High-strength aluminum composite board, barrier layer for high-strength aluminum composite board and preparation method of barrier layer
By adding Ti, Sc, V or Hf elements to the barrier layer, the diffusion activation energy of Mg elements is improved, and the optimized three-layer structure is designed to solve the strength loss and welding problems caused by Mg element diffusion, achieving high strength and high strength Welding performance aluminum composite board.
Patent Information
- Application Number
- CN202411190603.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-28
AI Technical Summary
The existing high-strength aluminum composite panels have problems such as Mg element diffusion during brazing, and the existing barrier layer design is difficult to effectively block Mg element diffusion, affecting the overall material strength.
By adding Ti, Sc, V or Hf elements to the barrier layer, the total solid solubility is controlled to be at least 0.06 wt% to improve the diffusion activation energy of the Mg element, reduce the diffusion channel, reduce the barrier layer thickness or increase the core layer Mg element content, design the barrier layer-core layer-barrier layer structure of three-layer structure, optimize the grain morphology and orientation to prevent the diffusion of Mg elements.
Effectively block the diffusion of Mg elements, improve the strength and welding performance of composite materials, reduce the proportion of barrier layer thickness, and maintain high-strength Mg elements content to meet brazing requirements.
Smart Images

Figure CN119078306A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite plate brazing, and in particular to a high-strength aluminum composite plate and a barrier layer used therefor and a preparation method thereof. Background Art
[0002] With the rapid development of new energy vehicles, the demand for battery liquid cooling plates is growing. At the same time, in order to improve the range of new energy vehicles and overcome range anxiety, battery pack production technology is always in a rapid innovation process. In addition to continuous exploration in the battery field, in terms of liquid cooling plate materials, aluminum alloy materials with higher strength have also been in the process of iteration. The improvement of material strength can provide its upper limit of load-bearing as a structural part, and more importantly, it can reduce the thickness of the plate to achieve the purpose of lightweighting.
[0003] The idea of improving the strength performance of liquid cooling plate materials in the prior art is generally to use an alloy system containing elements such as Mg and Si that can provide precipitation strengthening, and higher strength can be obtained through aging heat treatment after brazing. However, the technical difficulties that cannot be avoided with high-strength brazing materials of the Al-Mg-Si alloy system are: the Mg element in the core layer is very easy to diffuse during the brazing process. On the one hand, the reduction of Mg content in the core layer leads to a loss of strength; on the other hand, if Mg diffuses to the surface of the material, it will cause flux poisoning and lead to poor welding. Therefore, Mg-containing alloys need to be used as the core layer and the barrier layers on the upper and lower surfaces to form a composite plate. How to design an effective barrier layer to prevent the diffusion of the Mg element, the prior art also provides some methods and ideas.
[0004] For example, CN114752829B discloses a composite aluminum alloy plate for a new energy power battery liquid cooling plate and a preparation method thereof, including a core layer and a protective layer. The core layer is an Al-Mg-Si alloy with a heat treatment strengthening effect, and the protective layer is an Al-Mn alloy or a 1xxx alloy. During the brazing process, the protective layer can prevent the Mg element of the core layer from diffusing to the surface, thereby avoiding the poisoning effect of Mg affecting the welding effect.
[0005] CN113897523A discloses a brazable high-strength aluminum alloy composite plate and its preparation method and application, which has a composite layer structure, including an upper barrier layer, a core layer and a lower barrier layer. Among them, the ratio of the grain intercept X parallel to the rolling direction to the grain intercept Y perpendicular to the rolling direction in the barrier layer is 2.5 to 9, X is at least 100um, and at least 90% of the longitudinal sections of the grains have <110> Grain orientation, by controlling grain morphology and grain orientation, hinders the diffusion of Mg element.
[0006] In summary, it is also necessary to design an effective barrier layer to block the diffusion of Mg elements and reduce the composite ratio of the barrier layer to improve the strength of the high-strength aluminum composite plate. Summary of the invention
[0007] In order to solve the above technical problems, the present invention provides a high-strength aluminum composite plate and a barrier layer and a preparation method thereof. It is worth noting that the function of the barrier layer is to prevent the Mg element in the core layer from diffusing to the surface of the high-strength aluminum composite plate. Therefore, the thickness of the barrier layer is determined by the diffusion depth of the Mg element in the core layer. The diffusion depth of the Mg element depends on the content concentration of the Mg element in the core layer on the one hand, and on the diffusion coefficient of the Mg element in the barrier layer on the other hand.
[0008] The diffusion coefficient of Mg is expressed as:
[0009] Where D is the diffusion coefficient, D0 is the diffusion constant, Q is the diffusion activation energy, R is the gas constant, which is 8.314 J / (mol·K), and T is the thermodynamic temperature.
[0010] The diffusion distance of Mg is expressed as:
[0011] Where λ is the diffusion distance, D is the diffusion coefficient, and t is the time.
[0012] The diffusion coefficient D of the barrier material can be calculated from the λ test value; the D0 and Q values can be calculated from the Mg diffusion distance in the sample after the same insulation time at a set of different temperatures. The larger the diffusion coefficient D, the stronger the ability to diffuse to the surface, and the larger Q, the smaller D, the more difficult it is to diffuse.
[0013] It is well known that in terms of liquid cooling plate materials, when Mg-Si reinforced materials are used as the substrate, a barrier layer needs to be compounded, that is, a barrier layer-core layer-barrier layer three-layer structure, wherein the core layer is set to a 6-series alloy or a 6-series modified alloy component with better strength. The more Mg and Si content in the core material is increased, the more magnesium-silicon aging strengthening phases are obtained through aging strengthening, and the higher the strength of the core material alloy; however, when the Mg content of the core material is higher, a thicker barrier layer needs to be compounded to avoid the risk of Mg diffusion to the surface (Mg diffusion to the surface will cause the surface to turn yellow and react with the flux to affect the brazing performance). For composite materials, the strength of the material is affected by the strength level and thickness ratio of each composite material. Obviously, blindly increasing the Mg content of the core material will result in the gain of the core material Mg element to the overall composite material strength being lower than the loss of the overall composite material strength caused by the increase in the thickness of the barrier layer. The inventors are committed to the design of barrier layer materials and obtain a barrier layer with a low Mg diffusion coefficient, so that compared with the existing conventional barrier layer, at the same barrier layer thickness, more Mg elements can be added to the core layer, and the Mg element maintained in the core layer after welding is higher (after Mg diffuses into the barrier layer, the Mg content of the core material will decrease, and the higher the Mg diffusion degree and depth, the less Mg element content maintained in the core material); or at the same core layer Mg addition amount, the core layer can be designed to be thicker, and the Mg element maintained in the core layer after welding is higher, and the final result is that the strength of the composite material is higher.
