Environment-friendly vacuum casting method for iron casting of coke oven
Through environmentally friendly vacuum casting and 3D printing technology, the problems of environmental pollution and low production efficiency of traditional coke oven cast iron casting methods are solved, high-quality and low-cost casting production are achieved, and the stability and resource utilization of castings are improved.
Patent Information
- Application Number
- CN202411235002.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-12-06
AI Technical Summary
The traditional coke oven cast iron casting method has problems such as environmental pollution, complex production process, high cost, low efficiency, unstable quality and easy generation of pores and inclusions.
The environmentally friendly vacuum casting method is used to combine 3D printing technology to reduce pores and inclusions through casting and ultrasonic vibration treatment under vacuum environment, use recycled 3D printing materials, install waste gas treatment equipment for purification, and optimize the ratio of raw materials and alloy addition.
Significantly reduce dust and harmful gas emissions, simplify production processes, reduce costs and labor intensity, improve casting quality and reliability, shorten production cycles, reduce waste gas generation, and improve resource utilization and economic benefits.
Smart Images

Figure CN119076921A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of iron casting, and in particular to an environmentally friendly vacuum casting method for coke oven iron castings. Background Art
[0002] With the rapid development of industry, the demand for coke oven iron castings in metallurgy, chemical industry and other fields is growing. However, the traditional casting method of coke oven iron castings, such as sand casting, has many problems.
[0003] In the traditional sand casting process, a large amount of dust and harmful gases will be generated, causing serious pollution to the environment. At the same time, its production process is relatively complicated, labor-intensive, high in production cost, long in production cycle, and low in efficiency. Moreover, the traditional casting method is prone to produce pores and inclusions in the casting, which affects the quality of the casting and reduces its reliability and stability in actual use. In addition, in the traditional casting process, the metal and air are in contact at high temperature, which will produce a large amount of waste gas. If it is not effectively treated, it will cause great harm to the atmospheric environment.
[0004] In order to solve these problems, meet the increasingly stringent environmental protection requirements and improve production efficiency and casting quality, an environmentally friendly vacuum casting method for coke oven cast iron parts has emerged. This method aims to overcome the drawbacks of traditional casting methods and achieve efficient, high-quality and environmentally friendly production of coke oven cast iron parts by adopting environmentally friendly vacuum casting technology and advanced 3D printing mold technology. Summary of the invention
[0005] In view of the deficiencies of the prior art, the present invention solves the technical problems by adopting a technical solution: an environmentally friendly vacuum casting method for coke oven cast iron parts, the method comprising the following steps:
[0006] Step 1: Raw material preparation: prepare pig iron, scrap steel and recycled scrap iron in a weight ratio of 40:30:30, and prepare the alloy materials and auxiliary materials required for addition;
[0007] Step 2: Casting preparation: According to the shape and size of the required cast iron parts, a casting mold is made by 3D printing. 3D printed molds can be quickly formed directly according to the design model, which greatly shortens the time from design to obtaining the mold, and significantly shortens the entire production cycle. 3D printing technology can accurately control the size and shape accuracy of the mold. The printed mold has good surface quality and relatively small dimensional errors. Less waste is generated during the 3D printing process, and some 3D printing materials can be recycled, which meets environmental protection requirements.
[0008] Step 3: vacuum preparation: install the casting mold made in step 2 into a vacuum furnace with a pouring system and an exhaust system;
[0009] Step 4, smelting molten iron: adding the raw materials in step 1 into a vacuum furnace for smelting to make cast iron;
[0010] Step 5, casting: through the casting system on the vacuum device in step 3, the cast iron prepared in step 4 is poured into the casting mold under vacuum environment, and alloy materials and auxiliary materials are added during the smelting process, and ultrasonic vibration treatment and mechanical stirring treatment are performed. After the casting is completed, it is cooled and solidified in a vacuum environment to obtain a precast iron part;
[0011] Step 6, post-processing: demoulding the precast iron part obtained in step 5, and cleaning its surface by sandblasting after demoulding;
[0012] Step 7: Environmental protection treatment: Classify the waste generated during the casting process and purify the waste gas generated during the casting process. By installing waste gas treatment equipment on the exhaust system, the waste gas generated during the smelting process is purified to remove harmful substances; the waste slag and waste sand generated during the casting process are recycled or properly treated to avoid arbitrary discharge.
[0013] The invention is further configured as follows: in step 1, the weight of pig iron is 40-50 parts, the weight of scrap steel is 30-40 parts, and the weight of recycled scrap iron is 30-40 parts. High-quality raw materials of pig iron and scrap steel reduce the impurity content, reduce the waste slag and waste gas generated during the smelting process, and consider using part of the recycled iron materials, such as the recycled materials of waste cast iron parts after reasonable treatment, to improve resource utilization.
