Composite material for forming paper-plastic composite bag and preparation method of composite material

The method of preparing modified polypropylene carbonate as a sizing agent for paper-plastic composite materials addresses the bonding and mechanical strength issues, enhancing the composite's integrity and thermal stability.

CN119078334AActive Publication Date: 2024-12-06瑞安市现代包装有限公司
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411179866.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-06
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

Existing paper-plastic composite materials face challenges in achieving high bonding tightness and mechanical strength between paper-based and polymer materials.

Method used

A method involving the preparation of modified polypropylene carbonate, using it as a sizing agent for a paper base layer, and combining it with polybutylene adipate terephthalate to form a polymer layer, followed by hot-pressing to create a composite material.

Benefits of technology

Enhances the bonding between paper and polymer layers, improving mechanical strength and thermal stability, while maintaining environmental friendliness.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a composite material for forming a paper-plastic composite bag and a preparation method of the composite material. The preparation method comprises the following steps: S100, preparing modified polypropylene carbonate; s200, waterborne polyurethane containing the modified polypropylene carbonate is used as a sizing agent, and a paper base layer is prepared; s300, preparing a polymer layer by adopting raw materials including modified polypropylene carbonate and polybutylene terephthalate adipate; and S400, performing hot-pressing compounding on the paper base layer and the polymer layer to obtain the composite material. In the composite material, the paper base layer and the polymer layer can be tightly combined, the mechanical strength is higher, and the composite material is easy to degrade and more environmentally friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of packaging materials, and in particular to a composite material for forming a paper-plastic composite bag and a preparation method thereof. Background Art

[0002] Paper-plastic composite materials are widely used in the packaging of food, cosmetics and medicines due to their good moisture-proof, oil-proof and drop-resistant properties. For example, paper-plastic-aluminum composite packaging materials are widely used in the packaging of liquid dairy products, plant protein beverages and other products. In the production of printed materials such as posters, leaflets, and labels, paper-plastic composite materials are favored because of their smooth surface and high gloss. In addition, paper-plastic composite notebook covers, folders, file boxes, etc. are not only beautiful, but also durable. In summary, paper-plastic composite materials are gradually being used in many fields with their unique performance and cost advantages, and are welcomed by the market.

[0003] In the prior art, coating dry, wet, hot melt and other laminating methods can achieve the lamination of plastic and paper. However, paper-plastic composite materials still have the following shortcomings: How to improve the lamination tightness between paper-based materials and polymer materials has always been a technical problem that technicians in this field have been committed to solving. Summary of the invention

[0004] One of the problems solved by the present invention is how to provide a composite material for forming a paper-plastic composite bag with a high degree of bonding between a paper-based material and a polymer material and a higher mechanical strength.

[0005] In order to solve at least one of the above problems, the present invention provides a method for preparing a composite material for forming a paper-plastic composite bag, the preparation method comprising:

[0006] S100, preparing modified polypropylene carbonate;

[0007] S200, using water-based polyurethane containing modified polypropylene carbonate as a sizing agent to prepare a paper base layer;

[0008] S300, preparing a polymer layer using raw materials including modified polypropylene carbonate and polybutylene adipate terephthalate;

[0009] S400, hot-pressing the paper base layer and the polymer layer to obtain a composite material.

[0010] In the above technical solution, S100 specifically includes:

[0011] S110, uniformly mixing an antioxidant, a first chain extender, maleic anhydride, methacrylic acid monomer and polypropylene carbonate to obtain a first mixture;

[0012] S120, kneading the first mixture at a temperature of 170° C. to 175° C. for 2 h to 2.5 h, and then extruding and granulating the mixture to obtain modified polypropylene carbonate.

[0013] In any of the above technical solutions, in S110, the mass ratio of antioxidant: first chain extender: maleic anhydride: methacrylic acid monomer: polypropylene carbonate = (1-2): (2-4): (3-5): (15-20): 100.

