Preparation method and device of silicon wafer

By controlling the temperature and cutting depth in stages during the silicon wafer cutting process, and using the thermal expansion and contraction characteristics of the mechanical structure, the problem of high warp parameters during the silicon wafer cutting process is solved, and the quality of the silicon wafer is significantly improved.

CN119077995APending Publication Date: 2024-12-06ZHONGHUAN ADVANCED SEMICONDUCTOR TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411422551.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-12
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing silicon wafer preparation methods lead to higher warp parameters of silicon wafers during the cutting process, affecting their quality.

Method used

By controlling the temperature and cutting depth in stages in the cutting machine, the thermal expansion and contraction characteristics of the mechanical structure are used to change the morphology of the silicon wafer, thereby reducing the warp parameters. The specific steps include setting the first reaction temperature T1 in the cutting machine, raising the temperature to the second reaction temperature T2 for the first cutting, maintaining T2 for the second cutting, cooling to the third reaction temperature T3 for the third cutting, and maintaining at T3 Cut the fourth, until the cutting is completed.

Benefits of technology

The warp parameters of the silicon wafer are significantly reduced and the flatness and quality of the silicon wafer are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119077995A_ABST
    Figure CN119077995A_ABST
Patent Text Reader

Abstract

The invention provides a silicon wafer preparation method and device, and the method comprises the following steps: providing a crystal bar, placing the crystal bar in a cutting machine, and enabling the temperature in the cutting machine to have a first reaction temperature T1; raising the temperature to a second reaction temperature T2, and synchronously carrying out first cutting treatment; maintaining the second reaction temperature T2, and synchronously carrying out second cutting treatment; cooling to a third reaction temperature T3, and synchronously carrying out third cutting treatment; maintaining the third reaction temperature T3, and synchronously carrying out fourth cutting treatment until the cutting of the crystal bar is completed, so as to obtain a silicon wafer; wherein T2 > = T3 > = T1. By cutting the crystal bar in stages and controlling the temperature change of different depths in the cutting process of the crystal bar, the wafer body morphology of the silicon wafer formed by cutting can be changed by utilizing the characteristic of thermal expansion and cold contraction of a mechanical structure, so that the warp parameter is reduced, and the quality of the silicon wafer is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of semiconductor manufacturing, and specifically relates to a method and device for preparing a silicon wafer. Background Art

[0002] Silicon wafers are the most important semiconductor materials. Integrated circuit chips and sensors are manufactured based on semiconductor single crystal silicon wafers. With the increasing requirements for the surface quality of silicon wafers, there are requirements for no damage layer, less roughness and better flatness. Therefore, the process requirements for preparing silicon wafers are also gradually increasing.

[0003] The current common method is to use wire cutting to process the crystal rod into silicon wafers. During the cutting process, the silicon wafer will be partially deformed, resulting in defects. How to improve the existing crystal rod cutting process to reduce the parameters such as the warp of the silicon wafer is a problem that needs to be solved. Summary of the invention

[0004] The present invention provides a method and device for preparing a silicon wafer, aiming to solve the problem that the warp parameter of the existing silicon wafer preparation method is high during the cutting process, resulting in unsatisfactory silicon wafer quality.

[0005] The first embodiment of the present application provides a method for preparing a silicon wafer, comprising the following steps:

[0006] Providing a crystal rod, and placing the crystal rod in a cutting machine, wherein the cutting machine has a first reaction temperature T1;

[0007] The temperature is raised to the second reaction temperature T2, and the first cutting process is performed simultaneously;

[0008] Maintaining the second reaction temperature T2, and simultaneously performing the second cutting process;

[0009] Cooling down to the third reaction temperature T3, and simultaneously performing the third cutting process;

[0010] Maintaining the third reaction temperature T3, and simultaneously performing the fourth cutting process until the cutting of the crystal rod is completed to obtain the silicon wafer;

[0011] Among them, T2>T3≥T1.

[0012] In some embodiments, the endpoint of the first cutting process step has a first cutting depth x1%, the endpoint of the second cutting process step has a second cutting depth x2%, and the endpoint of the third cutting process step has a third cutting depth x3%, satisfying at least one of the following characteristics:

[0013] i) T2-T1=(0.05-0.5)x1;

[0014] ii)T2-T3=(0~0.375)(x3-x2).

