Preparation method of large-size long-strip ceramic
By preparing large-size long ceramics, using molds and cold isostatic pressing technology, the problems of slow forming speed and high cost of large-size ceramics in the existing technology are solved, and fast and low-cost ceramic preparation is achieved, which is suitable for a variety of products. Chemical product demand.
Patent Information
- Application Number
- CN202411098491.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-12-06
AI Technical Summary
The existing manufacturing process cannot rapidly form large-size long ceramics, resulting in long procurement cycles and high costs, and cannot meet the requirements of different product size structures.
A large-size long-sized ceramic preparation method is adopted, including making long-sized molds, filling alumina ceramic granulation powder, and forming by vacuum sealing and cold isostatic pressing, followed by sintering to prepare large-sized long-sized ceramic products. . This method is simple and low-cost, and can set molds according to the shape of the product to meet the needs of various shape specifications.
It realizes rapid molding of large-size long-sized ceramics, reduces production costs, is suitable for large-scale production and diversified custom processing, meets the preparation needs of different shapes and specifications, and is especially suitable for the manufacturing of large-sized long-sized ceramics of 2000mm and above. .
Smart Images

Figure CN119077896A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of functional ceramics, and in particular to a method for preparing large-size long strip ceramics. Background Art
[0002] In recent years, due to the demand and development of semiconductor equipment, the demand for large-size long ceramic materials has increased rapidly. However, according to the current existing process, only products with a length of less than 1500mm can be produced, and the molding technology of ceramic strips with a size of more than 2000mm is still mainly purchased. The purchase price of such materials is high and the procurement cycle is long. Therefore, it is urgent to introduce the molding technology of large-size alumina ceramics. Summary of the invention
[0003] The purpose of the present invention is to solve the problems that the existing manufacturing process cannot achieve rapid prototyping of large-sized long ceramic strips, has a long procurement cycle, high cost, and cannot meet the requirements of different product size structures. By providing a method for preparing large-sized long ceramic strips, the method has a simple preparation process, low cost, and can quickly form large-sized long ceramic strips of various shapes and specifications.
[0004] The technical solution adopted by the present invention to achieve its invention object is: a method for preparing a large-sized long ceramic strip, comprising the following steps: Step 1: Make a long strip mold; Step 2: Powder filling: install the whole set of molds on the vibration platform, turn on the vibration platform, and fill the alumina ceramic granulation powder into the mold; Step 3: Vacuum and seal: After filling the powder, use a vacuum packaging machine to vacuum and seal the PE inner bag; Step 4: Cold isostatic pressing: hoist the mold filled with powder in step 3 into the cavity of the cold isostatic pressing equipment as a whole, and perform cold isostatic pressing to form a long ceramic green body; Step 5: Sintering: After the sintering plate is covered with sintering sand, the long ceramic green body is placed on the sintering plate and sintered to finally produce a large-sized long ceramic product.
[0005] The large-size long strip ceramic preparation method sets a long strip mold according to the size and shape of the product, fills the mold with alumina ceramic granulation powder, then seals the mold, forms a long strip ceramic green body by cold isostatic pressing, roughly processes the long strip ceramic green body, and finally forms a large-size long strip ceramic product by sintering. The rapid molding of large-size long strip ceramics is achieved, the preparation process is simple, the cost is low, and the corresponding long strip mold can be set according to the shape of different products, which can meet the preparation needs of long strip ceramic products of various shapes and specifications, and can be widely used in the manufacturing and production of various long strip ceramic products, suitable for mass production and diversified customized processing requirements.
[0006] Preferably, the mold includes a rubber mold body, a PE inner bag and a cover plate, and an inner cavity is designed inside the mold body according to the molding shrinkage rate. The mold mainly includes a rubber mold body, a PE inner bag and a cover plate. The cooperation between the PE inner bag and the inner cavity of the mold body can form the required long ceramic shape, and it is also convenient to realize the vacuum sealing operation inside the mold. At the same time, the rubber mold body and the PE inner bag are also convenient in the subsequent cold isostatic pressing process. Ensure that the force is not effectively transmitted, so as to achieve uniform pressure in all directions of the product. The pressurization, pressure holding and pressure relief processes are different in the molding process of ceramic powders of different shapes, which can be set according to the specific product.
[0007] Preferably, the mold further comprises a metal iron plate for fixing, and the size of the metal iron plate is set in coordination with the mold. The mold design process after forming also needs to consider that the straightness of the strip after forming meets the requirement of ±1°, therefore, it is preferred that a metal iron plate for fixing is used in coordination with the mold.