[0014] The inventors have improved the diffusion activation energy of Mg in the barrier layer and the diffusion difficulty of Mg in the barrier layer by changing the material and structure of the existing barrier layer, and can relatively reduce the thickness of the barrier layer or further increase the Mg content in the core layer. In this way, the mechanical properties of the composite aluminum plate can be maintained while meeting the brazing requirements.
[0015] To achieve this object, the present invention adopts the following technical solutions:
[0016] In a first aspect, the present invention provides a barrier layer for a high-strength aluminum composite plate.
[0017] The barrier layer includes any one or a combination of at least two of the alloy elements Ti, Sc, V or Hf, and the alloy elements Ti, Sc, V or Hf are recorded as barrier elements;
[0018] The total solid solubility of the barrier elements in the barrier layer is at least 0.06 wt %.
[0019] It is worth noting that the role of the barrier layer is to prevent the Mg element in the core layer from diffusing to the surface of the composite aluminum plate. The inventors found in the experimental process that when the barrier layer contains Ti and / or Sc and / or V and / or Hf elements, although the grains are equiaxed, the grains are relatively small and uniform, and still have a good barrier effect on Mg diffusion; in particular, the effect of Hf element is better. According to analysis, at least one of Ti, Sc, V or Hf elements and controlling its total solid solubility to at least 0.06wt% can contribute to the improvement of diffusion activation energy.
[0020] Specifically: when the barrier layer contains Ti and / or Sc and / or V and / or Hf elements, and the precipitation amount of Ti and / or Sc and / or V and / or Hf elements is controlled to control the total solid solubility (solid solubility + precipitation amount = element content) to at least 0.06wt%, a higher diffusion activation energy can be obtained. It is speculated that Ti and / or Sc and / or V and / or Hf elements are easily combined with vacancies in the aluminum matrix, so that more Ti and / or Sc and / or V and / or Hf elements can be kept in a solid solution state, and more vacancies can be captured during the brazing process to form solute-vacancy coordination pairs, reduce vacancy concentration, reduce diffusion channels, and increase the diffusion activation energy of the Mg element.
[0021] Preferably, the addition of Hf element makes it easier to obtain higher diffusion activation energy. It is speculated that Hf can more easily capture vacancies during the brazing process, and its combination with vacancies is relatively stable, which can effectively reduce the vacancy concentration and increase the diffusion activation energy.
[0022] The total solid solubility of the added elements in the barrier layer is at least 0.06wt%, for example, it can be 0.06wt%, 0.07wt%, 0.08wt%, 0.09wt%, 0.1wt%, 0.12wt%, 0.13wt%, 0.15wt%, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt% or 0.6wt%, etc.
[0023] The total solid solubility of Ti and / or Sc and / or V and / or Hf elements is at least 0.06wt%; since Ti, Sc, V, and Hf have the property of easily forming solute-vacancy pairing with vacancies, the vacancy concentration can be reduced, and the solid solubility of these elements has a significant influence on the diffusion activation energy Q.
[0024] Preferably, the barrier layer includes recrystallized grains; the recrystallized grains are in the form of at least two layers of grains, and the grain boundary length per unit area accounts for less than 35%.
[0025] The recrystallized grains have at least two layers of grains, and the grain boundary length per unit area accounts for less than 35%, for example, it can be 3.0%, 3.5%, 4%, 5%, 10%, 15%, 20%, 25%, 30% or 35%, etc.
[0026] In the present invention, the recrystallized grain morphology is such that at least two layers of grains exist. When at least two layers of grains exist, it is not conducive to the diffusion of elements, and the overall diffusion activation energy Q can be improved. When the grain boundary length accounts for a small proportion, the grain boundary in the barrier layer is suppressed as a fast diffusion channel with low diffusion activation energy, which can improve the overall diffusion activation energy Q. If the structure is a single-layer grain, the grain boundary becomes a fast diffusion channel from the core layer to the surface, which reduces the diffusion activation energy. When the grain boundary length accounts for a large proportion, too many grain boundaries act as fast diffusion channels to reduce the diffusion activation energy.
[0027] By comprehensively regulating the recrystallized grains and the total solid solubility of the added elements, the diffusion activation energy of the Mg element in the barrier layer can be made higher than 150 kJ / mol.
[0028] Preferably, the diffusion activation energy of the Mg element in the barrier layer is greater than 150 kJ / mol, for example, it may be 151 kJ / mol, 152 kJ / mol, 153 kJ / mol, 154 kJ / mol, 155 kJ / mol, 158 kJ / mol or 160 kJ / mol.
[0029] Preferably, at least 0.05wt% of the barrier element is present in the aluminum alloy in the form of dispersed phase precipitation, for example, it can be 0.05wt%, 0.06wt%, 0.07wt%, 0.08wt%, 0.1wt%, 0.12wt%, 0.13wt%, 0.15wt% or 0.2wt%, etc.
[0030] Preferably, the dispersed phase in the barrier layer is an Al3X dispersed phase and / or an Al3(X,Y) dispersed phase.
[0031] In the present invention, part of the Ti and / or Sc and / or V and / or Hf elements are dissolved in the aluminum alloy, and the rest are precipitated in the form of Al3X or Al3(X,Y) dispersed phases, which have a pinning effect on the grain boundaries.
[0032] Preferably, the barrier layer comprises Mn≤0.01wt% and Cr≤0.01wt% by mass.
[0033] Wherein Mn≤0.01wt%, for example, it can be 0.01wt%, 0.009wt%, 0.008wt%, 0.007wt%, 0.006wt%, 0.005wt%, 0.004wt%, 0.003wt% or 0.002wt%, etc.; Cr≤0.01wt%, for example, it can be 0.01wt%, 0.009wt%, 0.008wt%, 0.007wt%, 0.006wt%, 0.005wt%, 0.004wt%, 0.003wt% or 0.002wt%, etc.
