Production control method for improving surface quality of high-chromium-nickel gear steel

By adjusting the combustion atmosphere of the heating furnace, the water descaling roller speed and nozzle angle, combined with shot blasting treatment and high-pressure water descaling technology, the problem of iron oxide thickness on the surface of high-chromium nickel gear steel is solved, and the surface quality and production efficiency of rolled materials are improved. Reduced production costs.

CN119076640AInactive Publication Date: 2024-12-06NANJING IRON & STEEL CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411156970.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

High chromium nickel gear steel has severe surface oxidation during high-temperature heating, which makes it difficult to remove the thickness of the iron oxide, affecting the surface quality and production cost of rolled materials.

Method used

By adjusting the combustion atmosphere in the high-temperature section of the heating furnace, adjusting the speed reduction of the water descaling roller and adjusting the angle of the descaling nozzle, combined with shot blasting and high-pressure water descaling technology, the iron oxide on the surface of the blank is effectively removed.

Benefits of technology

The surface flaw detection pass rate of rolled material is improved, production costs are reduced, cracks caused by iron oxide are avoided during the rolling process, and the surface quality pass rate of more than 98%.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a production control method for improving the surface quality of high-chromium-nickel gear steel, which comprises the following steps of: (1) carrying out shot blasting treatment on a blank before the blank is fed into a furnace, and removing oxide scale left on the surface of the blank; 2) reducing the proportion of H2O and O2 in blast furnace and converter gas in the high-temperature section of the heating furnace, and reducing the thickness of oxide scale on the surface of the blank; (3) the angle of a descaling nozzle is adjusted to be 30-45 degrees through AI descaling equipment; (4) two pumps are started during descaling, and the descaling pressure is larger than 28 MPa; and (5) during production, the speed of the water descaling roller way is reduced in advance, the blank descaling time is prolonged, and the gear steel surface quality is improved. By adjusting the combustion atmosphere in the furnace at the high-temperature section of the heating furnace, reducing the speed of the water descaling roller way and adjusting the angle of the descaling nozzle, the scale on the surface of the blank can be effectively removed, the surface flaw detection qualification rate of the rolled metal is increased, and the production cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of steel rolling, and in particular to a production control method for improving the surface quality of high-chromium-nickel gear steel. Background Art

[0002] Gear steel is used in transmission parts for automobiles, aerospace, and engineering machinery. It not only needs to have high transmission efficiency and withstand strong alternating stress loads, but also needs to have good fatigue strength. This makes gear steel more and more demanding in terms of surface quality. In order to maintain high strength, fatigue performance, and good grain size, high-chromium-nickel gear steel usually adds high chromium and nickel alloys for high-temperature heating and diffusion. The billet stays in the furnace for a long time under high temperature conditions. During production, it is heated to 1200-1240°C, and the high-temperature diffusion time is greater than 100 minutes, which causes severe surface oxidation. During production, the surface oxide scale is thick and cannot be removed. The remaining oxide scale is pressed into the rolled material during repeated rolling, causing cracks on the surface of the rolled material. The rolled material needs to be peeled on the surface, which not only increases production costs and affects the delivery cycle, but also affects the fatigue life of gear parts when the peeling is not clean.

[0003] Therefore, it is necessary to develop new production control methods to reduce the iron oxide scale on the surface of the billet. Summary of the invention

[0004] Purpose of the invention: In view of the shortcomings and defects of the prior art, the present invention provides a production control method for improving the surface quality of high chromium-nickel gear steel. By adjusting the combustion atmosphere in the high-temperature section of the heating furnace, reducing the speed of the water descaling roller and adjusting the angle of the descaling nozzle, the iron oxide scale on the surface of the billet can be effectively removed, thereby improving the surface flaw detection pass rate of the rolled material and reducing the production cost.

[0005] Technical solution: A production control method for improving the surface quality of high chromium-nickel gear steel of the present invention is characterized by comprising the following steps:

[0006] 1) Before the blank enters the furnace, the blank is shot blasted to remove the iron oxide scale left on the surface of the blank;

[0007] 2) Reduce the ratio of H2O and O2 in the blast furnace and converter gas in the high temperature section of the heating furnace, and reduce the thickness of the iron oxide scale on the surface of the billet;

[0008] 3) Use AI descaling equipment to adjust the descaling nozzle angle to 30°-45°;

[0009] 4) When descaling, turn on two pumps, and the descaling pressure should be greater than 28MPa;

[0010] 5) During production, reduce the speed of the water descaling roller in advance to extend the descaling time of the billet and improve the surface quality of the gear steel.