[0014] The invention is further configured as follows: in the step 1, the alloy materials are silicon, manganese, phosphorus and sulfur, and the silicon, manganese, phosphorus and sulfur are 1.5% to 2.5%, 0.5% to 1.2%, 0.05% to 0.1% and 0.05% to 0.12% of the sum of the mass of pig iron, scrap steel and recycled scrap iron, respectively; the auxiliary materials are desulfurizer and dephosphorizer, and the desulfurizer and dephosphorizer are 0.5% to 2% and 1% to 3% of the sum of the mass of pig iron, scrap steel and recycled scrap iron, respectively. Silicon helps to promote graphitization, improve the strength and hardness of cast iron, and also increase the flow of molten iron; manganese can improve the strength and wear resistance of cast iron, and can also neutralize the harmful effects of sulfur; phosphorus can improve the flow of molten iron; sulfur combines with elements such as manganese to form sulfides such as manganese sulfide. These sulfides are dispersed in cast iron and play a role in chip breaking during the cutting process, making the chips easy to break and avoiding the generation of long ribbon chips, thereby improving the cutting performance. Sulfur can lower the melting point of molten iron, making it easier for the molten iron to flow and fill the mold during the casting process.
[0015] The invention is further configured as follows: a vacuum pump is provided inside the vacuum device in step 5, and a vacuum is formed on the upper part of the aluminum liquid surface by vacuuming during production, and the vacuum degree of the vacuum is 10-20Kpa. Casting in a vacuum environment can reduce pores and inclusions in the casting and improve the quality of the casting; at the same time, vacuum casting can reduce the pouring temperature, reduce energy consumption and waste gas emissions, and maintain the vacuum state for a period of time after the molten iron completely fills the casting mold, allowing the casting to solidify and cool in a vacuum environment, which helps to reduce defects such as shrinkage cavities and shrinkage in the casting and improve the density and mechanical properties of the casting.
[0016] The invention is further configured as follows: the temperature of the molten cast iron in step four is 1400-1450°C; the temperature of the poured cast iron in step five is 1330-1350°C.
[0017] The invention is further configured as follows: in step 5, the ultrasonic vibration treatment time is 1-4 minutes, the ultrasonic vibration amplitude is 0.1-2 mm, the mechanical stirring treatment uses an electromagnetic machine, the stirring speed is 500-800 r / min, and the mechanical stirring time is 1-3 minutes. Ultrasonic vibration treatment helps to make the distribution of alloy elements in the casting more uniform, reduce the difference in element content in the microscopic area, improve the overall quality and performance stability of the casting, and the generated sound pressure effect and cavitation effect can promote the flow and shrinkage of molten metal, reduce the generation of casting defects such as shrinkage cavities and shrinkage, and improve the density of the casting; mechanical stirring treatment promotes the full mixing of alloy elements and substances in the molten iron, ensures that the chemical composition of each part of the cast iron part is consistent, promotes the removal of gas and inclusions, and improves the fluidity of the molten iron.
[0018] The invention is further configured as follows: in step six, the sandblasting machine abrasive uses 150 mesh glass beads, the sandblasting distance is 100-200mm, and the sandblasting pressure is 0.3-0.7MPa. For cast iron parts with high surface hardness and simple shape, a higher sandblasting pressure, such as 0.6-0.7MPa, can be selected; while for cast iron parts with low surface hardness, complex shape or thin wall, a lower sandblasting pressure, such as 0.3-0.5MPa, should be used. If it is to remove the oxide scale and rust on the surface of the cast iron part, moderate particle size, such as 40-80 mesh, and high hardness corundum can be selected; if it is to perform fine treatment or finishing on the surface of the cast iron part, finer particle size, such as 80-200 mesh, and relatively low hardness glass beads can be selected.