[0034] In the barrier layer materials of the prior art, Mn is usually added to improve the strength of the barrier layer, thereby compensating for the problem of insufficient strength of the composite material to a certain extent. However, in actual research, the effect of this strengthening method is limited. Increasing the concentration of Mn in the barrier layer contributes much less to the strength of the composite material than increasing the concentration of Mg in the core layer. In the barrier layer system of the present invention, it is necessary to control Mn≤0.01wt% and Cr≤0.01wt% in the barrier layer. This is because Mn and / or Cr elements can easily react with Al, Fe, Si, Ti, Sc, V, and Hf to form intermetallic compounds, which reduces the amount of Al3X dispersed phase and / or Al3(X,Y) dispersed phase in the barrier layer, and the ideal grain structure cannot be obtained.
[0035] Preferably, the total content of barrier elements in the barrier layer is at least 0.11wt%, for example, it may be 0.11wt%, 0.12wt%, 0.15wt%, 0.2wt%, 0.28wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.8wt%, 0.9wt%, 1.0wt%, 1.1wt%, 1.2wt%, 2wt% or 2.5wt%, etc., and the preferred total content is 0.2wt% to 1.2wt%.
[0036] Exemplarily, the Ti content in the barrier layer is 0.01 to 1 wt%, for example, it can be 0.01 wt%, 0.12 wt%, 0.23 wt%, 0.34 wt%, 0.45 wt%, 0.56 wt%, 0.67 wt%, 0.78 wt%, 0.89 wt% or 1 wt%, etc. The Sc content in the barrier layer is 0.01 to 0.3 wt%, for example, it can be 0.01 wt%, 0.05 wt%, 0.08 wt%, 0.11 wt%, 0.14 wt%, 0.18 wt%, 0.21 wt%, 0.24 wt%, 0.27 wt% or 0.3 wt%, etc. The V content in the barrier layer is 0.01 to 0.5 wt%, for example, it can be 0.01 wt%, 0.07 wt%, 0.12 wt%, 0.18 wt%, 0.23 wt%, 0.29 wt%, 0.34 wt%, 0.4 wt%, 0.45 wt% or 0.5 wt%, etc. The Hf content in the barrier layer is 0.01 to 1 wt%, for example, it can be 0.01 wt%, 0.12 wt%, 0.23 wt%, 0.34 wt%, 0.45 wt%, 0.56 wt%, 0.67 wt%, 0.78 wt%, 0.89 wt% or 1 wt%, etc.
[0037] In a second aspect, the present invention provides a three-layer aluminum alloy composite plate, which is composed of a first barrier layer, a core layer, and a second barrier layer stacked in sequence, and the first barrier layer and the second barrier layer are the barrier layers for the high-strength aluminum composite plate;
[0038] The thickness ratios X of the first barrier layer and the second barrier layer to the thickness of the three-layer aluminum alloy composite plate each independently satisfy (λ(C Mg ) + 10 μm) / d * 100% < X; and the thickness of the core material > [1 - 2 * (λ’(C Mg ) + 10 μm) / d] * 100%;
[0039] In the formula, C represents the Mg concentration of the core material in the three-layer aluminum alloy composite plate before brazing Mg under which the value ranges of the barrier layer and the core layer are as follows. Among them, λ(C Mg ) is the average value of the diffusion distance of the Mg element in the core material into the barrier layer after brazing in the present invention, with the unit of μm; λ’(C Mg ) is the average value of the diffusion distance of the Mg element in the core material into the barrier layer after brazing when using a barrier layer of 135 kJ / mol, with the unit of μm; d is the total thickness of the three-layer aluminum alloy composite plate, with the unit of μm.
[0040] The best barrier diffusion level Q of the prior art = 135 kJ / mol. At the same C Mg concentration, the thickness of the barrier layer in the prior art is λ’(C Mg)+10μm, it is known that the design value of the barrier layer thickness needs to be higher than the critical value by more than 10um (10μm is a safety value that usually needs to be considered in the actual production process); fitting the diffusion distance λ' of the Mg element after brazing at 603℃ for 10min and the Mg element content C in the core material Mg The relationship between is, λ'=12exp(1.9758*C Mg ), this λ' is the critical value of the barrier layer thickness. When the barrier layer is lower than this thickness, there is a risk of Mg diffusing to the surface. The present invention reduces Q, which can reduce the Mg diffusion distance and achieve a smaller barrier layer thickness ratio.
[0041] More preferably, the thickness ratio of the core material is ≥[1-2*(λ)(C Mg )+10μm) / d]*100%,λ”(C Mg ) is the average diffusion distance of Mg element in the barrier layer after brazing when the diffusion activation energy of Mg element in the barrier layer is 150 kJ / mol, in μm; d is the total thickness of the three-layer aluminum alloy composite plate, in μm.
[0042] The core layer of the present invention is a 6 series aluminum alloy, which is strengthened by aging with Mg and Si. Preferably, the core layer includes Mg: 0.5-1.3% and Si: 0.05-0.9% by mass percentage.
[0043] Among them, Mg: 0.5-1.3%, for example, it can be 0.5%, 0.59%, 0.68%, 0.77%, 0.86%, 0.95%, 1.04%, 1.13%, 1.22% or 1.3%; Si: 0.05-0.9%, for example, it can be 0.05%, 0.15%, 0.24%, 0.34%, 0.43%, 0.53%, 0.62%, 0.72%, 0.81% or 0.9%.
[0044] Preferably, the thickness of the three-layer aluminum alloy composite plate is 0.6-3.0 mm, for example, it can be 0.6 mm, 0.9 mm, 1.2 mm, 1.4 mm, 1.7 mm, 2 mm, 2.2 mm, 2.5 mm, 2.8 mm or 3.0 mm, preferably 1.0-3.0 mm, more preferably 2.0-3.0 mm.
[0045] In a third aspect, the present invention provides a functional composite plate, wherein the functional composite plate comprises the three-layer aluminum alloy composite plate;
[0046] The functional composite plate further comprises a functional layer arranged on a single side or both sides of the three-layer aluminum alloy composite plate, and the functional layer comprises a sacrificial layer and / or a brazing layer.
[0047] The functional layer is a brazing layer, and the alloy composition of the brazing layer includes: Si is 4.5-12.0wt%, Fe≤0.8wt%, Cu≤0.8wt%, Mn≤1.0wt%, Mg≤0.6wt%, and Zn≤0.6wt%; illustratively, the brazing layer can be selected from conventional 4 series aluminum alloys such as AA4043, AA4045, and AA4343.