[0015] In some embodiments, the first reaction temperature T1 and the second reaction temperature T2 satisfy:

[0016] 1℃≤T2-T1≤5℃.

[0017] In some embodiments, the second reaction temperature T2 and the third reaction temperature T3 satisfy:

[0018] T1<T3.

[0019] In some embodiments, the first reaction temperature T1 satisfies: 21°C≤T1≤25°C.

[0020] In some embodiments, the second reaction temperature T2 satisfies: 24°C≤T2≤26°C.

[0021] In some embodiments, the third reaction temperature T3 satisfies: 23°C≤T3≤25°C.

[0022] In some embodiments, the first cutting depth x1% and the second cutting depth x2% satisfy:

[0023] x1:x2=1:4~6.

[0024] In some embodiments, the second cutting depth x2% and the third cutting depth x3% satisfy:

[0025] x2:x3=1:1.05~1.5.

[0026] In some embodiments, the first cutting depth x1% satisfies: 10%≤x1%≤15%.

[0027] In some embodiments, the second cutting depth x2% satisfies: 50%≤x2%≤65%.

[0028] In some embodiments, the third cutting depth x3% satisfies: 70%≤x3%≤75%.

[0029] In some embodiments, the first cutting process step has a first cutting rate v1, the second cutting process step has a second cutting rate v2, the third cutting process step has a third cutting rate v3, and the fourth cutting process step has a fourth cutting rate v4, satisfying:

[0030] v3≤v4≤v2≤v1.

[0031] In some embodiments, the first cutting rate v1 satisfies: 0.26 mm / min≤v1≤0.4 mm / min.

[0032] In some embodiments, the second cutting rate v2 satisfies: 0.2 mm / min≤v2≤0.25 mm / min.

[0033] In some embodiments, the third cutting rate v3 satisfies: 0.18 mm / min≤v3≤0.21 mm / min.

[0034] In some embodiments, the fourth cutting rate v4 satisfies: 0.21 mm / min≤v4≤0.3 mm / min.

[0035] In some embodiments, the crystal rod is cut by sanding.

[0036] A second embodiment of the present application provides a silicon wafer preparation device, comprising:

[0037] A heat transfer module, used for fixing the crystal rod to be cut and transferring temperature to the crystal rod;

[0038] Cutting module, used for cutting crystal rods;

[0039] The control module is used to control the cutting machine to have a first reaction temperature T1; control the heat transfer module to heat up to a second reaction temperature T2, and synchronously control the cutting module to perform a first cutting process; control the heat transfer module to maintain the second reaction temperature T2, and synchronously control the cutting module to perform a second cutting process; control the heat transfer module to cool down to a third reaction temperature T3, and synchronously control the cutting module to perform a third cutting process; control the heat transfer module to maintain the third reaction temperature T3, and synchronously control the cutting module to perform a fourth cutting process until the cutting of the crystal rod is completed to obtain the silicon wafer.

[0040] In some embodiments, the cutting module is provided with a cutting wire for cutting, so that the cutting module can perform wire cutting on the crystal rod.

[0041] The present application provides a method for preparing a silicon wafer, comprising the following steps: providing a crystal rod, placing the crystal rod in a cutting machine, wherein the cutting machine has a first reaction temperature T1; heating to a second reaction temperature T2, and simultaneously performing a first cutting process; maintaining the second reaction temperature T2, and simultaneously performing a second cutting process; cooling to a third reaction temperature T3, and simultaneously performing a third cutting process; maintaining the third reaction temperature T3, and simultaneously performing a fourth cutting process until the cutting of the crystal rod is completed to obtain a silicon wafer; wherein T2>T3≥T1. By cutting the crystal rod in stages and controlling the temperature changes at different depths during the cutting of the crystal rod, the characteristics of thermal expansion and contraction of the mechanical structure can be utilized to change the body morphology of the silicon wafer formed by cutting, thereby reducing the warp parameter and improving the quality of the silicon wafer. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] The technical solution and other beneficial effects of the present application will be made apparent by describing in detail the specific implementation methods of the present application in conjunction with the accompanying drawings.