[0019] The beneficial effects of the present invention are as follows:
[0020] The present invention adopts environmentally friendly vacuum casting, which can not only reduce dust and harmful gases and improve the environment compared with traditional sand casting; but also simplify the production process, reduce labor intensity, reduce production costs, shorten the production cycle, and improve production efficiency. The 3D printing mold technology can be directly formed according to the design model, which greatly shortens the time from design to mold. This greatly shortens the development cycle of new products, and the 3D printing materials can be recycled, which not only meets environmental protection requirements, but also reduces the waste of raw materials, further improves production efficiency and economic benefits, and effectively reduces the pores and inclusions in the castings through vacuum casting, thereby greatly improving the quality of the castings, so that the cast iron parts can withstand greater external forces in actual use, have higher reliability and stability, and reduce the contact between metal and air at high temperature, thereby reducing the generation of waste gas. At the same time, the exhaust gas treatment equipment is installed on the exhaust system to purify the waste gas generated during the smelting process, remove the harmful substances therein, and effectively reduce the pollution to the atmospheric environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 is a casting flow chart of the present invention;
[0022] Figure 2 It is a performance test comparison table of the present invention. DETAILED DESCRIPTION
[0023] The present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. The embodiments of the present invention are provided for the purpose of illustration and description, and are not intended to be exhaustive or to limit the present invention to the disclosed forms. Many modifications and variations will be apparent to those of ordinary skill in the art. The embodiments are selected and described in order to better illustrate the principles and practical applications of the present invention, and to enable those of ordinary skill in the art to understand the present invention and thereby design various embodiments with various modifications suitable for specific uses.
[0024] Embodiment 1:
[0025] See also Figure 1 - Figure 2 The present invention provides a technical solution: an environmentally friendly vacuum casting method for coke oven cast iron parts, the method comprising the following steps:
[0026] Step 1: Raw material preparation: prepare pig iron, scrap steel and recycled scrap iron in a weight ratio of 40:30:30, and prepare the alloy materials and auxiliary materials required for addition;
[0027] Step 2: Casting preparation: According to the shape and size of the required cast iron parts, a casting mold is made by 3D printing;
[0028] Step 3: vacuum preparation: install the casting mold made in step 2 into a vacuum furnace with a pouring system and an exhaust system;
[0029] Step 4, smelting molten iron: adding the raw materials in step 1 into a vacuum furnace for smelting to make cast iron;
[0030] Step 5, casting: through the casting system on the vacuum device in step 3, the cast iron prepared in step 4 is poured into the casting mold under vacuum environment, and alloy materials and auxiliary materials are added during the smelting process, and ultrasonic vibration treatment and mechanical stirring treatment are performed. After the casting is completed, it is cooled and solidified in a vacuum environment to obtain a precast iron part;
[0031] Step 6, post-processing: demoulding the precast iron part obtained in step 5, and cleaning its surface by sandblasting after demoulding;
[0032] Step 7: Environmental protection treatment: Classify the waste generated during the casting process and purify the waste gas generated during the casting process.
[0033] In step 1, the weight portion of pig iron is 40-50 parts, the weight portion of scrap steel is 30-40 parts, and the weight portion of recycled scrap iron is 30-40 parts.
[0034] In step 1, the alloy materials are silicon, manganese, phosphorus and sulfur, and the silicon, manganese, phosphorus and sulfur are 1.5% to 2.5%, 0.5% to 1.2%, 0.05% to 0.1% and 0.05% to 0.12% of the sum of the mass of pig iron, scrap steel and recycled scrap iron respectively. The auxiliary materials are desulfurizer and dephosphorizer, and the desulfurizer and dephosphorizer are 0.5% to 2% and 1% to 3% of the sum of the mass of pig iron, scrap steel and recycled scrap iron respectively.
[0035] In step 5, a vacuum pump is arranged inside the vacuum device. During production, a vacuum is formed above the aluminum liquid surface by evacuating the vacuum, and the vacuum degree is 10-20Kpa.
[0036] The temperature of the molten cast iron in step 4 is 1400-1450°C; the temperature of the cast iron poured in step 5 is 1330-1350°C.
[0037] In step 5, the ultrasonic vibration treatment time is 1-4 minutes, the ultrasonic vibration amplitude is 0.1-2 mm, the mechanical stirring treatment adopts an electromagnetic machine, the stirring speed is 500-800 r / min, and the mechanical stirring time is 1-3 minutes.
[0038] In step six, the sandblasting machine uses 150-mesh glass beads as abrasive, the sandblasting distance is 100-200mm, and the sandblasting pressure is 0.3-0.7MPa.
[0039] Embodiment 2:
[0040] Based on the first embodiment, a method for casting a coke oven iron casting is provided, the method comprising the following steps:
[0041] Step 1: Raw material preparation: prepare pig iron, scrap steel and recycled scrap iron in a weight ratio of 40:30:30, and prepare the alloy materials and auxiliary materials required for addition;
[0042] Step 2: Casting preparation: Make a casting mold according to the shape and size of the required cast iron parts;
[0043] Step 3, smelting molten iron: adding the raw materials in step 1 into a high-frequency induction furnace for smelting to make cast iron;
[0044] Step 4: Casting: The molten iron prepared in step 3 is poured into a casting mold, and after the casting is completed, the molten iron is cooled and solidified to obtain a precast iron part;
[0045] Step 5, post-processing: demoulding the precast iron part obtained in step 5, and cleaning its surface by a sandblasting machine after demoulding;
[0046] Step 6: Environmental protection treatment: Classify the waste generated during the casting process and purify the waste gas generated during the casting process.