[0048] The Si content is 4.5wt%, 5wt%, 5.5wt%, 6wt%, 6.5wt%, 7wt%, 7.5wt%, 8wt%, 8.5wt%, 9wt%, 10wt%, 11wt% or 12wt%, etc.
[0049] The functional layer is a sacrificial layer, and the alloy composition of the sacrificial layer includes: Zn is 0.1-5.0wt%, Si≤0.5wt%, Fe≤0.8wt%, Cu≤0.5wt%, Mn≤0.5wt%, Mg≤0.6wt%. Exemplarily, the sacrificial layer can be selected from conventional AA7072 alloy.
[0050] The Zn content is 0.1-5.0wt%, for example, 0.1wt%, 0.2wt%, 0.5wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt% or 5wt%.
[0051] In the functional composite plate, the thickness of the three-layer aluminum alloy composite plate accounts for at least 84% of the total functional composite plate, for example, it can be 84%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 95%, 96% or 97%, etc., and the brazing layer accounts for at least 3% of the total functional composite plate, for example, it can be 3%, 3.2%, 3.5%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15% or 16%, etc.
[0052] The post-weld tensile strength of the functional composite plate is ≥239MPa, for example, it can be 239MPa, 240MPa, 242MPa, 245MPa, 250MPa, 252MPa, 260MPa or 265MPa, etc.; the weld length of the functional composite plate is ≥12mm, for example, it can be 12mm, 13mm, 13.5mm, 14mm, 14.5mm, 15mm, 15.5mm, 16mm, 16.5mm or 17mm, etc.
[0053] In a fourth aspect, the present invention provides a method for preparing the three-layer aluminum alloy composite plate according to the second aspect or the functional composite plate according to the third aspect, the preparation method comprising:
[0054] (1) melting, casting, homogenizing, heat treating and milling raw materials according to the composition ratio of the alloys of the barrier layer and the core layer to obtain barrier layer alloy ingots and core layer alloy ingots respectively;
[0055] (2) preheating the barrier layer alloy ingot in step (1) at 430-448° C., keeping the temperature for 2-4 hours, and hot rolling to obtain a barrier layer alloy plate; preheating and hot rolling the core layer alloy ingot in step (1) to obtain a core layer alloy plate;
[0056] (3) stacking the barrier layer alloy plate and the core layer alloy plate in step (2) in sequence, preheating and hot rolling them in turn to obtain a primary composite plate;
[0057] (4) cold rolling the primary composite plate obtained in step (3) to obtain a secondary composite plate;
[0058] (5) Annealing the secondary composite plate obtained in step (4) to finally obtain a high-strength aluminum composite plate.
[0059] The present invention controls the addition amount of Ti and / or Sc and / or V and / or Hf elements and controls the preheating process to obtain the solid solubility and precipitation amount within the target range. Specifically:
[0060] On the one hand, when the barrier layer contains Ti and / or Sc and / or V and / or Hf elements, and the precipitation amount of Ti and / or Sc and / or V and / or Hf elements is controlled through the preheating process and the annealing process to control the total solid solubility (solid solubility+precipitation amount=element content) to at least 0.06wt%, a higher diffusion activation energy can be obtained. It is speculated that the Ti and / or Sc and / or V and / or Hf elements are easily combined with the vacancies in the aluminum matrix, and their precipitation during the preheating process is controlled, so that more Ti and / or Sc and / or V and / or Hf elements are kept in a solid solution state, and more vacancies can be captured during the brazing process to form solute-vacancy coordination pairs, reduce the vacancy concentration, reduce the diffusion channel, and increase the diffusion activation energy of the Mg element.
[0061] On the other hand, a part of Ti and / or Sc and / or V and / or Hf elements are dissolved in the aluminum alloy, and the rest are precipitated in the form of Al3X or Al3(X,Y) dispersed phase. When the total amount of precipitation is controlled to be at least 0.05wt% by the preheating process and annealing process, an ideal annealed state structure can be obtained.
[0062] The precipitation amount in the preheating process is at least 0.03wt%, and the precipitation amount in the annealing process is controlled to be at least 0.02wt%. Al3X or Al3(X,Y) dispersed phase has a pinning effect on the grain boundary. The dispersed phase formed in the preheating process has a greater effect on the grain boundary length ratio, and the dispersed phase formed in the annealing process has a greater effect on the number of grain layers. Aluminum alloy material forms dispersed phase in the preheating process. After the subsequent rolling process, the dispersed phase is randomly and evenly distributed, which plays a pinning role on the grain boundary of the recrystallized grains in the annealing process, making the grain size uniform. The precipitation amount in the preheating process is at least 0.03wt%, so that the grain boundary length per unit area accounts for less than 35%; the dispersed phase formed in the annealing process is mostly distributed along the line consistent with the rolling direction. This is because the cast grains are in the form of slender fibers after rolling. The grain boundaries consistent with the rolling direction are easy to become the nucleation points of the dispersed phase during the annealing process, so that the dispersed phase is distributed in a line along the rolling direction (observed on the longitudinal section), so that the migration of the recrystallized grains in the thickness direction is restricted, and the precipitation amount in the annealed state is controlled to be at least 0.02wt%, so that the recrystallized grain morphology is at least 2 layers of grains. When there are at least 2 layers of grains, it is not conducive to the diffusion of elements, and the overall diffusion activation energy Q can be improved. When the grain boundary length accounts for a large proportion, the grain boundary in the barrier layer is suppressed as a fast diffusion channel with low diffusion activation energy, which can improve the overall diffusion activation energy Q.
[0063] The specific selection of preheating temperature, preheating holding time, annealing temperature and annealing holding time in the present invention should be adjusted according to the target values of the solid solution and precipitation of Ti, Sc, V and Hf, and the solid solution and precipitation of Ti, Sc, V and Hf are controlled to be at least 0.06% and the precipitation is at least 0.05%, wherein the precipitation in the preheating process is at least 0.03%, and the precipitation in the annealing process is controlled to be at least 0.02%.