[0014] In any of the above technical solutions, the antioxidant includes at least one of the following or a combination thereof: antioxidant 1010, antioxidant 1076, antioxidant 1098; and / or the first chain extender includes at least one of the following or a combination thereof: BASF ADR-4370, BASF ADR-4368, BASF ADR-4380.

[0015] In any of the above technical solutions, S200 specifically includes:

[0016] S210, mixing dibutyltin dilaurate, polyester diol, and isophorone diisocyanate, reacting at a temperature of 80° C. to 85° C. for 3 to 4 hours, and then cooling to obtain a second mixture;

[0017] S220, mixing Tween 60, ethylenediamine, the second mixture, modified polypropylene carbonate, ethyl acetate and water and performing ultrasonic emulsification to obtain a sizing agent;

[0018] S230, 8g / m 2 Up to 12g / m 2 The sizing agent is applied to the base paper to obtain a paper base layer.

[0019] In any of the above technical solutions, in S210, the mass ratio of dibutyltin dilaurate: polyester diol: isophorone diisocyanate = (0.2-0.4): (80-120): 100; and / or in S220, the mass ratio of Tween 60: ethylenediamine: second mixture: modified polypropylene carbonate: ethyl acetate: water = (4-6): (4-6): (15-20): (10-15): (40-50): 100.

[0020] In any of the above technical solutions, S300 specifically includes:

[0021] S310, uniformly mixing the compatibilizer, the second chain extender, the modified polypropylene carbonate and the polybutylene terephthalate adipate to obtain a third mixture;

[0022] S320, melt-extrude the third mixture at a temperature of 150° C. to 170° C. to obtain a polymer layer.

[0023] In any of the above technical solutions, in S310, the mass ratio of compatibilizer: second chain extender: modified polypropylene carbonate: polybutylene terephthalate adipate is (1-2): (1-2): (50-60): 100.

[0024] In any of the above technical solutions, the compatibilizer includes at least one of the following or a combination thereof: succinic anhydride, maleic anhydride, ethylene-methyl acrylate-glycidyl methacrylate; and / or the second chain extender includes at least one of the following or a combination thereof: BASF ADR-4370, BASF ADR-4368, BASF ADR-4380.

[0025] The present invention also provides a composite material for forming a paper-plastic composite bag. The composite material is obtained by using the preparation method of any of the above technical solutions.

[0026] Beneficial Effects

[0027] The invention provides a preparation method of a composite material for forming a paper-plastic composite bag. The preparation method first prepares modified polypropylene carbonate, then uses an aqueous polyurethane containing the modified polypropylene carbonate as a sizing agent to prepare a paper base layer, then uses a raw material including modified polypropylene carbonate and polybutylene adipate to prepare a polymer layer, and finally hot presses the paper base layer and the polymer layer to obtain a composite material. One of the improvements made by the present invention to the prior art is: using polypropylene carbonate as a raw material to prepare a paper-plastic composite material. Polypropylene carbonate is a material prepared by copolymerization of carbon dioxide and propylene oxide, which has good biodegradability and is more environmentally friendly. The paper used in the paper-plastic composite material needs to be sizing treated to improve its water resistance. The sizing agent is generally rosin glue or polyurethane. The surface properties of such materials are greatly different from polypropylene carbonate, making it difficult to effectively composite. Even after heating and pressurizing composite treatment, it is easy to separate and peel off. To this end, considering the problem of the composite tightness between the polypropylene carbonate polymer material and the paper base material, the present invention improves the sizing agent used in the paper base material. The invention uses waterborne polyurethane as a sizing agent and uses polypropylene carbonate to modify the waterborne polyurethane sizing agent, so as to improve the composite tightness between the polypropylene carbonate polymer material and the paper-based material, thereby making the mechanical strength of the product higher. DETAILED DESCRIPTION

[0028] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the following is a detailed description of the specific embodiments of the present invention.

[0029] Unless otherwise specified, the reagents and raw materials used in the present invention can be purchased through commercial channels. The experimental methods in the following examples without specifying specific conditions are selected according to conventional methods and conditions, or according to the product specifications.