[0011] The gear steel comprises the following components in percentage by mass: C: 0.15%-0.21%, Si: 0.15%-0.35%, Mn: 0.70%-1.05%, Cr: 1.19%-1.25%, Ni: 0.95%-1.20%, Cu≤0.20%, Mo≤0.20%; the remainder is Fe.

[0012] Wherein, the gear steel is a high chromium nickel gear steel round steel with a diameter of Φ35mm-60mm.

[0013] Wherein, the gear steel is produced using 250mm×300mm×10500mm billets.

[0014] Among them, when producing the gear steel, a 42.6m×11.8m heating furnace is configured online. The heating furnace is divided into three sections: preheating, heating and soaking. There are high-pressure water descaling equipment, 23 horizontal and vertical alternating short stress line rolling mills, and 4 three-roll KOCKS rolling mills.

[0015] Wherein, in the step 2), H2O and O2 in the blast furnace and converter gas in the high temperature section of the heating furnace are reduced, and the volume percentages of the components of the converter gas are: CO 57%, H2 1%, CO2 15%, N2 26.6%, O2 0.4%.

[0016] Wherein, in the step 2), H2O and O2 in the blast furnace and converter gas in the high temperature section of the heating furnace are reduced, and the volume percentage of each component of the blast furnace gas is: CO 24.8%, H2 0.8%, CO2 17.8%, N2 56.6%, and the residual oxygen ratio is controlled to be less than 0.02.

[0017] Wherein, in the step 5), when the water descaling roller is decelerated in advance during production, the speed is reduced from the original 1.4 m / s to 0.8 m / s.

[0018] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: The present invention solves the problem that the thick iron oxide scale of high chromium-nickel gear steel cannot be removed, and improves the surface quality of gear steel. By adjusting the combustion atmosphere in the high-temperature section of the heating furnace, reducing the speed of the water descaling roller table and adjusting the angle of the descaling nozzle, the iron oxide scale on the surface of the billet can be effectively removed, avoiding the iron oxide scale from being pressed into the rolled material during the rolling process to cause continuous cracks on the surface of the rolled material, and improving the surface flaw detection pass rate of the rolled material. The surface flaw detection pass rate reaches more than 98%, reducing production costs and improving delivery efficiency. DETAILED DESCRIPTION

[0019] The technical solution of the present invention is further described below in conjunction with specific implementation methods.

[0020] The present invention adopts 250mm×300mm×10500mm billet to produce Φ35mm-60mm high chromium nickel gear steel round steel. The online configuration includes a 42.6m×11.8m heating furnace, which is divided into three sections: preheating, heating and soaking, high-pressure water descaling equipment, 23 horizontal and vertical alternating short stress line rolling mills, and 4 three-roller KOCKS rolling mills.

[0021] The production control method for improving the surface quality of high chromium-nickel gear steel of the present invention comprises the following steps:

[0022] 1) Before the blank enters the furnace, the blank is shot blasted to remove the iron oxide scale left on the surface of the blank.

[0023] 2) Reduce the ratio of H2O and O2 in the blast furnace and converter gas in the high-temperature section of the heating furnace. The volume percentage of each component of the converter gas is: CO 57%, H2 1%, CO2 15%, N2 26.6%, O2 0.4%; the volume percentage of each component of the blast furnace gas is: CO 24.8%, H2 0.8%, CO2 17.8%, N2 56.6%, and the residual oxygen ratio is controlled to be <0.02; reduce the thickness of the oxide scale on the surface of the billet.

[0024] 3) Use AI descaling equipment to adjust the descaling nozzle angle to 30°-45° to ensure that the descaling water covers the entire blank.

[0025] 4) When descaling, turn on two pumps and set the descaling pressure to >28MPa to ensure that the water pressure can break through the oxide on the surface of the blank and break and flush out the oxidized iron scale.