[0064] Furthermore, the preheating process and annealing process jointly affect the solid solution and precipitation of Ti, Sc, V, and Hf. In principle, the preheating process should ensure the largest possible solid solubility to reduce the vacancy density during the brazing process; at the same time, the appropriate amount of precipitation should be controlled to form Al3X or Al3 (X, Y) dispersed phases, which act on the grain boundary length per unit area in the annealed state. The annealing process has the precipitation and recrystallization behavior of these elements. Ensuring the appropriate amount of precipitation to obtain the appropriate number of grain layers, while controlling the precipitation amount and ensuring a high solid solubility, can improve the diffusion activation energy in many aspects.
[0065] During the preheating process, the precipitation of Ti, Sc, V, and Hf is controlled to ensure the solid solubility of these alloy elements in the aluminum alloy matrix. In the cast structure, the sensitive temperature for the precipitation of Ti, Sc, V, and Hf to form Al3X or Al3 (X, Y) dispersed phase is 450-480°C. When the preheating temperature is higher than 450°C, the precipitation power is sufficient. Excessive precipitation of Ti, Sc, V, and Hf leads to a decrease in solid solubility, a decrease in the number of vacancies captured during brazing heat treatment, and an increase in the vacancy concentration in the aluminum matrix, which reduces the diffusion activation energy. If the preheating temperature is too low, the material is too hard to be rolled.
[0066] If the holding time is less than 2h, the ingot cannot be completely stress relieved, and the core of the ingot is not heated to the target temperature, so it cannot be rolled. If the holding time is more than 4h, the incubation period of the Ti, Sc, V, and Hf dispersed phases is exceeded, and these elements precipitate in large quantities, increasing the vacancy concentration of the aluminum matrix and causing a decrease in the diffusion activation energy of the Mg element during brazing.
[0067] The barrier layer alloy ingot of step (1) is preheated at 430-448°C and kept warm for 2-4 hours and hot rolled to obtain a barrier layer alloy plate. The preheating temperature can be, for example, 430°C, 432°C, 434°C, 436°C, 438°C, 440°C, 442°C, 444°C, 446°C or 448°C; the holding time can be, for example, 2h, 2.3h, 2.5h, 2.7h, 2.9h, 3.2h, 3.4h, 3.6h, 3.8h or 4h.
[0068] Preferably, the cold deformation rate of the cold rolling in step (4) is 60-80%, for example, it can be 60%, 62.3%, 64.5%, 66.7%, 68.9%, 71.2%, 73.4%, 75.6%, 77.8% or 80%, etc.
[0069] Preferably, the annealing temperature in step (5) is 300-350°C, and the annealing holding time is 1-3h. The annealing temperature can be, for example, 300°C, 306°C, 312°C, 317°C, 323°C, 328°C, 334°C, 339°C, 345°C or 350°C, etc.; the annealing holding time is 1-3h, for example, 1h, 1.3h, 1.5h, 1.7h, 1.9h, 2.2h, 2.4h, 2.6h, 2.8h or 3h, etc.
[0070] During the annealing process, the precipitation of Ti, Sc, V, and Hf is controlled, and the microstructure is controlled. When the annealing temperature is higher than 350°C, the recrystallization process takes precedence over the precipitation of the dispersed phase, and the recrystallized grain boundaries migrate smoothly in the thickness direction, resulting in the formation of single-layer grains; when the annealing temperature is too low, the structure of the material cannot be completely recrystallized, resulting in the grain boundary length per unit area not being able to meet ≤35%.
[0071] The target thickness of hot rolling in step (3) of the present invention is based on the desired cold deformation rate and thickness of the cold-rolled product. For example, 4 to 7 mm can be selected, for example, 4 mm, 4.2 mm, 4.5 mm, 4.6 mm, 4.8 mm, 4.9 mm, 5.0 mm, 5.2 mm, 5.5 mm, 5.8 mm, 6.0 mm, 6.2 mm, 6.5 mm, 6.8 mm or 7.0 mm, etc.
[0072] The high-strength aluminum composite plate provided by the present invention can be used for brazing processes under the conditions of a temperature of 590-620°C and a time of 2-15 minutes. After simulated brazing and subsequent aging heat treatment, the composite aluminum plate precipitates a β" strengthening phase in the structure, which significantly improves the material strength. Excessive Mg elements cause the alloy melting point to be lower than 600°C, which is not suitable for traditional brazing processes.
[0073] The high-strength aluminum composite plate of the present invention is used for a liquid cooling plate.
[0074] Compared with the prior art, the present invention has at least the following beneficial effects:
[0075] (1) The barrier layer for high-strength aluminum composite plate provided by the present invention can effectively block the diffusion of Mg through composition regulation and process coordination, while avoiding the increase in the quenching sensitivity of the core material due to the diffusion of the Mn element in the traditional Al-Mn barrier layer, thereby effectively improving the strength of the water-cooled plate;
[0076] (2) The diffusion activation energy Q of the Mg element in the barrier layer provided by the present invention is higher than 150 kJ / mol; under the simulated brazing condition of 600°C insulation for 10 min, the yield strength of the composite plate after artificial aging is improved;
[0077] (3) The preparation method of the high-strength aluminum composite plate provided by the present invention is simple to operate, has low raw material and process costs, a wide range of applications, and broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0078] Figure 1 It is a schematic diagram of the structure of the high-strength aluminum composite plate provided in Example 1 of the present invention.
[0079] Figure 2 It is a schematic diagram of the structural organization of the high-strength aluminum composite plate after annealing in Example 1 of the present invention.
[0080] Figure 3 This is the EPMA line scan result of the Mg element of the high-strength aluminum composite plate in Example 1 of the present invention after brazing at 600° C. for 10 minutes.
[0081] Figure 4 It is a schematic diagram of the structure of the high-strength aluminum composite plate provided in Application Example 1 of the present invention.
[0082] Figure 5It is a schematic diagram of the structure of the high-strength aluminum composite plate provided in Application Example 2 of the present invention.
[0083] Among them, 1 is the core layer, 2 is the first barrier layer, 3 is the second barrier layer, and 4 is the brazing layer. DETAILED DESCRIPTION
[0084] For the convenience of understanding the present invention, the present invention lists the following embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0085] The components of different barrier layers in the present invention are shown in Table 1, with the unit being %.