[0030] An embodiment of the present invention provides a method for preparing a composite material for forming a paper-plastic composite bag, the method comprising:

[0031] S100, preparing modified polypropylene carbonate;

[0032] S200, using water-based polyurethane containing modified polypropylene carbonate as a sizing agent to prepare a paper base layer;

[0033] S300, preparing a polymer layer using raw materials including modified polypropylene carbonate and polybutylene adipate terephthalate;

[0034] S400, hot-pressing the paper base layer and the polymer layer to obtain a composite material.

[0035] Polypropylene carbonate (PPC), also known as polymethylethylene carbonate, is a new type of aliphatic polyester. It uses carbon dioxide, propylene oxide and (or) 1,4-butanediol (BDO) as raw materials and is a completely degradable and environmentally friendly plastic. The molecular structure of polypropylene carbonate contains a large number of ester bonds and carbonate bonds, which gives it relatively stable chemical properties and good biocompatibility. Its molecular structure can be linear, branched or cyclic, and the molecular weight is usually between several thousand and several hundred thousand. The finished plastics made of polypropylene carbonate are transparent and non-toxic, suitable for use in food packaging and medical materials, and have excellent barrier properties, especially in oxygen barrier performance.

[0036] In order to obtain a composite material for forming a paper-plastic composite bag, the present invention first modifies polypropylene carbonate. The polypropylene carbonate of the present invention is obtained through commercial procurement, and the modification method is to graft-modify the polypropylene carbonate with methacrylic acid monomer.

[0037] In order to achieve the modification of polypropylene carbonate, S100 specifically includes:

[0038] S110, uniformly mixing an antioxidant, a first chain extender, maleic anhydride, methacrylic acid monomer and polypropylene carbonate to obtain a first mixture;

[0039] S120, kneading the first mixture at a temperature of 170° C. to 175° C. for 2 h to 2.5 h, and then extruding and granulating the mixture to obtain modified polypropylene carbonate.

[0040] Specifically, in S110, the mass ratio of antioxidant: first chain extender: maleic anhydride: methacrylic acid monomer: polypropylene carbonate is (1-2): (2-4): (3-5): (15-20): 100.

[0041] Preferably, in S110, the weight ratio of antioxidant: first chain extender: maleic anhydride: methacrylic acid monomer: polypropylene carbonate is 1:3:5:15:100.

[0042] In some embodiments of the present invention, the antioxidant includes at least one of the following or a combination thereof: antioxidant 1010 , antioxidant 1076 , and antioxidant 1098 .

[0043] In some embodiments of the present invention, the first chain extender includes at least one of the following or a combination thereof: BASF ADR-4370, BASF ADR-4368, BASF ADR-4380.

[0044] The reason for adopting the above steps is that although polypropylene carbonate has excellent biocompatibility, its thermal stability is poor. During the extrusion molding process, polypropylene carbonate is prone to chain scission and degradation under high temperature conditions. This leads to harsh processing conditions for polypropylene carbonate, and the low-temperature brittleness and weather resistance of its finished product are not ideal.

[0045] In order to solve the above problems, the present invention compounds methacrylic acid monomer with polypropylene carbonate material, uses maleic anhydride as a compatibilizer, and a large number of carboxyl groups in the methacrylic acid monomer can react chemically with the terminal hydroxyl groups of the polypropylene carbonate material, thereby obtaining a polypropylene carbonate material containing an ester bond. The formation of the ester bond inhibits the chain scission degradation of the polypropylene carbonate material at high temperature, thereby improving the thermal stability, processing performance and weather resistance of the polypropylene carbonate material.

[0046] After the modified polypropylene carbonate is prepared, the invention uses the waterborne polyurethane containing the modified polypropylene carbonate as a sizing agent to prepare the paper base layer.

[0047] In order to prepare the paper base layer, S200 specifically includes:

[0048] S210, mixing dibutyltin dilaurate, polyester diol, and isophorone diisocyanate, reacting at a temperature of 80° C. to 85° C. for 3 to 4 hours, and then cooling to obtain a second mixture;

[0049] S220, mixing Tween 60, ethylenediamine, the second mixture, modified polypropylene carbonate, ethyl acetate and water and performing ultrasonic emulsification to obtain a sizing agent;

[0050] S230, 8g / m 2 Up to 12g / m 2 The sizing agent is applied to the base paper to obtain a paper base layer.