[0043] Figure 1 A flow chart of a method for preparing a silicon wafer provided in an embodiment of the present application;

[0044] Figure 2 A schematic diagram of a first cutting process in a method for preparing a silicon wafer provided in an embodiment of the present application;

[0045] Figure 3 A schematic diagram of a second cutting process in a method for preparing a silicon wafer provided in an embodiment of the present application;

[0046] Figure 4 A schematic diagram of a third cutting process in a method for preparing a silicon wafer provided in an embodiment of the present application;

[0047] Figure 5 This is a comparison chart of the surface test results of the silicon wafers prepared in Example 2 of the present application and Comparative Example 1;

[0048] Reference numerals:

[0049] 10-crystal rod, 20-sand line, Y-first direction. DETAILED DESCRIPTION

[0050] The technical solutions in the embodiments of the present application will be described clearly and completely below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present application.

[0051] In the description of the present application, it should be noted that, unless otherwise clearly specified and limited, the terms "connected" and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection, an electrical connection, or can communicate with each other; it can be directly connected, or indirectly connected through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to the specific circumstances. In the description of the present application, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined. In addition, the terms "first" and "second" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more features.

[0052] The disclosure below provides many different embodiments or examples to realize the different structures of the present application. In order to simplify the disclosure of the present application, the parts and settings of specific examples are described below. Of course, they are only examples, and the purpose is not to limit the present application.

[0053] The first embodiment of the present application provides a method for preparing a silicon wafer, see Figure 1 , including the following steps:

[0054] Providing a crystal rod 10, placing the crystal rod 10 in a cutting machine, wherein the cutting machine has a first reaction temperature T1;

[0055] The temperature is raised to the second reaction temperature T2, and the first cutting process is performed simultaneously;

[0056] Maintaining the second reaction temperature T2, and simultaneously performing the second cutting process;

[0057] Cooling down to the third reaction temperature T3, and simultaneously performing the third cutting process;

[0058] The third reaction temperature T3 is maintained, and the fourth cutting process is performed simultaneously until the cutting of the crystal rod 10 is completed to obtain a silicon wafer;

[0059] Among them, T2>T3≥T1.

[0060] Specifically, the cutting machine includes a frame and a sand wire 20. During the first cutting process, the second cutting process, the third cutting process and the fourth cutting process of the crystal rod 10, the crystal rod 10 is fixed on the frame, and the sand wire 20 cuts the crystal rod 10 along the radial section of the crystal rod 10 to obtain a silicon wafer. The control of the first reaction temperature, the second reaction temperature and the third reaction temperature in the cutting machine can be achieved by controlling the temperature of the frame.

[0061] By cutting the crystal rod 10 in stages and controlling the temperature changes at different depths during the cutting process of the crystal rod 10, the thermal expansion and contraction characteristics of the mechanical structure can be used to change the physical deformation of the frame, thereby driving the displacement of the single crystal crystal rod 10. During the cutting process, the displacement of the single crystal crystal rod 10 is changed so that it is relatively level with the cutting wire grid, thereby changing the body morphology of the silicon wafer, thereby reducing the warp parameter and improving the quality of the silicon wafer.

[0062] In some embodiments, the endpoint of the first cutting process step has a first cutting depth x1%, the endpoint of the second cutting process step has a second cutting depth x2%, and the endpoint of the third cutting process step has a third cutting depth x3%, satisfying at least one of the following characteristics:

[0063] i) T2-T1=(0.05-0.5)x1;

[0064] ii)T2-T3=(0~0.375)(x3-x2).

[0065] Specifically, see Figure 2 to Figure 4 The radial cross section of the cut crystal rod 10 has a maximum size D. During the cutting process, the sand wire 20 moves along the first direction Y from the top edge of the radial cross section of the crystal rod 10 to the bottom edge of the radial cross section of the crystal rod 10 to complete the cutting of the crystal rod 10, thereby obtaining a silicon wafer. Figure 2 When the first cutting process step is performed, the moving distance of the sand wire 20 along the first direction Y is L1, wherein the first cutting depth x1% refers to the ratio of L1 / D; see Figure 3 When the second cutting process is performed, the moving distance of the sand wire 20 along the first direction Y is L2, wherein the second cutting depth x2% refers to the ratio of L2 / D; see Figure 4 When the third cutting process step is performed, the moving distance of the sand line 20 along the first direction Y is L3, wherein the third cutting depth x3% refers to the ratio of L3 / D. Since the cutting depth affects the degree of heating of the crystal rod 10, and further affects the displacement of the crystal rod 10, when the relationship between the first reaction temperature, the second reaction temperature, the third reaction temperature and the first cutting depth, the second cutting depth, and the third cutting depth satisfies equations i and ii, the temperature of each cutting process stage can be matched with the displacement of the crystal rod 10, the morphology of the silicon wafer can be balanced to the greatest extent, and the warp parameter can be reduced.