[0008] Preferably, the inner cavity is a regular cavity; or the inner cavity is a variable diameter cavity; or the inner cavity is an irregular cavity. Depending on the shape of the prepared long ceramic strips, the inner cavity can be set as a regular cavity for producing long ceramic products of regular shapes. When it is necessary to prepare long ceramic products with variable diameter structures, the inner cavity can be set as a variable diameter cavity. When the prepared product is not of a regular shape, it is necessary to set the inner cavity as an irregular cavity. In order to facilitate the removal of the formed blank, the mold body can be set as a combined structure, for example, it can be a snap-fit shape, a snap-fit structure, etc.
[0009] Preferably, the PE inner bag is a regular strip structure; or the PE inner bag has a variable diameter strip structure; or the PE inner bag is an irregular strip structure. Based on the different shapes of different strip products, the corresponding PE inner bag is also designed with a corresponding shape, so as to cooperate with the inner cavity of the mold body to form the product shape required by the design.
[0010] Preferably, the purity of the alumina ceramic granulation powder is greater than 99.7%, the bulk density is 1.24g / cm3, and the powder is spherical. The selection of granulation powder needs to have a certain particle gradation to ensure that the ceramic grains grow normally after sintering and the grain size is normal; and the powder should have high purity, certain fluidity, and moderate bulk density, which is conducive to powder filling operation and improves the density after powder filling. The ceramic green body density is high after cold pressing, and the ceramic density and bending strength are high after sintering. As a preferred alumina ceramic granulation powder, AM type is selected, which has a purity greater than 99.7%, a bulk density of 1.24g / cm3, good fluidity, a basically spherical powder, and a uniform distribution of particle gradation.
[0011] Preferably, the powder filling in step 2 includes sieving and iron removal of the powder and vibrating filling. A vibrating screen is used to remove iron and impurities before powder filling. During powder filling, the frequency of the vibration platform is maintained at 20HZ to 80HZ. The powder filling operation includes sieving and iron removal of the powder and vibrating filling. The purity of the powder and the filling density of the powder are the main factors affecting the performance of the ceramic after sintering. Therefore, a vibrating screen is used to remove iron and impurities before powder filling. During powder filling, the frequency of the vibration platform is moderate. While increasing the filling density, the distribution uniformity of the powder in the mold is ensured, that is, the particle size distribution of the powder in different areas is basically consistent.
[0012] Preferably, in step 4, a high-pressure container is used for cold isostatic pressing, and a liquid medium is injected into the high-pressure container through a pressure pump for uniform pressurization, and the cold isostatic pressing pressure is 110-200 MPa. Cold isostatic pressing is to place the sample to be pressed in a high-pressure container, and use the incompressible nature of the liquid medium and the property of uniformly transmitting pressure to uniformly pressurize the sample from all directions. When the liquid medium is injected into the pressure container through a pressure pump, according to the principles of fluid mechanics, its pressure remains unchanged and is evenly transmitted to all directions. The pressurization, pressure holding, and pressure relief processes are different in the molding process of ceramic powders of different shapes. The cold isostatic pressing pressure is 110-200 MPa.
[0013] Preferably, the sintering sand in step 6 is 44# sintering sand, and the sintering temperature is 1600°C to 1770°C. Due to the large size of the product, it is easy to cause cracking due to uneven force during the sintering process, so the placement of the product before sintering and the selection of the sintering process are very important. Preferably, 44# sintering sand is used for sintering.
[0014] Preferably, the sintering platen in step 6 requires a flatness of ±1°.
[0015] Preferably, the long ceramic green body is rough-machined before sintering to form a long ceramic formed body. Since the size of the ceramic green body is not uniform after forming, removing excess powder through rough machining is beneficial for placement during sintering and reduces finishing time.
[0016] The beneficial effects of the present invention are as follows: the method for preparing large-size long ceramic strips realizes the rapid prototyping of large-size long ceramic strips, has a simple preparation process and low cost, and can set corresponding long strip molds according to the shapes of different products, which can meet the preparation needs of long ceramic products of various shapes and specifications, and can be widely used in the manufacture and production of various long ceramic products, and is suitable for mass production and diversified customized processing requirements. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 It is a structural schematic diagram of the mold in the present invention.