[0047] In step 1, the weight portion of pig iron is 40-50 parts, the weight portion of scrap steel is 30-40 parts, and the weight portion of recycled scrap iron is 30-40 parts.
[0048] In step 1, the alloy materials are silicon, manganese, phosphorus and sulfur, and the silicon, manganese, phosphorus and sulfur are 1.5% to 2.5%, 0.5% to 1.2%, 0.05% to 0.1% and 0.05% to 0.12% of the sum of the mass of pig iron, scrap steel and recycled scrap iron respectively. The auxiliary materials are desulfurizer and dephosphorizer, and the desulfurizer and dephosphorizer are 0.5% to 2% and 1% to 3% of the sum of the mass of pig iron, scrap steel and recycled scrap iron respectively.
[0049] The temperature of the molten cast iron in step 4 is 1400-1450°C; the temperature of the cast iron poured in step 5 is 1330-1350°C.
[0050] In step 5, the sandblasting machine uses 150-mesh glass beads as abrasive, the sandblasting distance is 100-200 mm, and the sandblasting pressure is 0.3-0.7 MPa.
[0051] Embodiment three:
[0052] Based on the first embodiment, a vacuum casting method for coke oven cast iron parts is provided, the method comprising the following steps:
[0053] Step 1: Raw material preparation: prepare pig iron, scrap steel and recycled scrap iron in a weight ratio of 30:40:30, and prepare the alloy materials and auxiliary materials required for addition;
[0054] Step 2: Casting preparation: Make a casting mold according to the shape and size of the required cast iron parts;
[0055] Step 3: vacuum preparation: install the casting mold made in step 2 into a vacuum furnace with a pouring system and an exhaust system;
[0056] Step 4, smelting molten iron: adding the raw materials in step 1 into a vacuum furnace for smelting to make cast iron;
[0057] Step 5, casting: through the casting system on the vacuum device in step 3, the cast iron prepared in step 4 is poured into the casting mold under vacuum environment, and alloy materials and auxiliary materials are added during the smelting process, and ultrasonic vibration treatment and mechanical stirring treatment are performed. After the casting is completed, it is cooled and solidified in a vacuum environment to obtain a precast iron part;
[0058] Step 6, post-processing: demoulding the precast iron part obtained in step 5, and cleaning its surface by sandblasting after demoulding;
[0059] In step 1, the weight portion of pig iron is 30-40 parts, the weight portion of scrap steel is 40-50 parts, and the weight portion of recycled scrap iron is 30-500 parts.
[0060] In step 1, the alloy materials are silicon, manganese, phosphorus and sulfur, and the silicon, manganese, phosphorus and sulfur are 1.5% to 2%, 0.5% to 1%, 0.08% to 0.1% and 0.05% to 0.1% of the sum of the mass of pig iron, scrap steel and recycled scrap iron respectively; the auxiliary materials are desulfurizer and dephosphorizer, and the desulfurizer and dephosphorizer are 0.5% to 2% and 1% to 3% of the sum of the mass of pig iron, scrap steel and recycled scrap iron respectively.
[0061] In step 5, a vacuum pump is arranged inside the vacuum device. During production, a vacuum is formed above the aluminum liquid surface by evacuating the vacuum, and the vacuum degree is 10-40Kpa.
[0062] The temperature of the molten cast iron in step 4 is 1400-1450°C; the temperature of the cast iron poured in step 5 is 1330-1350°C.
[0063] In step 5, the ultrasonic vibration treatment time is 1-4 minutes, the ultrasonic vibration amplitude is 0.1-2 mm, the mechanical stirring treatment adopts an electromagnetic machine, the stirring speed is 500-800 r / min, and the mechanical stirring time is 1-3 minutes.
[0064] In step six, the sandblasting machine uses 150-mesh glass beads as abrasive, the sandblasting distance is 100-200mm, and the sandblasting pressure is 0.3-0.7MPa.