[0086] Table 1
[0087] Barrier layer components Ti Sc V Hf Mn Cr Z1 0 0 0 0.3 0 0 Z2 1 0.01 0 0.01 0.001 0 Z3 0 0 0.5 1 0 0 Z4 0.01 0.04 0.01 0.05 0.01 0.01 Z5 0 0 0.3 0 0 0 Z6 0 0.3 0 0 0 0 Z7 0.3 0 0 0 0 0 DZ1 Same as 1 Same as 1 Same as 1 0 Same as 1 Same as 1 DZ2 Same as 1 Same as 1 Same as 1 0.005 Same as 1 Same as 1 DZ3 Same as 1 Same as 1 Same as 1 Same as 1 0.1 Same as 1 DZ4 Same as 1 Same as 1 Same as 1 Same as 1 Same as 1 0.1
[0088] The core layer in the present invention is a 6 series aluminum alloy, and the components of different core layers are shown in Table 2, in %.
[0089] Table 2
[0090]
[0091]
[0092] Examples 1 to 10 and Comparative Examples 1 to 9 provide three-layer aluminum alloy composite plates, and the preparation method includes:
[0093] (1) melting, casting, homogenizing, heat treating and milling raw materials according to the composition ratio of the alloys of the barrier layer and the core layer to obtain barrier layer alloy ingots and core layer alloy ingots respectively;
[0094] (2) preheating the barrier layer alloy ingot in step (1) at 430-448° C., keeping the temperature for 2-4 hours, and hot rolling to obtain a barrier layer alloy plate; preheating and hot rolling the core layer alloy ingot in step (1) to obtain a core layer alloy plate;
[0095] (3) stacking the barrier layer alloy plate and the core layer alloy plate in step (2) in sequence, preheating and hot rolling them in turn to obtain a primary composite plate;
[0096] (4) cold rolling the primary composite plate obtained in step (3) with a cold deformation rate of 60 to 80% to obtain a secondary composite plate;
[0097] (5) Annealing the secondary composite plate obtained in step (4) at a temperature of 300° C. to 350° C. for a holding time of 1 to 3 hours, thereby finally obtaining a high-strength aluminum composite plate.
[0098] The specific composite structures and process parameters in Examples 1 to 10 are shown in Table 3.
[0099] Table 3
[0100]
[0101]
[0102] In the experiment, λ'(C Mg ) / μm is measured using the barrier layer of Comparative Example 2. “Same as 1” means the same as Example 1.
[0103] The structural schematic diagram of the high-strength aluminum composite plate provided in Example 1 is as follows Figure 1 As shown, the high-strength aluminum composite plate includes a core layer 1, and a first barrier layer 2 and a second barrier layer 3 arranged on both sides of the surface of the core layer 1. In addition, the structural organization diagram of the high-strength aluminum composite plate after annealing in Example 1 is shown in Figure 2 ,from Figure 2 It can be seen that the barrier layer after annealing has recrystallized grains and dispersed phases. The EPMA line scan results of the Mg element after the three-layer composite aluminum alloy plate in Example 1 was brazed at 600°C for 10 minutes can be found in Figure 3 ,from Figure 3 It can be seen that the diffusion distance of Mg element in the barrier layer is very short.
[0104] The specific composite structures and process parameters in Comparative Examples 1 to 8 are shown in Table 4.
[0105] Table 4
[0106]
[0107]
[0108] The product structures and properties of the three-layer composite boards in Examples 1 to 10 and Comparative Examples 1 to 8 were tested, and the test results are shown in Table 5.
[0109] Table 5
[0110]
[0111] “ / ” in the above tables indicates that relevant data is not required or available.
[0112] From Tables 3 to 5, we can see the following points:
[0113] (1) It can be seen from Examples 1 to 10 that the three-layer aluminum alloy composite plate provided by the present invention can optimize the diffusion activation energy of the Mg element in the barrier layer by adding any one or a combination of at least two of Ti, Sc, V or Hf in the barrier layer, and ultimately prevent the Mg element from diffusing to the surface when the core layer composite ratio is higher, thereby improving the strength of the three-layer aluminum alloy composite plate;
[0114] (2) Influence of blocking elements
[0115] By comparing Example 1 with Comparative Examples 1 to 2, it can be seen that the barrier layer of Example 1 contains 0.3% barrier element Hf, while Comparative Example 1 does not contain any barrier element, and Comparative Example 2 contains only 0.005% barrier element Hf. When Comparative Example 1 and Example 1 use the same composite ratio and thickness, the Mg element in Comparative Example 1 eventually diffuses to the surface, which is difficult to meet the requirements of the composite plate. In Comparative Example 2, when the lowest composite ratio of the barrier layer is used, the tensile strength of the composite plate is only 265 MPa, which shows that the present invention can improve the strength of the composite plate by adding barrier elements and controlling the total solid solubility of the barrier elements in the barrier layer to be at least 0.06wt%.
[0116] By comparing Example 1 with Examples 8 to 10, it can be seen that the barrier element used in Example 1 is Hf. Compared with the same amount of V, Sc and Ti used in Examples 8 to 10, the λ(CMg) in the barrier layer of Example 1 is the smallest, which is only 59 μm. Therefore, when both Examples 1 and Examples 8 to 10 use the lowest line of the barrier layer composite ratio, the barrier layer in Example 1 has the lowest composite ratio, which is only 4.60%, while the lowest lines of the barrier layer composite ratios in Examples 8 to 10 are 5.13%, 5.67% and 5.33%, respectively. Ultimately, under the same total thickness of the composite plate, the tensile strength of Example 1 is as high as 285 MPa, while the tensile strengths in Examples 8 to 10 are only 275 MPa, 270 MPa and 273 MPa, respectively. This shows that the present invention further prefers that the barrier element contains Hf, which has a better effect of improving the diffusion activation energy of the Mg element in the barrier layer, and ultimately can better improve the tensile strength of the composite plate under the same thickness.
[0117] (3) Effects of Mn and Cr
[0118] By comparing Example 1 with Comparative Examples 3-4, it can be seen that the Mn and / or Cr elements are excessive in Comparative Examples 3-4, and Mn and / or Cr elements can easily form intermetallic compounds with Al, Fe, Si, Ti, Sc, V, and Hf, thereby reducing the amount of Al3X dispersed phase and / or Al3(X,Y) dispersed phase in the barrier layer, and the ideal recrystallized grain structure cannot be obtained.
