Lithium bis (fluorosulfonyl) imide solution as well as preparation method and application thereof
By performing metathesis reaction of lithium chloride and bisfluorosulfonimide in a non-aqueous solvent, combined with degassing and concentration and resin deacidification treatment, the problem of difficult removal of impurities in the preparation of lithium bisfluorosulfonimide is solved, and the problem of obtaining High-purity products, simplify process flow and reduce costs, and are suitable for industrial production.
Patent Information
- Application Number
- CN202411193289.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-06
AI Technical Summary
In the prior art, the preparation method of lithium difluorosulfonimide is complicated and difficult to remove impurities, resulting in high impurities content of the product, affecting the internal resistance, capacity and cycle life of the lithium battery, and has a long process route and high cost.
Suspend lithium chloride in a non-aqueous solvent for metathesis reaction, followed by degassing and concentration, resin deacidification and filtration to obtain a high-purity lithium difluorosulfonimide solution, avoiding the water removal process Impurities are introduced into it, controlling the moisture content and acidic impurity concentration of the product.
The preparation of high-purity and low-impact lithium bisfluorosulfonimide solution is achieved, which simplifies the process flow, reduces costs, is suitable for industrial production, and ensures the working performance of lithium batteries.
Smart Images

Figure CN119079942A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium batteries, in particular to an electrolyte of a lithium battery, and in particular to a lithium bis(fluorosulfonyl)imide solution and a preparation method and application thereof. Background Art
[0002] Lithium bis(fluorosulfonyl)imide is mainly used as an important electrolyte salt for non-aqueous electrolyte of lithium battery, and requires high purity (usually not less than 99.5%). The content of impurities such as water, alkali metals, heavy metals, chloride ions, sulfate, and other free acids must be strictly controlled, otherwise it will lead to increased internal resistance of lithium battery, rapid battery capacity decay, short cycle life, and even affect battery safety. Therefore, it is of great significance to obtain lithium bis(fluorosulfonyl)imide products with high purity and low content of harmful impurities.
[0003] The synthesis method of lithium bis(fluorosulfonyl)imide (LiFSI) commonly used in the prior art is to first synthesize bis(chlorosulfonyl)imide (HClSI), and then prepare the corresponding bis(fluorosulfonyl)imide (HFSI) or salt (MFSI) intermediate through a fluorination reaction, and the intermediate is then reacted with lithium hydroxide or a lithium salt to undergo acid-base neutralization or cation exchange, thereby obtaining lithium bis(fluorosulfonyl)imide.
[0004] When lithium hydroxide or lithium carbonate is used for neutralization reaction to prepare lithium bis(fluorosulfonyl)imide, such as patents US2013331609, US 2012041233, US 9156692, EP 2415757, and CN 14735665A, not only is the reaction highly exothermic and requires cooling, but water is also generated, increasing the difficulty of post-processing. Cation exchange by double decomposition reaction is a commonly used strategy, such as patents CN 116143086A and CN 101747242A use potassium bis(fluorosulfonyl)imide and lithium perchlorate to undergo double decomposition reaction to obtain lithium bis(fluorosulfonyl)imide; patent CN 116654882A uses potassium bis(fluorosulfonyl)imide and lithium chloride to exchange in anhydrous acetonitrile; patent CN 116835539A first uses potassium carbonate to replace triethylamine salt to obtain potassium bis(fluorosulfonyl)imide, and then uses lithium tetrafluoroborate and potassium bis(fluorosulfonyl)imide to undergo double decomposition reaction to obtain lithium bis(fluorosulfonyl)imide; patent CN116495711A uses potassium bis(fluorosulfonyl)imide and lithium nitrate to undergo double decomposition reaction to obtain lithium bis(fluorosulfonyl)imide. However, the disadvantage of these methods is that the cation exchange only reaches an equilibrium and is difficult to be carried out completely, and the unexchanged cations are difficult to be completely separated from the lithium bis(fluorosulfonyl)imide, so that high-quality products cannot be obtained. Patents CN 107055493A and CN 115959636A respectively use bis(fluorosulfonyl)imide to react with lithium carboxylate and lithium fluoride to prepare lithium bis(fluorosulfonyl)imide, but the generated carboxylic acid and hydrogen fluoride are difficult to remove.
