim 8 as a reverse water gas shift catalyst in a reverse water gas shift reaction.

Citation Information

Patent Citations

  • Preparation method of two-dimensional lamellar carbon-based molybdenum carbide composite material

    CN112609197A

  • Preparation method and application of carbon nanotube confined molybdenum carbide-based catalyst

    CN117884151A

  • Catalytic material for water gas shift reaction as well as preparation method and application of catalytic material

    CN117884159A

  • Alkali metal doped molybdenum carbide supported on gamma-alumina for selective co2 hydrogenation into co

    US20180015444A1