[0119] (4) Influence of Mg content in the core layer
[0120] By comparing Example 1 and Comparative Example 5, it can be seen that when the Mg content of the core layer is as low as less than 0.5%, the strength of the composite board significantly decreases to 265 MPa, which indicates that a certain amount of Mg needs to be added to the core layer to improve the strength of the composite board.
[0121] (5) Influence of preheating temperature
[0122] It can be seen from Example 1 and Comparative Example 6 that the preheating temperature in Comparative Example 6 is too high, which leads to a decrease in the total solid solubility of the barrier element, and the diffusion activation energy of the Mg element in the barrier layer decreases to 133 kJ / mol. Finally, the Mg element in the composite plate diffuses to the surface, indicating that controlling the preheating temperature within a reasonable range in the present invention can increase the total solid solubility of the barrier element and the diffusion activation energy of the Mg element in the barrier layer, thereby avoiding the diffusion of Mg element in the composite plate to the surface.
[0123] (6) Effect of annealing temperature
[0124] It can be seen from Example 1 and Comparative Examples 7 to 8 that the annealing temperature in Comparative Examples 7 to 8 is too high or too low, resulting in the inability to form an ideal recrystallized grain structure, especially in Example 7, the grain boundary length per unit area accounts for as high as 83.1%. Finally, the Mg element in the composite plates of Comparative Examples 7 to 8 diffuses to the surface, which means that the present invention can better regulate the recrystallized grain structure and the grain boundary length ratio in the barrier layer by controlling the annealing temperature within a reasonable range, thereby increasing the diffusion activation energy of the Mg element in the barrier layer and reducing the diffusion distance of the Mg element.
[0125] Application Example 1
[0126] This application example provides a functional composite board. The structural schematic diagram of the functional composite board is shown in Figure 4 Specifically, the functional composite plate includes the three-layer aluminum alloy composite plate in Example 1, and the functional composite plate also includes a brazing layer 4 arranged on one side of the three-layer aluminum alloy composite plate, and the components of the brazing layer 4 include Si: 4.5%; Fe: 0.6%; Cu: 0.8%; Mn: 1%; Mg: 0.6%; Zn: 0.5% in terms of mass fraction; wherein the composite ratio of the brazing layer 4 is 7.5%, and the composite ratio of the three-layer aluminum alloy composite plate in Example 1 is 92.5%. The preparation method thereof is the same as the preparation process of Example 1 except that the brazing layer is laminated on one side of the three-layer composite plate in step (3).
[0127] The tensile strength of the functional composite plate provided in this application example is 265 MPa, and the weld length is 12.6 mm.
[0128] Application Example 2
[0129] This application example provides a functional composite board. The structural schematic diagram of the functional composite board is shown in Figure 5 Specifically, the functional composite plate includes the three-layer aluminum alloy composite plate in Example 1, and the functional composite plate also includes a brazing layer 4 arranged on both sides of the three-layer aluminum alloy composite plate, and the components of the brazing layer 4 include Si: 12%; Fe: 0.8%; Cu: 0.7%; Mn: 0.9%; Mg: 0.4%; Zn: 0.6% in terms of mass fraction; wherein the composite ratios of the brazing layers 4 on both sides are 7.5% respectively, and the composite ratio of the three-layer aluminum alloy composite plate in Example 1 is 85%. The preparation method thereof is the same as the preparation process of Example 1 except that the brazing layers on both sides are stacked on the outside of the three-layer composite plate in step (3).
[0130] The tensile strength of the functional composite plate provided in this application example is 239 MPa, and the weld length is 25.6 mm.
[0131] Test methods include:
[0132] 1. Simulate brazing
[0133] The simulated brazing conditions were set to heat up to 600° C. within 25 minutes, keep the temperature for 10 minutes, and then take out and cool.
[0134] 2. Aging heat treatment
[0135] The conditions of the aging heat treatment are set as follows: heating to 230° C. within 15 minutes, keeping the temperature for 30 minutes, and then taking out to cool.
[0136] 3. Mg diffusion distance: Use a microscope to mark the thickness of each layer of the sample, use the HITACHI electron probe equipment to perform quantitative line scanning analysis of the Mg element on the longitudinal section of the sample to determine the change in Mg element content in the longitudinal section of the plate. Based on the marked thickness information of each layer of the sample, determine the starting position of the corresponding barrier layer in the figure, thereby determining the diffusion depth of Mg in the barrier layer.
[0137] 4. Diffusion activation energy Q: The three-layer aluminum alloy composite plate was kept at 525℃, 550℃, 575℃, 600℃ and 625℃ for 10 minutes, then taken out and air-cooled. The HITACHI electron probe equipment was used to perform quantitative line scanning analysis of the Mg element on the longitudinal section of the sample. The Mg element content changes, thereby determining the diffusion depth of Mg in the barrier layer. By analyzing formula (1) and formula (2), Q can be obtained. The Q value is related to the diffusion mechanism of the material, the material and structure of the barrier layer itself, and has nothing to do with parameters such as temperature, time, core material composition, thickness, etc.
[0138] 5. Solid solution content of barrier elements: Take 2 samples with a thickness of 20 mm × 20 mm, mount the longitudinal sections and perform mechanical grinding and polishing, followed by vibration polishing, and use a ZEISSsigma300 electron microscope for EDS analysis. Perform micro-area point scanning on 10 random aluminum matrix areas in each sample at 1000x magnification to obtain the element content. The average value of 20 results in each group is the solid solution content of the corresponding element.
[0139] 6. Morphology of recrystallized grains and proportion of grain boundary length per unit area: Take 2 annealed samples with a thickness of 20 mm × 20 mm, mount the longitudinal sections and grind and polish them mechanically, then perform vibration polishing, and use a ZEISSsigma300 electron microscope equipped with an Oxford electron backscatter diffraction (EBSD) camera for EBSD analysis. At 100x magnification, randomly measure 2 areas of each sample (the area of each area is approximately sample thickness × 1.1 mm), import the collected images into AZCrystal software, and the system automatically performs area and grain boundary length analysis and statistics to calculate the proportion of grain boundary length per unit area in μm / μm 2 On the barrier layer structure in the random field of view, draw a vertical line at random. This line passes through two or more grains, which is defined as the morphology of the recrystallized grains with at least two layers of grains.