[0005] Therefore, how to produce lithium bis(fluorosulfonyl)imide with low impurity content and harmless impurities has become a difficult problem faced by various manufacturers. Summary of the invention
[0006] In view of the problems existing in the prior art, the present invention provides a lithium bis(fluorosulfonyl)imide solution and a preparation method and application thereof, wherein the preparation method comprises: performing a double decomposition reaction on lithium chloride suspended in a non-aqueous solvent and bis(fluorosulfonyl)imide, and sequentially performing degassing and concentration, resin deacidification, and filtration on the obtained reaction system to obtain a lithium bis(fluorosulfonyl)imide solution. The lithium bis(fluorosulfonyl)imide solution obtained by the preparation method of the present invention has the advantages of high concentration and low impurity content, and can be directly used as an electrolyte for the production of lithium battery electrolytes. Moreover, the preparation method of the present invention has the advantages of cheap and readily available reaction raw materials, simple operation, recyclable by-products, and is suitable for industrial production.
[0007] To achieve this object, the present invention adopts the following technical solutions:
[0008] One of the purposes of the present invention is to provide a method for preparing a lithium bis(fluorosulfonyl)imide solution, the preparation method comprising the following steps:
[0009] (1) Lithium chloride suspended in a non-aqueous solvent is subjected to a double decomposition reaction with bis(fluorosulfonyl)imide to obtain a reaction system;
[0010] (2) The reaction system of step (1) is sequentially degassed and concentrated, resin deacidified, and filtered to obtain a lithium bis(fluorosulfonyl)imide solution.
[0011] The preparation method of the present invention allows lithium chloride and bis(fluorosulfonyl)imide to undergo double decomposition reaction in a non-aqueous solvent to generate lithium bis(fluorosulfonyl)imide and hydrogen chloride, and the reaction system obtained by the reaction is subjected to degassing and concentration, ion exchange resin deacidification, filtration and other refining processes in sequence. The obtained lithium bis(fluorosulfonyl)imide solution has the advantages of high concentration and low impurity content, and can be directly used as an electrolyte for lithium battery electrolyte production. Moreover, the preparation method of the present invention has the advantages of cheap and readily available reaction raw materials, simple operation, recyclable by-products, and suitability for industrial production, and is helpful to solve the problems of complex preparation methods, difficult impurity removal, and long process routes of lithium bis(fluorosulfonyl)imide products in the prior art.
[0012] The preparation method of the present invention obtains lithium bis(fluorosulfonyl)imide by reacting bis(fluorosulfonyl)imide and lithium chloride in a non-aqueous solvent, thereby avoiding the process of water removal and the introduction of impurities in the water removal process, effectively controlling the water content of the product, and removing most of the generated hydrogen chloride by degassing and concentration, and removing the residual acid by ion exchange resin, thereby obtaining a high-purity lithium bis(fluorosulfonyl)imide solution.
[0013] It should be noted that degassing and concentration refers to a method of removing acidic gases from the reaction solution by volatilizing the hydrogen chloride gas dissolved in the solvent and discharging it outside the system under reduced pressure or by passing a carrier gas such as nitrogen. The present invention finds that by using degassing and concentration, the concentration of the solute is increased, and the acidic impurities are also discharged along with the solvent, so that a high-purity lithium bis(fluorosulfonyl)imide solution can be produced. The lower the concentration of acidic impurities contained in the lithium bis(fluorosulfonyl)imide solution, the better. The concentration of acidic impurities contained in the concentrated solution obtained in the present invention is less than 100 ppm, and more preferably less than 60 ppm. When the concentration of the acidic impurities exceeds the above range, it will have an adverse effect on the characteristics of the lithium battery. This method can easily produce a high-purity lithium bis(fluorosulfonyl)imide solution, only requires one reactor, and does not require a complex heating or cooling device, thereby reducing the manufacturing cost.