[0066] In some embodiments, the first reaction temperature T1 and the second reaction temperature T2 satisfy:

[0067] 1℃≤T2-T1≤5℃.

[0068] It is understandable that the value of T2-T1 (unit: °C) can be any value among 1, 2, 3, 4, 5 or a range between any two values. As the cutting depth increases, the heat generated during the cutting process will also increase. Controlling the reaction temperature to increase appropriately can reduce the friction and shear force during the cutting process, thereby reducing scratches and unevenness on the surface of the silicon wafer. When T2-T1 meets the above value range, it can improve the cutting process, especially the quality of the silicon wafer surface in the second cutting process and the third cutting process, while avoiding excessive displacement of the crystal rod 10 due to excessive temperature rise and excessive temperature difference, resulting in a high warp parameter.

[0069] In some embodiments, the second reaction temperature T2 and the third reaction temperature T3 satisfy:

[0070] T1<T3.

[0071] Controlling the reaction temperature of the third cutting process stage and the fourth cutting process stage between the first reaction temperature and the second reaction temperature can prevent cracks and warping on the surface of the silicon wafer as the cutting depth increases.

[0072] In some embodiments, the first reaction temperature T1 satisfies: 21°C≤T1≤25°C.

[0073] It can be understood that the value of the first reaction temperature T1 (unit: °C) can be any value among 21, 22, 23, 24, 25 or a range between any two values.

[0074] In some embodiments, the second reaction temperature T2 satisfies: 24°C≤T2≤26°C.

[0075] It can be understood that the value of the second reaction temperature T2 (unit: °C) can be any value among 24, 24.5, 25, 25.5, 26 or a range between any two values.

[0076] In some embodiments, the third reaction temperature T3 satisfies: 23°C≤T3≤25°C.

[0077] It can be understood that the value of the third reaction temperature T3 (unit: °C) can be any value among 23, 23.5, 24, 24.5, 25 or a range between any two values.

[0078] When the first reaction temperature T1, the second reaction temperature T2, and the third reaction temperature T3 satisfy the above value range, the physical deformation of the frame during each stage of cutting the crystal rod 10 can be within an ideal range, thereby ensuring that the surface of the crystal rod 10 during the cutting process has an ideal morphology.

[0079] In some embodiments, the first cutting depth x1% and the second cutting depth x2% satisfy:

[0080] x1:x2=1:4~6.

[0081] It is understandable that the value of x1:x2 can be any value of 1:4, 1:5, 1:6 or a range between any two values. Since the temperature is raised simultaneously during the first cutting process, too fast a temperature rise may make the surface of the silicon rod unable to adapt to the temperature change, resulting in cracks or warping, while too slow a temperature rise may affect the cutting accuracy. Therefore, when the first cutting depth and the second cutting depth meet the above-mentioned proportional relationship, it can further ensure that the temperature and the displacement of the crystal rod 10 are matched during the cutting process, thereby reducing the warp parameter.

[0082] In some embodiments, the second cutting depth x2% and the third cutting depth x3% satisfy:

[0083] x2:x3=1:1.05~1.5.

[0084] It is understandable that the value of x2:x3 can be any value of 1:1.05, 1:1.1, 1:1.2, 1:1.3, 1:1.4, 1:1.5 or a range between any two values. Based on a similar principle, when the second cutting depth and the third cutting depth satisfy the above proportional relationship, it can further ensure that the temperature during the cutting process matches the displacement of the crystal rod 10, thereby reducing the warp parameter.

[0085] In some embodiments, the first cutting depth x1% satisfies: 10%≤x1%≤15%.