[0051] Specifically, in S210, the mass ratio of dibutyltin dilaurate:polyester diol:isophorone diisocyanate=(0.2-0.4):(80-120):100.

[0052] Preferably, in S210 , the mass ratio of dibutyltin dilaurate: polyester diol: isophorone diisocyanate=0.2:80:100.

[0053] Specifically, in S220, the mass ratio of Tween 60:ethylenediamine:second mixture:modified polypropylene carbonate:ethyl acetate:water=(4-6):(4-6):(15-20):(10-15):(40-50):100.

[0054] Preferably, in S220, the mass ratio of Tween 60:ethylenediamine:second mixture:modified polypropylene carbonate:ethyl acetate:water=6:4:15:15:50:100.

[0055] It should be noted that, in the present invention, those skilled in the art can select the base paper to be sized, or adjust the corresponding preparation process, according to actual needs, to obtain the base paper.

[0056] Exemplarily, the base paper of the present invention is prepared by the following process: mixing raw materials including a wet strength agent, aluminum sulfate, a filler, and wood pulp to obtain pulp; placing the pulp on a net to make a wet paper sheet; pressing and drying the wet paper sheet to obtain base paper. The filler may be silicon oxide, kaolin, titanium dioxide, montmorillonite, etc. The wood pulp may be bleached coniferous wood pulp or hardwood wood pulp.

[0057] Those skilled in the art can select and adjust the equipment, raw materials and process parameters used in pulping, papermaking and pressing according to actual needs. The base paper manufacturing is a prior art and will not be described in detail in the present invention.

[0058] The purpose of sizing is to enhance the anti-permeability of the paper-based facing material so that the paper-based facing material can better resist the penetration of liquids such as water and grease, thereby keeping it dry and tidy. In addition, the sizing agent can form a protective film on the surface of the paper-based facing material, which helps to prevent it from tearing and wrinkling, thereby improving the strength and stability of the paper. The present invention selects a surface sizing method for sizing, that is, spraying a thin layer of sizing agent on the surface of the paper-based facing material to form a protective film on the surface of the base paper. The surface sizing process of the present invention is carried out on a papermaking machine. After the base paper is sizing with the sizing agent, the paper base layer can also be dried and calendered.

[0059] One of the improvements made by the present invention over the prior art is that a sizing agent is prepared with modified polypropylene carbonate. The sizing agent of the present invention is an aqueous polyurethane obtained by reacting polyester diol and isophorone diisocyanate. Among them, dibutyltin dilaurate is used as a catalyst to accelerate the reaction rate in the polyurethane synthesis process, shorten the synthesis time, and improve production efficiency. After dibutyltin dilaurate, polyester diol, and isophorone diisocyanate are mixed and reacted for a certain period of time at a temperature of 80° C. to 85° C., a second mixture as a prepolymer can be obtained. Subsequently, the second mixture is mixed with ethylenediamine, which can form a nucleophilic addition product with isocyanate and further participate in the polymerization reaction, thereby improving the reaction efficiency. Tween 60 is used as an emulsifier, and modified polypropylene carbonate, ethyl acetate and water are mixed with the second mixture to obtain an aqueous polyurethane emulsion containing modified polypropylene carbonate. The aqueous polyurethane emulsion containing modified polypropylene carbonate is used as a sizing agent and applied to base paper, which can not only improve the water resistance of the paper, but also evenly apply the modified polypropylene carbonate on the surface of the base paper.

[0060] Preferably, S210 is carried out under nitrogen protection, and during the reaction of S210, stirring is performed at a rate of 200 r / min to 400 r / min. In the later stage of the reaction, the mass fraction of -NCO groups can be determined by the di-n-butylamine method. When the mass fraction reaches a theoretical value of 5% to 6%, the prepolymerization is completed to obtain a second mixture as a prepolymer.