[0026] 5) During production, the water descaling roller is slowed down in advance from the original 1.4m / s to 0.8m / s, which prolongs the descaling time of the billet, ensures that the oxidized iron scale on the billet surface is completely removed, and improves the surface quality of the gear steel.

[0027] The gear steel of the present invention comprises the following components in percentage by mass: C: 0.15%-0.21%, Si: 0.15%-0.35%, Mn: 0.70%-1.05%, Cr: 1.19%-1.25%, Ni: 0.95%-1.20%, Cu≤0.20%, Mo≤0.20%; the remainder is Fe.

[0028] The present invention can effectively remove the iron oxide scale on the surface of the billet by shot blasting the billet, adjusting the combustion atmosphere in the high temperature section of the heating furnace, reducing the speed of the water descaling roller table and adjusting the angle of the descaling nozzle. The first-time flaw detection pass rate of the rolled material surface reaches more than 98%, and the descaling cost of 110 yuan per ton of steel is saved, thereby improving the delivery rate.

Claims

1. A production control method for improving the surface quality of high chromium-nickel gear steel. Features: The steps include: 1) Before the blank enters the furnace, the blank is shot blasted to remove the iron oxide scale left on the surface of the blank; 2) Reduce the H in the blast furnace and converter gas in the high temperature section of the heating furnace 2 O and O 2 ratio, reducing the thickness of the oxide scale on the surface of the blank; 3) Use AI descaling equipment to adjust the descaling nozzle angle to 30°-45°; 4) When descaling, turn on two pumps, and the descaling pressure should be greater than 28MPa; 5) During production, reduce the speed of the water descaling roller in advance to extend the descaling time of the billet and improve the surface quality of the gear steel.

2. The production control method for improving the surface quality of high chromium-nickel gear steel according to claim 1, Features: The gear steel comprises the following components in percentage by mass: C: 0.15%-0.21%, Si: 0.15%-0.35%, Mn: 0.70%-1.05%, Cr: 1.19%-1.25%, Ni: 0.95%-1.20%, Cu≤0.20%, Mo≤0.20%; the remainder is Fe.

3. The production control method for improving the surface quality of high chromium-nickel gear steel according to claim 1, Features: The gear steel is a high chromium-nickel gear steel round steel with a diameter of Φ35mm-60mm.

4. The production control method for improving the surface quality of high chromium-nickel gear steel according to claim 3, Features: The gear steel is produced from a 250mm×300mm×10500mm billet.

5. The production control method for improving the surface quality of high chromium-nickel gear steel according to claim 4, Features: During the production of the gear steel, a 42.6m×11.8m heating furnace is configured online. The heating furnace is divided into three sections: preheating, heating and soaking. There is also high-pressure water descaling equipment, 23 horizontal and vertical alternating short stress line rolling mills, and 4 three-roller KOCKS rolling mills.

6. The production control method for improving the surface quality of high chromium-nickel gear steel according to claim 1, Features: In the step 2), the H in the blast furnace and converter gas in the high temperature section of the heating furnace is reduced. 2 O and O 2 The volume percentages of the converter gas components are: CO 57%, H 2 1%, CO 2 15%, N 2 26.6%, O 2 0.4%.

7. The production control method for improving the surface quality of high chromium-nickel gear steel according to claim 6, Features: In the step 2), the H in the blast furnace and converter gas in the high temperature section of the heating furnace is reduced. 2 O and O 2 The volume percentages of the components of blast furnace gas are: CO 24.8%, H 2 0.8%, CO 2 17.8%, N 2 56.6%, control residual oxygen ratio <0.

02.

8. The production control method for improving the surface quality of high chromium-nickel gear steel according to claim 1, Features: In the step 5), the speed of the water descaling roller is reduced in advance during production, and the speed is reduced from the original 1.4 m / s to 0.8 m / s.

Citation Information

Patent Citations

  • CrMnTi series gear steel production method

    CN103589957A

  • High-pressure water descaling method for alloy steel plates

    CN106140843A

  • Control method for air-fuel ratio of pusher heat accumulating type heating furnace

    CN106370021A

  • Ultra-pure high-temperature fine-grain gear steel as well as manufacturing method and application thereof

    CN111286671A

  • Method for improving descaling quality of nickel-containing steel plate

    CN111872141A