[0086] It can be understood that the value of the first cutting depth x1% can be any value of 10%, 11%, 12%, 13%, 14%, 15%, or a range between any two values.

[0087] In some embodiments, the second cutting depth x2% satisfies: 50%≤x2%≤65%.

[0088] It can be understood that the value of the second cutting depth x2% can be any value of 50%, 52%, 54%, 56%, 58%, 60%, 62%, 65%, or a range between any two values.

[0089] In some embodiments, the third cutting depth x3% satisfies: 70%≤x3%≤75%.

[0090] It can be understood that the value of the third cutting depth x3% can be any value of 70%, 71%, 72%, 73%, 74%, 75%, or a range between any two values.

[0091] When the first cutting depth x1%, the second cutting depth x2%, and the third cutting depth x3% meet the above value range, it can further ensure that the cutting of the crystal rod 10 has a reasonable cutting area at each stage, thereby ensuring that the surface of the crystal rod 10 has an ideal morphology during the cutting process.

[0092] In some embodiments, the first cutting process step has a first cutting rate v1, the second cutting process step has a second cutting rate v2, the third cutting process step has a third cutting rate v3, and the fourth cutting process step has a fourth cutting rate v4, satisfying:

[0093] v3≤v4≤v2≤v1.

[0094] By changing the single crystal cutting depth and the different diameters of the wafer when the steel wire is cutting, the table cutting rate can be controlled, which can effectively ensure the consistency of the line loss in the entire processing process and reduce the fluctuation of warp parameters caused by the variables generated by the steel wire.

[0095] In some embodiments, the first cutting rate v1 satisfies: 0.26 mm / min≤v1≤0.4 mm / min.

[0096] It can be understood that the value of the first cutting rate v1 (unit: mm / min) can be any value among 0.26, 0.3, 0.34, 0.38, 0.4, or a range between any two values.

[0097] In some embodiments, the second cutting rate v2 satisfies: 0.2 mm / min≤v2≤0.25 mm / min.

[0098] It can be understood that the value of the second cutting rate v2 (unit: mm / min) can be any value among 0.2, 0.21, 0.22, 0.23, 0.24, 0.25 or a range between any two values.

[0099] In some embodiments, the third cutting rate v3 satisfies: 0.18 mm / min≤v3≤0.21 mm / min.

[0100] It can be understood that the value of the third cutting rate v3 (unit: mm / min) can be any value among 0.18, 0.19, 0.2, 0.21 or a range between any two values.

[0101] In some embodiments, the fourth cutting rate v4 satisfies: 0.21 mm / min≤v4≤0.3 mm / min. In some embodiments, the crystal rod 10 is cut by the sand wire 20 .

[0102] It can be understood that the value of the fourth cutting rate v4 (unit: mm / min) can be any value among 0.21, 0.23, 0.25, 0.27, 0.29, 0.3, or a range between any two values.

[0103] When the first cutting rate v1, the second cutting rate v2, the third cutting rate v3 and the fourth cutting rate v4 meet the above value range, it can further ensure the consistency of wire loss during the processing and reduce the fluctuation of warp parameters caused by the variables generated by the steel wire.

[0104] A second embodiment of the present application provides a silicon wafer preparation device, comprising:

[0105] A heat transfer module, used for fixing the crystal rod 10 to be cut and transferring temperature to the crystal rod 10;

[0106] A cutting module, used for cutting the crystal rod 10;

[0107] The control module is used to control the first reaction temperature T1 in the cutting machine; control the heat transfer module to heat up to the second reaction temperature T2, and synchronously control the cutting module to perform the first cutting process; control the heat transfer module to maintain the second reaction temperature T2, and synchronously control the cutting module to perform the second cutting process; control the heat transfer module to cool down to the third reaction temperature T3, and synchronously control the cutting module to perform the third cutting process; control the heat transfer module to maintain the third reaction temperature T3, and synchronously control the cutting module to perform the fourth cutting process until the cutting of the crystal rod 10 is completed to obtain a silicon wafer.

[0108] In some embodiments, a cutting wire for cutting is provided in the cutting module so as to perform wire cutting on the crystal rod 10 .