[0061] Preferably, S220 is carried out at a temperature of 35° C. to 40° C., and during the reaction of S220, stirring is performed at a rate of 200 r / min to 400 r / min. In S220, Tween 60, modified polypropylene carbonate, and ethyl acetate are first mixed, and then ethylenediamine, the second mixture, and water are added and mixed, and ultrasonic emulsification is performed to make them uniform.

[0062] In order to prepare the polymer layer, S300 specifically includes:

[0063] S310, uniformly mixing the compatibilizer, the second chain extender, the modified polypropylene carbonate and the polybutylene terephthalate adipate to obtain a third mixture;

[0064] S320, melt-extrude the third mixture at a temperature of 150° C. to 170° C. to obtain a polymer layer.

[0065] In S310, the mass ratio of compatibilizer:second chain extender:modified polypropylene carbonate:polybutylene terephthalate adipate=(1-2):(1-2):(50-60):100.

[0066] Preferably, in S310, the mass ratio of compatibilizer: second chain extender: modified polypropylene carbonate: polybutylene terephthalate adipate is 1:2:50:100.

[0067] Preferably, the compatibilizer includes at least one of the following or a combination thereof: succinic anhydride, maleic anhydride, ethylene-methyl acrylate-glycidyl methacrylate.

[0068] Preferably, the second chain extender includes at least one of the following or a combination thereof: BASF ADR-4370, BASF ADR-4368, BASF ADR-4380.

[0069] In S320, melt extrusion can be performed by a twin-screw extruder, the aspect ratio of the twin-screw extruder is 36:1, and the rotation speed of the twin-screw extruder is 200 rpm to 300 rpm. Preferably, the process temperature of each section of the twin-screw extruder is: zone 1 is 150°C to 155°C, zone 2 is 155°C to 160°C, zone 3 is 160°C to 165°C, and zone 4 is 165°C to 170°C.

[0070] In S400, a hot press is used to heat-press and laminate the paper base layer and the polymer layer at a temperature of 120° C. to 130° C. to obtain a composite material.

[0071] Example 1

[0072] This embodiment provides a composite material for forming a paper-plastic composite bag, and the preparation method thereof is as follows:

[0073] S1. According to the mass ratio of antioxidant 1010: BASF ADR-4370: maleic anhydride: methacrylic acid monomer: polypropylene carbonate = 1:3:5:15:100, antioxidant 1010, BASF ADR-4370, maleic anhydride, methacrylic acid monomer and polypropylene carbonate are mixed uniformly to obtain a first mixture;

[0074] S2, kneading the first mixture at a temperature of 170° C. to 175° C. for 2 hours and then extruding and granulating the mixture to obtain modified polypropylene carbonate;

[0075] S3, dibutyltin dilaurate, polyester diol, and isophorone diisocyanate are mixed in a mass ratio of dibutyltin dilaurate: polyester diol: isophorone diisocyanate = 0.2:80:100, and reacted at a temperature of 80° C. for 3 hours and then cooled to obtain a second mixture;

[0076] S4, mixing Tween 60, ethylenediamine, the second mixture, modified polypropylene carbonate, ethyl acetate and water in a mass ratio of Tween 60: ethylenediamine: the second mixture: modified polypropylene carbonate: ethyl acetate: water = 6:4:15:15:50:100 and ultrasonically emulsifying to obtain a sizing agent;

[0077] S5, 8g / m 2 The sizing agent is applied to the base paper to obtain a paper base layer;

[0078] S6. Succinic anhydride, BASF ADR-4370, modified polypropylene carbonate and polybutylene terephthalate adipate are uniformly mixed in a mass ratio of succinic anhydride: BASF ADR-4370: modified polypropylene carbonate: polybutylene terephthalate adipate = 1:2:50:100 to obtain a third mixture;

[0079] S7, melt-extrude the third mixture at a temperature of 150° C. to 170° C. to obtain a polymer layer;

[0080] S8. Using a hot press machine, hot press the paper base layer and the polymer layer at a temperature of 125±2° C. to obtain a composite material.

