Preparation method of Al < 0.6 > Si < 0.25 > Cu < 1.0 > Mg < 0.20 > Cr aluminum alloy screw wire for rail transit

Through the preparation method of hot rolling and cold drawing of large-scale ingots, combined with large-cool deformation and annealing process, the problems of low production efficiency and poor moldability of aluminum alloy screw wires are solved, efficient and short-process preparation is achieved, and the continuous screws are improved and stability, suitable for rail transit and other fields.

CN119076680APending Publication Date: 2024-12-06NORTHEAST LIGHT ALLOY CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411299917.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The production efficiency of existing aluminum alloy screw wires is low, resulting in poor nailing continuity, unstable batches, and prone to cracking when upsetting screws.

Method used

The preparation method of hot rolling and cold drawing of large-scale ingots is adopted, combined with the large-cool deformation amount and annealing process, and hot rolling is carried out through Y-shaped rolling rolling and vortex induction furnace to control the wire temperature and deformation rate to achieve efficient and short-process preparation.

Benefits of technology

Solve the problem of poor nailing continuity caused by small weight of single reels of wire, improve the moldability and tissue uniformity of screws, extend the service life of screws, improve production efficiency and batch stability, and is suitable for rail transit and Other fields.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a preparation method of an Al < 0.6 > Si < 0.25 > Cu < 1.0 > Mg < 0.20 > Cr aluminum alloy screw wire for rail transit, and belongs to the field of aluminum alloy processing. The problems that due to the fact that an existing wire rod disc is small in weight, the nailing continuity is poor, batch-to-batch instability is caused, the preparing and forming dispersion is large, and due to large batch-to-batch performance fluctuation, cracking occurs during screw heading are solved. The method comprises the following steps: weighing raw materials for smelting and refining; casting to obtain a round cast ingot, heating, cooling, sawing and turning to obtain a cast ingot; after heating, rolling in a hot roughing mill, and after heating in an eddy current induction furnace, rolling in a hot finishing mill; and processing by a dual-die cold wire drawing machine, and performing stable annealing treatment when the total processing rate reaches 25-40%. The wire rod with the single coil weight larger than or equal to 150 kg is prepared, the production efficiency is improved, and meanwhile the batch-to-batch stability is improved; the wire rod has higher-grade corrosion resistance and good low-temperature use performance, and is particularly suitable for the service environment of northern areas or high and cold areas.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of aluminum alloy processing, and specifically relates to a method for preparing an Al0.6Si0.25Cu1.0Mg0.20Cr aluminum alloy screw wire for rail transportation. Background Art

[0002] Mechanical connection is the most commonly used part connection method in rail applications, and screws are very critical components in bolt connections. The number of screws used in my country's rail transit field is very large. For example, in subways, railway freight cars, urban rail vehicles, etc., the number of aluminum alloy screws used in a single set of vehicles is more than 300,000 pieces, weighing about 200kg. The screws mainly include pan head, round head, flat head, countersunk head, flat cone head and other external screws and ring groove screws, etc. In terms of alloy varieties, the aluminum alloy screws currently used are mainly made of 2024, 5052, 5056, 6082, 6B06, 7075 and other grades of aluminum alloy.

[0003] In order to adapt to the performance of the connected parts and ensure the reliability of the connection, the material of the screw should be the same as that of the connected parts as much as possible. Aluminum alloys are widely used in rail transit, and the application space of aluminum alloy fasteners in rail transit bodies is also very broad. The existing domestic wire production route is to produce wire blanks by extrusion. The weight of a single wire is small and the production efficiency is low. The small weight of the wire coil will lead to poor nailing continuity, instability between batches, and large discrete preparation and molding. In addition, the performance fluctuations between batches are large, which leads to cracking problems when upsetting screws. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing Al0.6Si0.25Cu1.0Mg0.20Cr aluminum alloy screw wire for rail transit, so as to solve the problems that the existing wire coil is light in weight, resulting in poor nailing continuity, instability between batches and large discrete preparation and forming, and large performance fluctuations between batches, resulting in cracking during screw upsetting.