[0014] Preferably, in the preparation method of the present invention, bis(fluorosulfonyl)imide is added dropwise to lithium chloride suspended in a non-aqueous solvent, and a double decomposition reaction is carried out under stirring.
[0015] As a preferred technical solution of the present invention, in step (1), the molar ratio of lithium chloride to bis(fluorosulfonyl)imide is (0.8-1.2):1, for example, 0.8:1, 0.85:1, 0.9:1, 0.92:1, 0.94:1, 0.96:1, 1:1, 1.02:1, 1.04:1, 1.06:1, 1.08:1, 1.1:1, 1.15:1 or 1.2:1, etc.
[0016] As a preferred technical solution of the present invention, in step (1), the purity of lithium chloride and bis(fluorosulfonyl)imide is greater than 99.5wt%, and the water content does not exceed 50ppm.
[0017] As a preferred technical solution of the present invention, in step (1), the water content of the non-aqueous solvent is less than 15 ppm, and the non-aqueous solvent includes at least one of dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethyl acetate, acetone, ether, dimethylformamide, ethylene glycol dimethyl ether, acetonitrile or tetrahydrofuran.
[0018] As a preferred technical solution of the present invention, in step (1), the reaction temperature of the double decomposition reaction is 0-40°C, for example, 0°C, 5°C, 10°C, 15°C, 20°C, 25°C, 30°C, 35°C or 40°C.
[0019] Preferably, in step (1), the reaction time of the metathesis reaction is 2 to 6 h, for example, 2 h, 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h, 5 h, 5.5 h or 6 h.
[0020] It should be noted that if the reaction temperature of the metathesis reaction of the present invention is higher than 40° C., side reactions may occur and the color of the solution may deepen. In addition, there is no particular restriction on the pressure during the reaction of the metathesis reaction of the present invention. Since hydrogen chloride gas is generated, it is necessary to discharge the reaction system in a timely manner.
[0021] As a preferred technical solution of the present invention, in step (1), the metathesis reaction is carried out under an inert gas atmosphere.
[0022] Preferably, the inert gas is at least one of nitrogen, argon or helium.
[0023] It should be noted that all operations in the preparation method of the present invention are carried out under an inert gas atmosphere to avoid the occurrence of side reactions as much as possible.
[0024] As a preferred technical solution of the present invention, in step (2), the degassing and concentration is a reduced pressure degassing, and the pressure range is 0.05 to 10 kPa, for example, 0.05 kPa, 0.5 kPa, 1 kPa, 1.5 kPa, 2 kPa, 2.5 kPa, 3 kPa, 3.5 kPa, 4 kPa, 4.5 kPa, 5 kPa, 5.5 kPa, 6 kPa, 6.5 kPa, 7 kPa, 7.5 kPa, 8 kPa, 8.5 kPa, 9 kPa, 9.5 kPa or 10 kPa, etc.
[0025] Preferably, in step (2), the temperature of the degassing and concentration is 20-80°C, for example, 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C or 80°C, etc.
[0026] Preferably, in step (2), the degassing and concentration time is 4 to 8 hours, for example, 4 hours, 4.5 hours, 5 hours, 5.5 hours, 6 hours, 6.5 hours, 7 hours, 7.5 hours or 8 hours.
[0027] It should be noted that in the preparation method of the present invention, degassing and concentration can not only remove the hydrogen chloride gas present in the reaction system, but also remove excess non-aqueous solvent. The degassing and concentration is decompression degassing. The lower the pressure in the system and the higher the temperature, the more effectively the degassing and concentration can be performed. However, when the temperature is too high, the obtained concentrated solution produces color, or the yield decreases due to the decomposition of lithium bis(fluorosulfonyl)imide, so the upper limit of the temperature is 80°C, preferably 60°C. In addition, when the temperature is too low, it is possible to solidify the non-aqueous organic solvent, and it is difficult to remove acidic impurities during solidification, so the lower limit of the temperature is 20°C, preferably 30°C. The pressure of the above-mentioned system decompression is determined according to the temperature of the reaction solution and the solvent vapor pressure, and cannot be generalized. It is preferred that the vacuum degree in the reactor is maintained below 10kPa. When the pressure maintained exceeds 10kPa, it takes a long time or cannot remove the impurity hydrogen chloride to below the target concentration. In addition, when the pressure maintained is below 3kPa, the aforementioned impurities can be excluded to a low concentration, so it is more preferred. Impurities can also be removed by passing a carrier gas, in which case it can be passed only over the liquid, but it is more effective to pass bubbles into the liquid. The degree of concentration depends on the initial concentration of lithium bis(fluorosulfonyl)imide, and the higher the concentration of lithium bis(fluorosulfonyl)imide after concentration, the better.