[0109] The following is a description of the method and device for preparing a silicon wafer provided by the present application in conjunction with specific embodiments:

[0110] Example 1

[0111] This embodiment provides a method for preparing a silicon wafer, comprising the following steps:

[0112] S1, providing a crystal ingot 10, placing the crystal ingot 10 on a rack in a cutting machine, the rack being used to fix the crystal ingot 10 and conduct temperature to the crystal ingot 10, and setting the temperature of the rack to 21° C.;

[0113] The rack is controlled to heat up to 25° C., and the abrasive wire 20 is used to perform the first cutting process on the crystal rod 10 until the cutting depth reaches 11%;

[0114] The rack temperature is maintained at 25° C., and the abrasive wire 20 is used to perform a second cutting process on the crystal rod 10 until the cutting depth reaches 51%;

[0115] The rack temperature is maintained at 25° C., and the abrasive wire 20 is used to perform a third cutting process on the crystal rod 10 until the cutting depth reaches 73%;

[0116] The rack temperature is maintained at 25° C., and the sand wire 20 is used to perform the fourth cutting process on the crystal rod 10 until the cutting depth reaches 100%, and the cutting of the crystal rod 10 is completed to obtain a silicon wafer.

[0117] Embodiments 2 to 12

[0118] The methods for preparing silicon wafers provided in Examples 2 to 12 are consistent with those in Example 1, with the only difference being that the process parameters are adjusted.

[0119] Comparative Example 1

[0120] Comparative Example 1 provides a method for preparing a silicon wafer, comprising the following steps:

[0121] S1. Provide a crystal ingot 10, and place the crystal ingot 10 on a rack in a cutting machine. The rack is used to fix the crystal ingot 10 and transfer temperature to the crystal ingot 10. The temperature of the rack is set to 19° C.;

[0122] The rack is controlled to heat up to 23° C., and the abrasive wire 20 is used to perform the first cutting process on the crystal rod 10 until the cutting depth reaches 11%;

[0123] The rack temperature is maintained at 23° C., and the sand wire 20 is used to perform a second cutting process on the crystal rod 10 until the cutting depth reaches 100%, and the cutting of the crystal rod 10 is completed to obtain a silicon wafer.

[0124] Comparative Examples 2 to 4

[0125] The preparation methods of silicon wafers provided in Comparative Examples 2 to 4 are consistent with those in Comparative Example 1, with the only difference being that the process parameters are adjusted.

[0126] The process parameters of Examples 1 to 12 and Comparative Examples 1 to 4 are shown in Table 1.

[0127] Table 1

[0128]

[0129]

[0130] The preparation method of Example 2 and the preparation method of Comparative Example 1 were repeated several times, and the surface of the prepared silicon wafer was tested for warp parameters. The Kobelco tester was used as the test equipment to perform surface scanning test on the silicon wafer. The test results are shown in Figure 5 .

[0131] according to Figure 5 It can be seen that the silicon wafer prepared in Example 2 generally has a lower warp parameter than the silicon wafer prepared in Comparative Example 1.

[0132] The warp parameter detection was performed on the silicon wafers of Examples 1 to 12 and Comparative Examples 1 to 4 using the same detection method as above. The results are shown in Table 2.

[0133] Table 2

[0134] Warp average value (μm) Example 1 8 Example 2 6 Example 3 6 Example 4 5 Example 5 7 Example 6 5 Example 7 7 Example 8 6 Example 9 4 Example 10 4 Embodiment 11 6 Example 12 7 Comparative Example 1 15 Comparative Example 2 11 Comparative Example 3 15 Comparative Example 4 13

[0135] According to Table 2, the silicon wafer obtained by the solution provided by the present application is cut in stages, and by controlling the temperature range of each stage, the warp parameter of the silicon wafer surface is significantly reduced, thereby improving the quality of the silicon wafer. According to Examples 2 to 12, it can be seen that by controlling the third reaction temperature to be lower than the second reaction temperature, the final quality of the silicon wafer can be further improved.

[0136] The above is a detailed introduction to a method and device for preparing a silicon wafer provided in the embodiments of the present application. Specific examples are used in the present application to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the technical solution and its core idea of ​​the present application. Ordinary technicians in this field should understand that they can still modify the technical solutions recorded in the aforementioned embodiments, or replace some of the technical features therein with equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present application.