[0065] Performance testing:
[0066] Casting was performed according to the methods of Example 1, Example 2 and Example 3, respectively as Experimental Group 1, Experimental Group 2 and Experimental Group 3, to obtain cast iron parts with different properties, and the performance of the three groups of cast iron parts was tested;
[0067] The experimental results show that the iron castings prepared in Experiment 1 have a tensile strength of 422 MPA, a yield strength of 320 MPA, and a hardness of 232. Compared with the castings in Experiment 2 and Experiment 3, the performance of the castings in Experiment 3 can be significantly improved. Compared with the method of using ordinary sand casting, the present invention can reduce the pores and inclusions in the castings and improve the quality of the castings through vacuum casting. At the same time, vacuum casting can reduce the pouring temperature, reduce energy consumption and waste gas emissions, and maintain the vacuum state for a period of time after the molten iron completely fills the casting mold, so that the castings can be cast in a vacuum environment. Solidification and cooling are carried out, which helps to reduce defects such as shrinkage cavities and shrinkage in castings, improve the density and mechanical properties of castings, and the 3D printing mold can be quickly formed directly according to the design model, which greatly shortens the time from design to obtaining the casting mold, generates less waste, and some 3D printing materials can be recycled, which meets environmental protection requirements. By installing exhaust gas treatment equipment on the exhaust system, the exhaust gas generated in the smelting process is purified to remove harmful substances; the waste slag and waste sand generated in the casting process are recycled or properly disposed of to avoid arbitrary discharge.
[0068] Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field and related fields without creative work should fall within the scope of protection of the present invention. The structures, devices and operating methods not specifically described and explained in the present invention are implemented according to the conventional means in the field unless otherwise specified and limited.
Claims
1. An environmentally friendly vacuum casting method for coke oven cast iron parts, It is characterized in that The method comprises the following steps: Step 1: Raw material preparation: prepare pig iron, scrap steel and recycled scrap iron in a weight ratio of 40:30:30, and prepare the alloy materials and auxiliary materials required for addition; Step 2: Casting preparation: According to the shape and size of the required cast iron parts, a casting mold is made by 3D printing; Step 3: vacuum preparation: install the casting mold made in step 2 into a vacuum furnace with a pouring system and an exhaust system; Step 4, smelting molten iron: adding the raw materials in step 1 into a vacuum furnace for smelting to make cast iron; Step 5, casting: through the casting system on the vacuum device in step 3, the cast iron prepared in step 4 is poured into the casting mold under vacuum environment, and alloy materials and auxiliary materials are added during the smelting process, and ultrasonic vibration treatment and mechanical stirring treatment are performed. After the casting is completed, it is cooled and solidified in a vacuum environment to obtain a precast iron part; Step 6, post-processing: demoulding the precast iron part obtained in step 5, and cleaning its surface by sandblasting after demoulding; Step 7: Environmental protection treatment: Classify the waste generated during the casting process and purify the waste gas generated during the casting process.
2. The environmentally friendly vacuum casting method for coke oven cast iron parts according to claim 1, Features: In the step 1, the weight portion of pig iron is 40-50 parts, the weight portion of scrap steel is 30-40 parts, and the weight portion of recycled scrap iron is 30-40 parts.
3. The environmentally friendly vacuum casting method for coke oven cast iron parts according to claim 1, Features: In the step 1, the alloy materials are silicon, manganese, phosphorus and sulfur, and the silicon, manganese, phosphorus and sulfur are 1.5% to 2.5%, 0.5% to 1.2%, 0.05% to 0.1% and 0.05% to 0.12% of the sum of the mass of pig iron, scrap steel and recycled scrap iron respectively; the auxiliary materials are desulfurizer and dephosphorizer, and the desulfurizer and dephosphorizer are 0.5% to 2% and 1% to 3% of the sum of the mass of pig iron, scrap steel and recycled scrap iron respectively.
4. The environmentally friendly vacuum casting method for coke oven cast iron parts according to claim 1, Features: In the step 5, a vacuum pump is arranged inside the vacuum device, and a vacuum is formed above the aluminum liquid surface by evacuating the vacuum during production, and the vacuum degree of the vacuum is 10-20Kpa.
5. The environmentally friendly vacuum casting method for coke oven cast iron parts according to claim 1, Features: The temperature of the molten cast iron in step 4 is 1400-1450°C; the temperature of the cast iron in step 5 is 1330-1350°C.
6. The environmentally friendly vacuum casting method for coke oven cast iron parts according to claim 1, Features: In the step 5, the ultrasonic vibration treatment time is 1-4 minutes, the ultrasonic vibration amplitude is 0.1-2 mm, and the mechanical stirring treatment adopts an electromagnetic machine, the stirring speed is 500-800 r / min, and the mechanical stirring time is 1-3 minutes.
7. The environmentally friendly vacuum casting method for coke oven iron castings according to claim 1, Features: In step 6, the sandblasting machine uses 150-mesh glass beads as abrasive, the sandblasting distance is 100-200 mm, and the sandblasting pressure is 0.3-0.7 MPa.