[0081] Example 2

[0082] This embodiment provides a composite material for forming a paper-plastic composite bag, and the preparation method thereof is as follows:

[0083] S1. According to the mass ratio of antioxidant 1010: BASF ADR-4370: maleic anhydride: methacrylic acid monomer: polypropylene carbonate = 2:2:3:20:100, antioxidant 1010, BASF ADR-4370, maleic anhydride, methacrylic acid monomer and polypropylene carbonate are mixed uniformly to obtain a first mixture;

[0084] S2, kneading the first mixture at a temperature of 170° C. to 175° C. for 2 hours and then extruding and granulating the mixture to obtain modified polypropylene carbonate;

[0085] S3, dibutyltin dilaurate, polyester diol, and isophorone diisocyanate are mixed in a mass ratio of dibutyltin dilaurate: polyester diol: isophorone diisocyanate = 0.4:100:100, and reacted at 80° C. for 3 hours and then cooled to obtain a second mixture;

[0086] S4, mixing Tween 60, ethylenediamine, the second mixture, modified polypropylene carbonate, ethyl acetate and water in a mass ratio of Tween 60: ethylenediamine: the second mixture: modified polypropylene carbonate: ethyl acetate: water = 4:6:20:10:40:100 and ultrasonically emulsifying to obtain a sizing agent;

[0087] S5, 10g / m 2 The sizing agent is applied to the base paper to obtain a paper base layer;

[0088] S6. Succinic anhydride, BASF ADR-4370, modified polypropylene carbonate and polybutylene terephthalate adipate are uniformly mixed in a mass ratio of succinic anhydride: BASF ADR-4370: modified polypropylene carbonate: polybutylene terephthalate adipate = 1:1:60:100 to obtain a third mixture;

[0089] S7, melt-extrude the third mixture at a temperature of 150° C. to 170° C. to obtain a polymer layer;

[0090] S8. Using a hot press machine, hot press the paper base layer and the polymer layer at a temperature of 125±2° C. to obtain a composite material.

[0091] Comparative Example 1

[0092] This comparative example provides a composite material for forming a paper-plastic composite bag, and the preparation method thereof is as follows:

[0093] S1. According to the mass ratio of antioxidant 1010: BASF ADR-4370: maleic anhydride: methacrylic acid monomer: polypropylene carbonate = 1:3:5:15:100, antioxidant 1010, BASF ADR-4370, maleic anhydride, methacrylic acid monomer and polypropylene carbonate are mixed uniformly to obtain a first mixture;

[0094] S2, kneading the first mixture at a temperature of 170° C. to 175° C. for 2 hours and then extruding and granulating the mixture to obtain modified polypropylene carbonate;

[0095] S3, succinic anhydride, BASF ADR-4370, modified polypropylene carbonate and polybutylene terephthalate adipate are uniformly mixed in a mass ratio of succinic anhydride: BASF ADR-4370: modified polypropylene carbonate: polybutylene terephthalate adipate = 1:2:50:100 to obtain a third mixture;

[0096] S4, melt-extrude the third mixture at a temperature of 150° C. to 170° C. to obtain a polymer layer;

[0097] S5. Using a hot press machine, hot-press the paper base layer and the polymer layer at a temperature of 125±2° C. to obtain a composite material, wherein the paper base layer is purchased through commercial channels.

[0098] Performance Testing

[0099] First, the samples obtained in Example 1, Example 2 and Comparative Example 1 were subjected to artificial accelerated aging at 365 nm, 20 W / m 2 The samples obtained in Example 1, Example 2 and Comparative Example 1 were irradiated with an ultraviolet light source for 10 days at a temperature of 60° C. and a humidity of 80 RH. The physical and chemical properties of the samples were tested after artificial accelerated aging, and the specific data are shown in Table 1.

[0100] Table 1

[0101] Serial number Example 1 Example 2 Comparative Example 1 Elongation at break 178.2% 172.5% 153.6% Tensile Strength 11.4MPa 10.8MPa 8.6MPa

[0102] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.