[0140] 7. Tensile strength: The room temperature mechanical properties test is carried out according to the method disclosed in GB / T228.1-2010 "Tensile test of metal materials". The testing instrument is ZWICK universal material testing machine, and the test index is tensile strength Rm.
[0141] 8. Weld length: The brazing effect is determined by a T-type test. The specific test method is based on the operating steps specified in paragraph
[0064] of the CN114473385A specification. A T-type brazing test is performed on a functional composite plate whose functional layer is a brazing layer, and the weld length of the T-type sample after brazing is statistically analyzed.
[0142] The present invention illustrates the detailed features of the present invention through the above embodiments, but the present invention is not limited to the above detailed features, that is, it does not mean that the present invention must rely on the above detailed features to be implemented. Those skilled in the art should understand that any improvement to the present invention, equivalent replacement of the technical features selected by the present invention, addition of auxiliary technical features, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A barrier layer for a high-strength aluminum composite plate, characterized in that: The barrier layer includes any one or a combination of at least two of the alloy elements Ti, Sc, V or Hf, and the alloy elements Ti, Sc, V or Hf are recorded as barrier elements; The total solid solubility of the barrier elements in the barrier layer is at least 0.06 wt %.
2. The barrier layer according to claim 1, characterized in that The barrier layer includes recrystallized grains; the recrystallized grains are in the form of at least two layers of grains, and the grain boundary length per unit area accounts for less than 35%; Preferably, the diffusion activation energy of the Mg element in the barrier layer is greater than 150 kJ / mol.
3. The barrier layer according to claim 2, characterized in that The barrier element is present in the aluminum alloy in the form of dispersed phase precipitation in an amount of at least 0.05 wt %; Preferably, the dispersed phase in the barrier layer is an Al3X dispersed phase and / or an Al3(X,Y) dispersed phase.
4. The barrier layer according to claim 2 or 3, characterized in that The barrier layer comprises Mn≤0.01wt% and Cr≤0.01wt% by mass percentage; Preferably, the total content of barrier elements in the barrier layer is at least 0.11 wt %, preferably 0.2 to 1.2 wt %.
5. A three-layer aluminum alloy composite plate, consisting of a first barrier layer, a core layer and a second barrier layer stacked in sequence, characterized in that: The first barrier layer and the second barrier layer are barrier layers for high-strength aluminum composite panels as described in any one of claims 1 to 4; The thickness of the first barrier layer and the second barrier layer and the thickness ratio X of the three-layer aluminum alloy composite plate independently satisfy (λ(C Mg ) + 10 μm) / d * 100% < X; and the thickness of the core material > [1 - 2 * (λ’(C Mg ) + 10 μm) / d] * 100% In the formula, C represents the Mg concentration of the core material of the three-layer aluminum alloy composite plate before brazing. Mg The barrier layer and the core layer have a value range of, where λ(C Mg ) is the average diffusion distance of the Mg element in the core material in the barrier layer after brazing in the present invention, in μm; λ'(C Mg ) is the average diffusion distance of the core material Mg element in the barrier layer after brazing when the diffusion activation energy of the Mg element in the barrier layer is 135 kJ / mol, in μm; d is the total thickness of the three-layer aluminum alloy composite plate, in μm; More preferably, the thickness ratio of the core material is ≥[1-2*(λ)(C Mg )+10μm) / d]*100%,λ”(C Mg ) is the average diffusion distance of Mg element in the barrier layer after brazing when the diffusion activation energy of Mg element in the barrier layer is 150 kJ / mol, in μm; d is the total thickness of the three-layer aluminum alloy composite plate, in μm.
6. The three-layer aluminum alloy composite plate according to claim 5, characterized in that: The core layer comprises Mg: 0.5-1.3% and Si: 0.05-0.9% by mass percentage.
7. A functional composite board, characterized in that: The functional composite plate comprises the three-layer aluminum alloy composite plate according to claim 5 or 6; The functional composite plate further comprises a functional layer arranged on one side or both sides of the three-layer aluminum alloy composite plate, and the functional layer comprises a sacrificial layer and / or a brazing material layer.
8. The functional composite panel according to claim 7, characterized in that: The functional layer is a brazing layer, and the alloy composition of the brazing layer includes: Si is 4.5-12.0wt%, Fe≤0.8wt%, Cu≤0.8wt%, Mn≤1.0wt%, Mg≤0.6wt%, and Zn≤0.6wt%; In the functional composite plate, the thickness of the three-layer aluminum alloy composite plate accounts for at least 84% of the total thickness of the functional composite plate, and the brazing layer accounts for at least 3% of the total thickness of the functional composite plate.
9. A method for preparing the three-layer aluminum alloy composite plate according to claim 5 or 6 or the functional composite plate according to claim 7 or 8, characterized in that: The preparation method comprises: (1) melting, casting, homogenizing, heat treating and milling raw materials according to the composition ratio of the alloys of the barrier layer and the core layer to obtain barrier layer alloy ingots and core layer alloy ingots respectively; (2) preheating the barrier layer alloy ingot in step (1) at 430-448° C., keeping the temperature for 2-4 hours, and hot rolling to obtain a barrier layer alloy plate; preheating and hot rolling the core layer alloy ingot in step (1) to obtain a core layer alloy plate; (3) stacking the barrier layer alloy plate and the core layer alloy plate in step (2) in sequence, preheating and hot rolling them in turn to obtain a primary composite plate; (4) cold rolling the primary composite plate obtained in step (3) to obtain a secondary composite plate; (5) Annealing the secondary composite plate obtained in step (4) to finally obtain a high-strength aluminum composite plate.
10. The preparation method according to claim 9, characterized in that: The cold rolling cold deformation rate in step (4) is 60-80%; Preferably, the annealing temperature in step (5) is 300° C. to 350° C., and the annealing holding time is 1 to 3 hours.
Citation Information
Patent Citations
High-strength aluminum alloy composite board capable of being brazed as well as preparation method and application thereof
CN113897523A
Pre-embedded brazing flux composite board as well as preparation method and application thereof
CN114473385A
Composite aluminum alloy plate for liquid cooling plate of new energy power battery and its preparation method
CN114752829B
High-strength aluminum alloy composite plate for brazing battery liquid cooling plate and preparation method of high-strength aluminum alloy composite plate
CN114670509A
Aluminium multi-layered brazing sheet product and fluxless brazing method
US20190077119A1