[0005] A method for preparing Al0.6Si0.25Cu1.0Mg0.20Cr aluminum alloy screw wire for rail transit, which is carried out according to the following steps:

[0006] 1. According to the weight percentage composition: Si: 0.4%-0.8%, Cu: 0.15%-0.4%, Mg: 0.8%-1.2%, Cr: 0.04%-0.35%, Fe: 0.01-0.70%, Mn: 0.01-0.15%, Zn: 0.01-0.15% and the balance Al, aluminum ingot, AlMn10 master alloy, AlCu20 master alloy, AlTi6 wire, AlCr3 master alloy, AlSi20 master alloy, Mg ingot, Zn ingot and Fe agent are weighed as raw materials;

[0007] Adding aluminum ingots, Zn ingots, Fe agent, AlMn10 master alloy, AlCu20 master alloy, AlCr3 master alloy, Mg ingots, AlSi20 master alloy and AlTi6 wire into a smelting furnace in sequence, and obtaining aluminum alloy melt after smelting and refining;

[0008] 2. The aluminum alloy melt is cast to obtain a round ingot, which is then kept at 525°C to 540°C for 16h to 20h, and then cooled to room temperature with the furnace to obtain an Al0.6Si0.25Cu1.0Mg0.20Cr aluminum alloy ingot. The ingot is then sawed off the head, tail and car body;

[0009] 3. The ingot is kept at 480°C to 520°C for 3h to 5h, then placed in a hot rough rolling mill, and rolled into a Φ20±0.5mm coil at 480°C to 510°C by a Y-type roller, and then heated in an eddy current induction furnace, and then directly sent to a hot finishing rolling mill, and rolled into a Φ10.8~13.8±0.5mm coil by a Y-type roller;

[0010] 4. The above-mentioned wire coil of Φ10.8~13.8±0.5mm is processed by a double-mode cold drawing machine, the deformation of a single mode is controlled at 10%~25%, the stretching speed is not higher than 60m / min, and the deformation passes are arranged according to the finished product specifications. When the total processing rate reaches 25%~40%, stabilization annealing treatment is carried out to obtain Al0.6Si0.25Cu1.0Mg0.20Cr aluminum alloy screw wire for rail transit, thereby completing the preparation method.

[0011] Furthermore, the smelting and refining in step 1 are: smelting at 710° C. to 750° C. for 2 h to 4 h, and refining in 95% argon inert gas for 20 min twice with an interval of more than 1 h.

[0012] Furthermore, the casting in step 2: the casting temperature is 715°C to 735°C, the casting speed is 90mm to 95mm / min, the number of teeth is 40, the cooling water pressure is 0.08MPa to 0.15MPa, and the water temperature is 10°C to 30°C.

[0013] Furthermore, the specification of the round ingot in step 2 is φ162mm.

[0014] Furthermore, the specifications of the ingot in step 2 are

[0015] Furthermore, the eddy current induction furnace in step three is heated: the outlet wire temperature is controlled at 480°C to 510°C.

[0016] Furthermore, the stabilization annealing treatment in step 4 is: keeping warm at 250°C to 280°C for 1 hour.

[0017] Beneficial effects of the present invention:

[0018] 1. The present invention adopts a preparation method of hot-rolling large-size ingots and then cold-drawing to achieve an efficient and short-process preparation procedure, which solves the problem that the weight of a single coil of wire is small, resulting in poor nailing continuity of screw manufacturers, and breaks through the core technology of preparing medium- and high-strength Al0.6Si0.25Cu1.0Mg0.20Cr alloy wire for large coils of wire for screws.

[0019] 2. The present invention adopts a preparation method that matches a large cold deformation amount with an annealing process, which solves the problem of cracking during screw upsetting caused by poor nailing formability and structural heterogeneity, so that the screws upset can be used in different important parts of rail transit vehicles, and has huge application potential. It can be used in many fields besides rail transit, such as automobiles, aerospace, and ships.

[0020] 3. The aluminum alloy manufactured by the present invention has excellent forming performance. After forming, it has the advantages of medium strength, good toughness, good corrosion resistance, etc. after heat treatment. The screws processed by Al0.6Si0.25Cu1.0Mg0.20Cr aluminum alloy wire have the same tensile strength and shear strength as traditional 6082 screws, and have a higher level of corrosion resistance and can be used below 80°C. In particular, Al0.6Si0.25Cu1.0Mg0.20Cr aluminum alloy has good low-temperature performance and is particularly suitable for service in northern or cold regions.

[0021] 4. The present invention uses an efficient and short-process hot rolling preparation process to prepare wire with a single coil weight ≥150kg, thereby improving production efficiency and batch-to-batch stability; the prepared Al0.6Si0.25Cu1.0Mg0.20Cr aluminum alloy screw wire for rail transit should meet the requirements of tensile strength: 150-210MPa, elongation: ≥22%, grain size: not more than level 2, cold forging: the sample is cold headed to 1 / 3 of the original height of the sample without cracks or orange peel, HV0.2: 40-60, and no cracking occurs in the subsequent nail forming process.