Claims

1. A method for preparing a composite material for forming a paper-plastic composite bag, characterized in that: The preparation method comprises: S100, preparing modified polypropylene carbonate; S200, using the aqueous polyurethane containing the modified polypropylene carbonate as a sizing agent to prepare a paper base layer; S300, preparing a polymer layer using raw materials including the modified polypropylene carbonate and polybutylene adipate terephthalate; S400, hot-pressing the paper base layer and the polymer layer to obtain the composite material.

2. The preparation method according to claim 1, characterized in that: S100 specifically includes: S110, uniformly mixing an antioxidant, a first chain extender, maleic anhydride, methacrylic acid monomer and polypropylene carbonate to obtain a first mixture; S120, kneading the first mixture at a temperature of 170° C. to 175° C. for 2 h to 2.5 h, and then extruding and granulating the mixture to obtain the modified polypropylene carbonate.

3. The preparation method according to claim 2, characterized in that: In S110, the weight ratio of antioxidant: first chain extender: maleic anhydride: methacrylic acid monomer: polypropylene carbonate is (1-2): (2-4): (3-5): (15-20):

100.

4. The preparation method according to claim 2, characterized in that: The antioxidant comprises at least one of the following or a combination thereof: antioxidant 1010, antioxidant 1076, antioxidant 1098; and / or The first chain extender includes at least one of the following or a combination thereof: BASF ADR-4370, BASF ADR-4368, BASF ADR-4380.

5. The preparation method according to any one of claims 1 to 4, characterized in that: S200 specifically includes: S210, mixing dibutyltin dilaurate, polyester diol, and isophorone diisocyanate, reacting at a temperature of 80° C. to 85° C. for 3 to 4 hours, and then cooling to obtain a second mixture; S220, mixing Tween 60, ethylenediamine, the second mixture, the modified polypropylene carbonate, ethyl acetate and water and performing ultrasonic emulsification to obtain the sizing agent; S230, 8g / m 2 Up to 12g / m 2 The sizing agent is applied to base paper to obtain the paper base layer.

6. The preparation method according to claim 5, characterized in that: In S210, in terms of mass ratio, dibutyltin dilaurate: polyester diol: isophorone diisocyanate = (0.2-0.4): (80-120): 100; and / or In S220, the mass ratio of Tween 60:ethylenediamine:second mixture:modified polypropylene carbonate:ethyl acetate:water=(4-6):(4-6):(15-20):(10-15):(40-50):

100.

7. The preparation method according to claim 5, characterized in that: S300 specifically includes: S310, uniformly mixing the compatibilizer, the second chain extender, the modified polypropylene carbonate and the polybutylene terephthalate adipate to obtain a third mixture; S320, melt-extrude the third mixture at a temperature of 150° C. to 170° C. to obtain the polymer layer.

8. The preparation method according to claim 7, characterized in that: In S310, the mass ratio of compatibilizer:second chain extender:modified polypropylene carbonate:polybutylene terephthalate adipate=(1-2):(1-2):(50-60):

100.

9. The preparation method according to claim 7, characterized in that: The compatibilizer includes at least one of the following or a combination thereof: succinic anhydride, maleic anhydride, ethylene-methyl acrylate-glycidyl methacrylate; and / or The second chain extender includes at least one of the following or a combination thereof: BASF ADR-4370, BASF ADR-4368, BASF ADR-4380.

10. A composite material for forming a paper-plastic composite bag, characterized in that: The composite material is obtained by the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Biodegradable polypropylene carbonate composite material and preparation method thereof

    CN101962470A

  • Poly(propylene carbonate)-based water-borne polyurethane adhesive and preparation method thereof

    CN102241956A

  • Blend of carbon dioxide-epoxypropane copolymer and preparation method of blend

    CN104177805A

  • Modified waterborne polyurethane emulsion and preparation method and application thereof

    CN108794717A

  • Carbon dioxide-propylene oxide copolymer based paper-plastic composite film and preparation method thereof

    CN111890761A