[0018] Figure 2It is a schematic diagram of the decomposition structure of the mold of the present invention.
[0019] Figure 3 It is a structural schematic diagram of the cold isostatic pressing process of the present invention.
[0020] Figure 4 It is a structural schematic diagram of the mold in Example 6 of the present invention.
[0021] Figure 5 It is a structural schematic diagram of the mold in Example 7 of the present invention.
[0022] In the figure: 1. mold, 2. rubber mold body, 3. PE inner bag, 4. cover plate, 5. inner cavity, 6. high-pressure container, 7. liquid medium, 8. inner bag cavity, 9. powder. DETAILED DESCRIPTION
[0023] The various aspects of the present invention are described in detail below through specific embodiments in conjunction with the accompanying drawings.
[0024] Embodiment 1: exist Figure 1 , Figure 2 , Figure 3 In the embodiment shown, a method for preparing a large-sized long ceramic strip is suitable for preparing a large-sized long ceramic strip product with a regular shape, and includes the following steps: (1) Selection of granulation powder; ① It has a certain particle gradation to ensure the normal growth of ceramic grains and normal grain size after sintering; ② The powder has high purity, certain fluidity, and moderate bulk density, which is conducive to powder filling operation and improves the density after powder filling. The ceramic green body has high density after cold pressing, and the ceramic density and bending strength are high after sintering.
[0025] The alumina ceramic granulation powder preferably has a purity greater than 99.7%, a bulk density of 1.24 g / cm3, good fluidity, a substantially spherical powder shape, and a uniform particle size distribution.
[0026] (2) Mold design: The mold 1 includes a rubber mold body 2, a PE inner bag 3 and a cover plate 4. An inner cavity 5 is provided inside the mold body 2. The rubber mold inner cavity size is designed to be 2900*580*145mm and 5mm thick according to the molding shrinkage rate; and the PE inner bag 3 is designed to be 3200*578*143mm and 1mm thick. An inner bag cavity 8 is provided in the PE inner bag. In order to facilitate powder filling, a powder filling port is also provided on the PE inner bag. To ensure that the size after molding meets the expected requirements, the design process of the mold 1 after molding also needs to consider that the straightness of the long strip after molding meets the ±1° requirement. Therefore, the mold 1 also includes a metal iron plate, and the design size of the fixed metal iron plate is 2900*580*5mm.
[0027] (3) Powder filling operation: The powder filling operation includes powder screening, iron removal and vibration filling. The purity of the powder and the filling density of the powder are the main factors affecting the performance of the ceramic after sintering. Therefore, a vibrating screen is required to remove iron and impurities before powder filling. When filling powder, the frequency of the vibration platform is moderate, generally maintained at 40HZ to 60HZ, which improves the filling density while ensuring the uniformity of the distribution of the powder 9 in the mold, that is, the particle size distribution of the powder in different regions is basically consistent. In this embodiment, the operating frequency of the vibrating screen is 50HZ.
[0028] (4) Cold isostatic pressing: like Figure 3 As shown, cold isostatic pressing is to place the sample to be pressed in a high-pressure container 6, and use the incompressible nature of the liquid medium and the property of uniformly transmitting pressure to uniformly pressurize the sample from all directions. When the liquid medium 7 is injected into the pressure container through a pressure pump, according to the principle of fluid mechanics, its pressure remains unchanged and is uniformly transmitted to all directions. The pressurization, pressure holding, and pressure relief processes are different in the molding process of ceramic powders of different shapes. In this embodiment, the cold isostatic pressing pressure is 110-130MPa.
[0029] (5) Rough machining: Since the size of the ceramic green body is not uniform after molding, removing excess powder through rough machining is beneficial to the placement during the sintering process and reduces the finishing time.
[0030] (6) Sintering. Due to the large size of the product, it is easy to crack due to uneven force during the sintering process. Therefore, the placement of the product before sintering and the selection of the sintering process are crucial. In this embodiment, the sintering platen requires a flatness of ±1°, 44# sintering sand is placed on the platen, and the sintering temperature is 1600℃~1640℃.