[0022] The invention is suitable for preparing Al0.6Si0.25Cu1.0Mg0.20Cr aluminum alloy screw wire for rail transportation. DETAILED DESCRIPTION

[0023] The technical solution of the present invention is not limited to the specific implementation modes listed below, but also includes any combination of the specific implementation modes.

[0024] Specific implementation method 1: This implementation method is a method for preparing Al0.6Si0.25Cu1.0Mg0.20Cr aluminum alloy screw wire for rail transit, which is carried out in the following steps:

[0025] 1. According to the weight percentage composition: Si: 0.4%-0.8%, Cu: 0.15%-0.4%, Mg: 0.8%-1.2%, Cr: 0.04%-0.35%, Fe: 0.01-0.70%, Mn: 0.01-0.15%, Zn: 0.01-0.15% and the balance Al, aluminum ingot, AlMn10 master alloy, AlCu20 master alloy, AlTi6 wire, AlCr3 master alloy, AlSi20 master alloy, Mg ingot, Zn ingot and Fe agent are weighed as raw materials;

[0026] Adding aluminum ingots, Zn ingots, Fe agent, AlMn10 master alloy, AlCu20 master alloy, AlCr3 master alloy, Mg ingots, AlSi20 master alloy and AlTi6 wire into a smelting furnace in sequence, and obtaining aluminum alloy melt after smelting and refining;

[0027] 2. The aluminum alloy melt is cast to obtain a round ingot, which is then kept at 525°C to 540°C for 16h to 20h, and then cooled to room temperature with the furnace to obtain an Al0.6Si0.25Cu1.0Mg0.20Cr aluminum alloy ingot. The ingot is then sawed off the head, tail and car body;

[0028] 3. The ingot is kept at 480°C to 520°C for 3h to 5h, then placed in a hot rough rolling mill, and rolled into a Φ20±0.5mm coil at 480°C to 510°C by a Y-type roller, and then heated in an eddy current induction furnace, and then directly sent to a hot finishing rolling mill, and rolled into a Φ10.8~13.8±0.5mm coil by a Y-type roller;

[0029] 4. The above-mentioned wire coil of Φ10.8~13.8±0.5mm is processed by a double-mode cold drawing machine, the deformation of a single mode is controlled at 10%~25%, the stretching speed is not higher than 60m / min, and the deformation passes are arranged according to the finished product specifications. When the total processing rate reaches 25%~40%, stabilization annealing treatment is carried out to obtain Al0.6Si0.25Cu1.0Mg0.20Cr aluminum alloy screw wire for rail transit, thereby completing the preparation method.

[0030] In this embodiment, AlTi6 wire is used as a grain refiner.

[0031] Specific embodiment 2: This embodiment is different from specific embodiment 1 in that the weight percentage composition in step 1 is: Si: 0.7%, Cu: 0.3%, Mg: 1.0%, Cr: 0.25%, Fe: 0.15%, Mn: 0.15%, Zn: 0.15% and the balance Al. The other steps and parameters are the same as those in specific embodiment 1.

[0032] Specific embodiment 3: This embodiment is different from specific embodiment 1 in that the smelting and refining in step 1 are: smelting at 710°C to 750°C for 2h to 4h, and refining in 95% argon inert gas for 20min twice with an interval of more than 1h. Other steps and parameters are the same as those in specific embodiment 1.

[0033] Specific embodiment 4: This embodiment is different from specific embodiment 1 in that the casting in step 2: the casting temperature is 715°C to 735°C, the casting speed is 90mm to 95mm / min, the number of teeth is 40, the cooling water pressure is 0.08MPa to 0.15MPa, and the water temperature is 10°C to 30°C. The other steps and parameters are the same as those in specific embodiment 1.

[0034] Specific implementation method 5: This implementation method is different from the specific implementation method 1 in that the specification of the round ingot in step 2 is φ162 mm. The other steps and parameters are the same as those in the specific implementation method 1.

[0035] Specific implementation method 6: This implementation method is different from specific implementation method 1 in that in step 2, the temperature is kept at 530° C. for 18 hours and then cooled to room temperature. Other steps and parameters are the same as those in specific implementation method 1.

[0036] Specific embodiment 7: This embodiment is different from the specific embodiment 1 in that the specifications of the ingot in step 2 are The other steps and parameters are the same as those in the first embodiment.

[0037] Specific embodiment eight: This embodiment differs from specific embodiment one in that the eddy current induction furnace in step three is used for heating: the outlet wire temperature is controlled at 480° C. to 510° C. The other steps and parameters are the same as those in specific embodiment one.