Claims

1. A method for preparing a silicon wafer, characterized in that: The steps include: Providing a crystal rod, and placing the crystal rod in a cutting machine, wherein the cutting machine has a first reaction temperature T1; The temperature is raised to the second reaction temperature T2, and the first cutting process is performed simultaneously; Maintaining the second reaction temperature T2, and simultaneously performing the second cutting process; Cooling down to the third reaction temperature T3, and simultaneously performing the third cutting process; Maintaining the third reaction temperature T3, and simultaneously performing the fourth cutting process until the cutting of the crystal rod is completed to obtain the silicon wafer; Among them, T2>T3≥T1.

2. The method for preparing a silicon wafer according to claim 1, characterized in that: The end point of the first cutting process step has a first cutting depth x1%, the end point of the second cutting process step has a second cutting depth x2%, and the end point of the third cutting process step has a third cutting depth x3%, satisfying at least one of the following characteristics: i) T2-T1=(0.05-0.5)x1; ii)T2-T3=(0~0.375)(x3-x2).

3. The method for preparing a silicon wafer according to claim 1, characterized in that: The first reaction temperature T1 and the second reaction temperature T2 satisfy: 1℃≤T2-T1≤5℃.

4. The method for preparing a silicon wafer according to claim 1, characterized in that: The second reaction temperature T2 and the third reaction temperature T3 satisfy: T1<T3.

5. The method for preparing a silicon wafer according to claim 1, characterized in that: The first reaction temperature T1 satisfies: 21°C≤T1≤25°C; and / or, The second reaction temperature T2 satisfies: 24°C≤T2≤26°C; and / or, The third reaction temperature T3 satisfies: 23°C≤T3≤25°C.

6. The method for preparing a silicon wafer according to claim 2, characterized in that: The first cutting depth x1% and the second cutting depth x2% satisfy: x1:x2=1:4~6.

7. The method for preparing a silicon wafer according to claim 2, characterized in that: The second cutting depth x2% and the third cutting depth x3% satisfy: x2:x3=1:1.05~1.

5.

8. The method for preparing a silicon wafer according to claim 2, characterized in that: The first cutting depth x1% satisfies: 10%≤x1%≤15%; and / or, The second cutting depth x2% satisfies: 50%≤x2%≤65%; and / or, The third cutting depth x3% satisfies: 70%≤x3%≤75%.

9. The method for preparing a silicon wafer according to claim 1, characterized in that: The first cutting process step has a first cutting rate v1, the second cutting process step has a second cutting rate v2, the third cutting process step has a third cutting rate v3, and the fourth cutting process step has a fourth cutting rate v4, satisfying: v3≤v4≤v2≤v1.

10. The method for preparing a silicon wafer according to claim 9, characterized in that: The first cutting rate v1 satisfies: 0.26 mm / min≤v1≤0.4 mm / min; and / or, The second cutting rate v2 satisfies: 0.2 mm / min≤v2≤0.25 mm / min; and / or, The third cutting rate v3 satisfies: 0.18 mm / min≤v3≤0.21 mm / min; and / or, The fourth cutting rate v4 satisfies: 0.21 mm / min≤v4≤0.3 mm / min.

11. The method for preparing a silicon wafer according to claim 1, characterized in that: The crystal rod is cut by sand wire.

12. A silicon wafer preparation device, used to complete the silicon wafer preparation method according to any one of claims 1 to 9, characterized in that: include: A heat transfer module, used for fixing the crystal rod to be cut and transferring temperature to the crystal rod; Cutting module, used for cutting crystal rods; The control module is used to control the cutting machine to have a first reaction temperature T1; control the heat transfer module to heat up to a second reaction temperature T2, and synchronously control the cutting module to perform a first cutting process; control the heat transfer module to maintain the second reaction temperature T2, and synchronously control the cutting module to perform a second cutting process; control the heat transfer module to cool down to a third reaction temperature T3, and synchronously control the cutting module to perform a third cutting process; control the heat transfer module to maintain the third reaction temperature T3, and synchronously control the cutting module to perform a fourth cutting process until the cutting of the crystal rod is completed to obtain the silicon wafer.

13. The silicon wafer preparation device according to claim 12, characterized in that: The cutting module is provided with a cutting wire for cutting, so that the cutting module can perform wire cutting on the crystal rod.