[0031] Embodiment 2: In this embodiment, a method for preparing a large-sized long ceramic strip includes the following steps: Step 1: Mold assembly: Place the PE inner bag in the inner cavity of the rubber mold body, and fix one side of the rubber mold body on the metal pressing plate; Step 2: Powder filling: The whole set of molds in step 1 is hoisted onto the vibration platform by a crane, and the vibration screen and the vibration platform are turned on. The AM alumina ceramic granulation powder with a purity greater than 99.7%, a bulk density of 1.24g / cm3, good fluidity, and uniform particle size distribution is sieved through the vibration screen to remove iron and then flows into the PE inner bag inside the mold body; Step 3: Vacuum and seal: After the powder filling is completed, the PE inner bag is vacuumed and sealed with a vacuum packaging machine, and the rubber mold cover is closed, and the mold and the pressing plate are tightly fixed with tape; Step 4: Cold isostatic pressing: hoist the mold filled with powder in step 3 into the cavity of the cold isostatic pressing equipment, set the pressure to 110 MPa to form a long ceramic green body; Step 5: Rough processing: Take out the formed long ceramic green body and place it in a rough processing lathe for processing, and process the plane of the long ceramic green body to meet the flatness of 0.05mm; Step 6: Sintering: After the sintering platen is fixed, when its flatness is measured to be less than 0.05 mm, 44# sintering sand is spread on the platen, and the rough-processed molded body in step 5 is placed on the platen. The sintering temperature is set to 1600°C to complete the preparation of large-size long ceramic strips.
[0032] Embodiment 3: In this embodiment, a method for preparing a large-sized long ceramic strip includes the following steps: Step 1: Mold assembly: Place the PE inner bag in the inner cavity of the rubber mold body, and fix one side of the rubber mold body on the metal pressing plate; Step 2: Powder filling: The whole set of molds in step 1 is hoisted onto the vibration platform by a crane, and the vibration screen and the vibration platform are turned on. The AM alumina ceramic granulation powder with a purity greater than 99.7%, a bulk density of 1.24g / cm3, good fluidity, and uniform particle size distribution is sieved through the vibration screen to remove iron and then flows into the PE inner bag inside the mold body; Step 3: Vacuum and seal: After the powder filling is completed, the PE inner bag is vacuumed and sealed with a vacuum packaging machine, and the rubber mold cover is closed, and the mold and the pressing plate are tightly fixed with tape; Step 4: Cold isostatic pressing: hoist the mold filled with powder in step 3 into the cavity of the cold isostatic pressing equipment, set the pressure to 120 MPa to form a long ceramic green body; Step 5: Rough processing: Take out the formed long ceramic green body and place it in a rough processing lathe for processing, and process the plane of the long ceramic green body to meet the flatness of 0.05mm; Step 6: Sintering: After the sintering platen is fixed, when its flatness is measured to be less than 0.05 mm, 44# sintering sand is spread on the platen, and the rough-processed molded body in step 5 is placed on the platen. The sintering temperature is set to 1620°C to complete the preparation of large-size long ceramic strips.
[0033] Embodiment 4: In this embodiment, a method for preparing a large-sized long ceramic strip includes the following steps: Step 1: Mold assembly: Place the PE inner bag in the inner cavity of the rubber mold body, and fix one side of the rubber mold body on the metal pressing plate; Step 2: Powder filling: The whole set of molds in step 1 is hoisted onto the vibration platform by a crane, and the vibration screen and the vibration platform are turned on. The AM alumina ceramic granulation powder with a purity greater than 99.7%, a bulk density of 1.24g / cm3, good fluidity, and uniform particle size distribution is sieved through the vibration screen to remove iron and then flows into the PE inner bag inside the mold body; Step 3: Vacuum and seal: After the powder filling is completed, the PE inner bag is vacuumed and sealed with a vacuum packaging machine, and the rubber mold cover is closed, and the mold and the pressing plate are tightly fixed with tape; Step 4: Cold isostatic pressing: hoist the mold filled with powder in step 3 into the cavity of the cold isostatic pressing equipment, set the pressure to 130 MPa to form a long ceramic green body; Step 5: Rough processing: Take out the formed long ceramic green body and place it in a rough processing lathe for processing, and process the plane of the long ceramic green body to meet the flatness of 0.05mm; Step 6: Sintering: After the sintering platen is fixed, when its flatness is measured to be less than 0.05 mm, 44# sintering sand is spread on the platen, and the rough-processed molded body in step 5 is placed on the platen. The sintering temperature is set at 1640°C to complete the preparation of large-size long ceramic strips.