[0038] Specific implementation method 9: This implementation method is different from specific implementation method 1 in that the single-mode secondary deformation in step 4 is controlled at 15%. Other steps and parameters are the same as those in specific implementation method 1.

[0039] Specific embodiment 10: This embodiment differs from specific embodiment 1 in that the stabilization annealing treatment in step 4 is: heat preservation at 250° C. to 280° C. for 1 hour. Other steps and parameters are the same as those in specific embodiment 1.

[0040] The beneficial effects of the present invention are verified by the following examples:

[0041] Example:

[0042] A method for preparing Al0.6Si0.25Cu1.0Mg0.20Cr aluminum alloy screw wire for rail transit, which is carried out according to the following steps:

[0043] 1. According to the weight percentage composition of Si: 0.7%, Cu: 0.3%, Mg: 1.0%, Cr: 0.25%, Fe: 0.15%, Mn: 0.15%, Zn: 0.15% and the balance Al, aluminum ingots, AlMn10 master alloy, AlCu20 master alloy, AlTi6 wire, AlCr3 master alloy, AlSi20 master alloy, Mg ingot, Zn ingot and Fe agent are weighed as raw materials;

[0044] Adding aluminum ingots, Zn ingots, Fe agent, AlMn10 master alloy, AlCu20 master alloy, AlCr3 master alloy, Mg ingots, AlSi20 master alloy and AlTi6 wire into a smelting furnace in sequence, and obtaining aluminum alloy melt after smelting and refining;

[0045] 2. The aluminum alloy melt is cast to obtain a round ingot, which is then kept at 530°C for 18 hours and cooled to room temperature to obtain an Al0.6Si0.25Cu1.0Mg0.20Cr aluminum alloy ingot. The ingot is then sawed off the head, tail and car body.

[0046] 3. The ingot is kept at 500°C for 4 hours, then placed in a hot rough rolling mill, and rolled into a Φ20±0.5mm coil at 490°C through a Y-type roller, and then heated in an eddy current induction furnace, and then directly sent to a hot finishing rolling mill, and rolled into a Φ10.8-13.8±0.5mm coil through a Y-type roller;

[0047] 4. The above-mentioned wire coil of Φ10.8~13.8±0.5mm is processed by a double-mode cold drawing machine, the deformation of a single mode is controlled at 15%, the drawing speed is not higher than 60m / min, the deformation passes are arranged according to the finished product specifications, and when the total processing rate reaches 35%, stabilization annealing treatment is carried out to obtain Al0.6Si0.25Cu1.0Mg0.20Cr aluminum alloy screw wire for rail transit, thereby completing the preparation method.

[0048] The smelting and refining in step 1 of this embodiment are as follows: smelting at 730° C. for 3 hours, followed by refining in 95% argon inert gas for 20 minutes at intervals of more than 1 hour.

[0049] The casting in step 2 of this embodiment: the casting temperature is 725°C, the casting speed is 95 mm / min, the number of teeth is 40, the cooling water pressure is 0.10 MPa, and the water temperature is 20°C.

[0050] The specification of the round ingot in step 2 of this embodiment is φ162mm.

[0051] The specifications of the ingot in step 2 of this embodiment are

[0052] In step 3 of this embodiment, the eddy current induction furnace is used for heating: the outlet wire temperature is controlled at 500°C.

[0053] The stabilization annealing treatment described in step 4 of this embodiment is: keeping warm at 270° C. for 1 hour.

[0054] The Al0.6Si0.25Cu1.0Mg0.20Cr aluminum alloy screw wire for rail transit prepared in this embodiment should meet the tensile strength of 150-210MPa, elongation of ≥22%, grain size of no more than grade 2, cold forging: the sample is cold headed to 1 / 3 of the original height of the sample without cracks or orange peel, HV0.2: 40-60, and no cracking occurs in the subsequent nail forming process.