[0034] Embodiment 5: A method for preparing large-sized long ceramic strips, which is suitable for preparing multiple large-sized long ceramic strips, comprises the following steps: (1) Selection of granulation powder; ① It has a certain particle gradation to ensure the normal growth of ceramic grains and normal grain size after sintering; ② The powder has high purity, certain fluidity, and moderate bulk density, which is conducive to powder filling operation and improves the density after powder filling. The ceramic green body has high density after cold pressing, and the ceramic density and bending strength are high after sintering.
[0035] The alumina ceramic granulation powder preferably has a purity greater than 99.7%, a bulk density of 1.24 g / cm3, good fluidity, a substantially spherical powder shape, and a uniform particle size distribution.
[0036] (2) Mold design: The mold includes a rubber mold body, a PE inner bag and a cover plate. An inner cavity is set inside the mold body. The size of the rubber mold inner cavity is designed according to the molding shrinkage rate. The size design of the PE inner bag needs to ensure that the size after molding meets the expected requirements. The mold design process after molding also needs to consider that the straightness of the strip after molding meets the ±1° requirement. Therefore, the mold also includes a metal iron plate. The design size of the fixed metal iron plate matches the mold body. The PE inner bag adopts an integrated arrangement with multiple longitudinal cavities, which can form multiple large-sized long ceramic products at one time.
[0037] (3) Powder filling operation: The powder filling operation includes powder screening and iron removal and vibration filling. The purity of the powder and the filling density of the powder are the main factors affecting the performance of the ceramic after sintering. Therefore, a vibrating screen is required to remove iron and impurities before powder filling. When filling powder, the frequency of the vibration platform is moderate, maintained at 20HZ~40HZ, which improves the filling density while ensuring the uniformity of the distribution of the powder in the mold, that is, the particle size distribution of the powder filled in each longitudinal inner bag cavity is basically the same. The particle size distribution of the powder in different longitudinal inner bag cavities can be set to be different according to product needs.
[0038] (4) Cold isostatic pressing: Cold isostatic pressing is to place the sample to be pressed in a high-pressure container, and use the incompressible nature of the liquid medium and the property of uniformly transmitting pressure to uniformly pressurize the sample from all directions. When the liquid medium is injected into the pressure container through a pressure pump, according to the principles of fluid mechanics, its pressure remains unchanged and is uniformly transmitted to all directions. The pressurization, pressure holding, and pressure relief processes are different in the molding process of ceramic powders of different shapes. In this embodiment, the cold isostatic pressing pressure is 130-150MPa.
[0039] (5) Rough machining: Since the size of the ceramic green body is not uniform after molding, removing excess powder through rough machining is beneficial to the placement during the sintering process and reduces the finishing time.
[0040] (6) Sintering. Due to the large size of the product, it is easy to crack due to uneven force during the sintering process. Therefore, the placement of the product before sintering and the selection of the sintering process are crucial. In this embodiment, the sintering platen requires a flatness of ±1°, 44# sintering sand is placed on the platen, and the sintering temperature is 1640℃~1660℃.
[0041] This method can form multiple large-sized long ceramic products at one time.
[0042] Embodiment 6: A method for preparing a large-sized long ceramic strip, which is suitable for making a large-sized variable-diameter long ceramic strip product, comprises the following steps: (1) Selection of granulation powder; ① It has a certain particle gradation to ensure the normal growth of ceramic grains and normal grain size after sintering; ② The powder has high purity, certain fluidity, and moderate bulk density, which is conducive to powder filling operation and improves the density after powder filling. The ceramic green body has high density after cold pressing, and the ceramic density and bending strength are high after sintering.
[0043] The alumina ceramic granulation powder preferably has a purity greater than 99.7%, a bulk density of 1.24 g / cm3, good fluidity, a substantially spherical powder shape, and a uniform particle size distribution.
[0044] (2) Mold design: like Figure 4 As shown, the mold includes a rubber mold body, a PE inner bag and a cover plate. An inner cavity is provided inside the mold body, and the size of the rubber mold inner cavity is designed according to the molding shrinkage rate. The size design of the PE inner bag needs to ensure that the size after molding meets the expected requirements. The mold design process after molding also needs to consider that the straightness of the long strip after molding meets the ±1° requirement. Therefore, the mold also includes a metal iron plate, and the design size of the fixed metal iron plate matches the mold body. The PE inner bag adopts an integrated variable diameter inner bag cavity, and the shape of the inner bag cavity is set according to the shape of the product. For example, if a variable diameter large-sized long ceramic product needs to be molded, the cavity diameter size of the inner bag cavity needs to be set according to the variable diameter size, so as to realize the one-time molding of a variable diameter large-sized long ceramic product. (3) Powder filling operation: The powder filling operation includes powder screening and iron removal and vibration filling. The purity of the powder and the filling density of the powder are the main factors affecting the performance of the ceramic after sintering. Therefore, a vibrating screen is required to remove iron and impurities before powder filling. When filling powder, the frequency of the vibration platform is moderate, maintained at 40HZ~60HZ, which improves the filling density while ensuring the uniformity of the distribution of the powder in the mold, that is, the particle size distribution of the powder filled in each longitudinal inner bag cavity is basically the same. The particle size distribution of the powder in different longitudinal inner bag cavities can be set to be different according to product needs.
[0045] (4) Cold isostatic pressing: Cold isostatic pressing is to place the sample to be pressed in a high-pressure container, and use the incompressible nature of the liquid medium and the property of uniformly transmitting pressure to uniformly pressurize the sample from all directions. When the liquid medium is injected into the pressure container through a pressure pump, according to the principles of fluid mechanics, its pressure remains unchanged and is uniformly transmitted to all directions. The pressurization, pressure holding, and pressure relief processes are different in the molding process of ceramic powders of different shapes. In this embodiment, the cold isostatic pressing pressure is 150-180MPa.
[0046] (5) Rough machining: Since the size of the ceramic green body is not uniform after molding, removing excess powder through rough machining is beneficial to the placement during the sintering process and reduces the finishing time.
[0047] (6) Sintering. Due to the large size of the product, it is easy to crack due to uneven force during the sintering process. Therefore, the placement of the product before sintering and the selection of the sintering process are crucial. In this embodiment, the sintering table requires a flatness of ±1°, 44# sintering sand is placed on the table, and the sintering temperature is 1660℃~1680℃.
[0048] This method can form long ceramic products with variable diameter and large size in one step.
[0049] Embodiment 7: A method for preparing large-sized long strip ceramics, which is applicable to irregular large-sized long strip ceramic products, comprises the following steps: (1) Selection of granulation powder; ① It has a certain particle gradation to ensure the normal growth of ceramic grains and normal grain size after sintering; ② The powder has high purity, certain fluidity, and moderate bulk density, which is conducive to powder filling operation and improves the density after powder filling. The ceramic green body has high density after cold pressing, and the ceramic density and bending strength are high after sintering.
[0050] The alumina ceramic granulation powder preferably has a purity greater than 99.7%, a bulk density of 1.24 g / cm3, good fluidity, a substantially spherical powder shape, and a uniform particle size distribution.
[0051] (2) Mold design: like Figure 5 As shown, the mold includes a rubber mold body, a PE inner bag and a cover plate. An irregular inner cavity is set inside the mold body. The size of the rubber mold inner cavity is designed according to the molding shrinkage rate. The size design of the PE inner bag needs to ensure that the size after molding meets the expected requirements. The mold design process after molding also needs to consider that the straightness of the long strip after molding meets the ±1° requirement. Therefore, the mold also includes a metal iron plate. The design size of the fixed metal iron plate matches the mold body. The PE inner bag adopts an integrated inner bag cavity that matches the irregular product, and the shape of the inner bag cavity is set according to the shape of the product.
[0052] (3) Powder filling operation: The powder filling operation includes powder screening and iron removal and vibration filling. The purity of the powder and the filling density of the powder are the main factors affecting the performance of the ceramic after sintering. Therefore, a vibrating screen is required to remove iron and impurities before powder filling. When filling powder, the frequency of the vibration platform is moderate, maintained at 60HZ~80HZ, which improves the filling density while ensuring the uniformity of the distribution of the powder in the mold, that is, the particle size distribution of the powder filled in each longitudinal inner bag cavity is basically the same. The particle size distribution of the powder in different longitudinal inner bag cavities can be set to be different according to product needs.
[0053] (4) Cold isostatic pressing: Cold isostatic pressing is to place the sample to be pressed in a high-pressure container, and use the incompressible nature of the liquid medium and the property of uniformly transmitting pressure to uniformly pressurize the sample from all directions. When the liquid medium is injected into the pressure container through a pressure pump, according to the principles of fluid mechanics, its pressure remains constant and is uniformly transmitted to all directions. The pressurization, pressure holding, and pressure relief processes are different in the molding process of ceramic powders of different shapes. In this embodiment, the cold isostatic pressing pressure is 180-200MPa.