[0055] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing Al0.6Si0.25Cu1.0Mg0.20Cr aluminum alloy screw wire for rail transit, characterized in that It proceeds as follows:

1. According to the weight percentage composition: Si: 0.4%-0.8%, Cu: 0.15%-0.4%, Mg: 0.8%-1.2%, Cr: 0.04%-0.35%, Fe: 0.01-0.70%, Mn: 0.01-0.15%, Zn: 0.01-0.15% and the balance Al, aluminum ingot, AlMn10 master alloy, AlCu20 master alloy, AlTi6 wire, AlCr3 master alloy, AlSi20 master alloy, Mg ingot, Zn ingot and Fe agent are weighed as raw materials; Adding aluminum ingots, Zn ingots, Fe agent, AlMn10 master alloy, AlCu20 master alloy, AlCr3 master alloy, Mg ingots, AlSi20 master alloy and AlTi6 wire into a smelting furnace in sequence, and obtaining aluminum alloy melt after smelting and refining; 2. The aluminum alloy melt is cast to obtain a round ingot, which is then kept at 525°C to 540°C for 16h to 20h, and then cooled to room temperature with the furnace to obtain an Al0.6Si0.25Cu1.0Mg0.20Cr aluminum alloy ingot. The ingot is then sawed off the head, tail and car body; 3. The ingot is kept at 480°C to 520°C for 3h to 5h, then placed in a hot rough rolling mill, and rolled into a Φ20±0.5mm coil at 480°C to 510°C by a Y-type roller, and then heated in an eddy current induction furnace, and then directly sent to a hot finishing rolling mill, and rolled into a Φ10.8~13.8±0.5mm coil by a Y-type roller; 4. The above-mentioned wire coil of Φ10.8~13.8±0.5mm is processed by a double-mode cold drawing machine, the deformation of a single mode is controlled at 10%~25%, the stretching speed is not higher than 60m / min, and the deformation passes are arranged according to the finished product specifications. When the total processing rate reaches 25%~40%, stabilization annealing treatment is carried out to obtain Al0.6Si0.25Cu1.0Mg0.20Cr aluminum alloy screw wire for rail transit, thereby completing the preparation method.

2. The method for preparing Al0.6Si0.25Cu1.0Mg0.20Cr aluminum alloy screw wire for rail transit according to claim 1, characterized in that In step 1, the composition according to weight percentage is: Si: 0.7%, Cu: 0.3%, Mg: 1.0%, Cr: 0.25%, Fe: 0.15%, Mn: 0.15%, Zn: 0.15% and the balance Al.

3. The method for preparing Al0.6Si0.25Cu1.0Mg0.20Cr aluminum alloy screw wire for rail transit according to claim 1, characterized in that The smelting and refining in step 1 are as follows: smelting at 710° C. to 750° C. for 2 h to 4 h, followed by refining in 95% argon inert gas for 20 min twice with an interval of more than 1 h.

4. The method for preparing Al0.6Si0.25Cu1.0Mg0.20Cr aluminum alloy screw wire for rail transit according to claim 1, characterized in that The casting in step 2: the casting temperature is 715°C to 735°C, the casting speed is 90mm to 95mm / min, the number of teeth is 40, the cooling water pressure is 0.08MPa to 0.15MPa, and the water temperature is 10°C to 30°C.

5. The method for preparing Al0.6Si0.25Cu1.0Mg0.20Cr aluminum alloy screw wire for rail transit according to claim 1, characterized in that The specification of the round ingot in step 2 is φ162mm.

6. The method for preparing Al0.6Si0.25Cu1.0Mg0.20Cr aluminum alloy screw wire for rail transit according to claim 1, characterized in that In step 2, the temperature is kept at 530°C for 18 hours and then cooled to room temperature.

7. The method for preparing Al0.6Si0.25Cu1.0Mg0.20Cr aluminum alloy screw wire for rail transit according to claim 1, characterized in that The specification of the ingot in step 2 is φ(140~155)mm×(3500~4500)mm.

8. The method for preparing Al0.6Si0.25Cu1.0Mg0.20Cr aluminum alloy screw wire for rail transit according to claim 1, characterized in that In step 3, the eddy current induction furnace is heated: the outlet wire temperature is controlled at 480°C to 510°C.

9. The method for preparing Al0.6Si0.25Cu1.0Mg0.20Cr aluminum alloy screw wire for rail transit according to claim 1, characterized in that In step 4, the deformation of a single mode is controlled at 15%.

10. The method for preparing Al0.6Si0.25Cu1.0Mg0.20Cr aluminum alloy screw wire for rail transit according to claim 1, characterized in that The stabilization annealing treatment in step 4 is: keeping at 250°C to 280°C for 1 hour.

Citation Information

Patent Citations

  • Method for manufacturing aluminum alloy bar for rail wagon body rivets

    CN101717870A

  • Energy-saving strong-strength aluminum alloy wire and manufacturing method thereof

    CN102610294A

  • Continuous casting and rolling preparation method of 6061 aluminum alloy round rod

    CN113369331A

  • High-conductivity high-strength aluminum alloy monofilament material and preparation method thereof

    CN117701957A

  • Method for producing aluminum alloy wire

    JP2010077535A