[0054] (5) Rough machining: Since the size of the ceramic green body is not uniform after molding, removing excess powder through rough machining is beneficial to the placement during the sintering process and reduces the finishing time.
[0055] (6) Sintering. Due to the large size of the product, it is easy to crack due to uneven force during the sintering process. Therefore, the placement of the product before sintering and the selection of the sintering process are crucial. In this embodiment, the sintering table requires a flatness of ±1°, 44# sintering sand is placed on the table, and the sintering temperature is 1680℃~1700℃.
[0056] This method can form irregular shaped large-sized long ceramic products in one go.
[0057] The results of the large-sized long ceramic strips prepared in the above examples are evaluated as follows: Green density g / cm3 2.366 Sintered body density g / cm3 3.935 Bending strength MPa 398 By evaluating the performance of long ceramic strips, their use requirements can be met.
[0058] The large-size long ceramic preparation method is particularly suitable for the rapid prototyping of large-size long ceramic strips of 2000 mm and above. Through the selection of the purity and particle gradation of alumina granulation powder, the selection and design of the forming mold, the selection of the mold sealing and the pressure during the forming process, and the selection of the sintering process, the rapid manufacturing of large-size long ceramic strips is effectively achieved, which saves costs and improves production efficiency.
[0059] The above-described embodiments are only preferred solutions of the present invention and are not intended to limit the present invention in any form. Other variations and modifications are possible without exceeding the technical solutions described in the claims.
Claims
1. A method for preparing large-size long ceramic strips, characterized in that The following steps are involved: Step 1: Make a long strip mold; Step 2: Powder filling: install the whole set of molds on the vibration platform, turn on the vibration platform, and fill the alumina ceramic granulation powder into the mold; Step 3: Vacuum and seal: After filling the powder, use a vacuum packaging machine to vacuum and seal the PE inner bag; Step 4: Cold isostatic pressing: hoist the mold filled with powder in step 3 into the cavity of the cold isostatic pressing equipment as a whole, and perform cold isostatic pressing to form a long ceramic green body; Step 5: Sintering: After the sintering plate is covered with sintering sand, the long ceramic green body is placed on the sintering plate for sintering, and finally a large-sized long ceramic product is made.
2. The method for preparing large-size long ceramic strips according to claim 1, characterized in that: The mold comprises a rubber mold body (2), a PE inner bag (3) and a cover plate (4), and an inner cavity (5) is designed inside the mold body (2) according to the molding shrinkage rate; the mold (1) also comprises a metal iron plate for fixing, and the size of the metal iron plate is set to match the mold.
3. The method for preparing large-size long ceramic strips according to claim 2, characterized in that: The inner cavity (5) is a regular cavity; or the inner cavity (5) is a cavity with a variable diameter; or the inner cavity (5) is an irregular cavity.
4. The method for preparing large-size long ceramic strips according to claim 2, characterized in that: The PE inner bag (3) is a regular long strip structure; or the PE inner bag (3) has a variable diameter long strip structure; or the PE inner bag (3) is an irregular long strip structure.
5. The method for preparing large-size long ceramic strips according to any one of claims 1 to 4, characterized in that: The purity of the alumina ceramic granulated powder is greater than 99.7%, the bulk density is 1.24 g / cm3, and the powder is spherical.
6. The method for preparing large-size long ceramic strips according to any one of claims 1 to 4, characterized in that: The powder filling in step 2 includes powder screening to remove iron and vibration filling. A vibrating screen is used to remove iron and impurities before powder filling. During powder filling, the frequency of the vibration platform is maintained at 20HZ to 80HZ.
7. The method for preparing large-size long ceramic strips according to any one of claims 1 to 4, characterized in that: In step 4, a high-pressure container is used for cold isostatic pressing, and a liquid medium is injected into the high-pressure container through a pressure pump for uniform pressurization. The cold isostatic pressing pressure is 110 to 200 MPa.
8. The method for preparing large-size long ceramic strips according to any one of claims 1 to 4, characterized in that: In step 6, the sintering sand uses 44# sintering sand, and the sintering temperature is 1600°C to 1770°C.
9. The method for preparing large-size long ceramic strips according to any one of claims 1 to 4, characterized in that: The sintering platen in step 6 requires a flatness of ±1°.
10. The method for preparing large-size long ceramic strips according to any one of claims 1 to 4, characterized in that: Before sintering, the surface of the long ceramic green body is roughly processed to form a long ceramic formed body.