[0028] As a preferred technical solution of the present invention, in step (2), the operating temperature of the resin deacidification is 20-60°C, for example, 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C or 60°C.
[0029] It should be noted that the preparation method of the present invention passes the concentrated solution obtained by degassing and concentration through an ion exchange resin to remove residual acidic impurities such as hydrogen chloride. In order to prevent the decomposition of lithium bis(fluorosulfonyl)imide, the solvent and the ion exchange resin, the temperature at this time is preferably 50° C. From the perspective of the viscosity of the concentrated solution passed through the ion exchange resin, 30° C. is more preferred.
[0030] Preferably, in step (2), the matrix structure of the ion exchange resin used for resin deacidification is any one of styrene divinyl benzene copolymer, styrene resin or acrylic (ester) resin, and the functional groups are -N(CH3)2, -N + (CH3)3, -N + Any one of (C2H4OH)(CH3)2.
[0031] Preferably, in step (2), the adsorption time of the resin deacidification is 1 to 5 hours, for example, 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours, 4.5 hours or 5 hours.
[0032] It should be noted that in the preparation method of the present invention, after the resin is deacidified, the insoluble matter is removed by precise filtration, and the concentration is adjusted with dimethyl carbonate to obtain a lithium bis(fluorosulfonyl)imide solution of the target concentration, for example, a lithium bis(fluorosulfonyl)imide solution with a weight concentration of 10-40%.
[0033] The second object of the present invention is to provide a lithium bis(fluorosulfonyl)imide solution, which is prepared by the preparation method described in the first object, wherein the chloride ion content of the lithium bis(fluorosulfonyl)imide solution is below 5 ppm and the acidity of the free acid is below 50 ppm.
[0034] It should be noted that the chloride ion content in the lithium bis(fluorosulfonyl)imide solution prepared by the present invention is below 5 ppm. The concentration of free acid in the concentrated solution is tested by titration, and the acidity result is below 50 ppm. Since the chloride and free acid contents in the solution are relatively low, the concentrated solution can be directly used as a lithium salt electrolyte material for lithium batteries.
[0035] The third object of the present invention is to provide an application of a lithium bis(fluorosulfonyl)imide solution, characterized in that the lithium bis(fluorosulfonyl)imide solution is used in a lithium battery;
[0036] Wherein, the lithium bis(fluorosulfonyl)imide solution is prepared by the preparation method described in the first purpose, or the lithium bis(fluorosulfonyl)imide solution is the lithium bis(fluorosulfonyl)imide solution described in the second purpose.
[0037] Compared with the prior art solutions, the present invention has at least the following beneficial effects:
[0038] (1) The preparation method of the present invention not only has mild reaction conditions and high yield of the obtained product, but also has cheap and readily available reaction raw materials, which can significantly save costs. In addition, the only by-product produced is hydrogen chloride gas, which can be absorbed by alkali solution, and is environmentally friendly.
[0039] (2) The preparation method of the present invention has few reaction steps, is easy to operate, and has simple post-reaction treatment, and is suitable for industrial production;
[0040] (3) The bis(fluorosulfonyl)imide lithium solution prepared by the present invention is used as a lithium salt electrolyte for lithium batteries, which can ensure the working performance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 The nuclear magnetic fluorine spectrum of the product obtained in Example 3 of the present invention is 19 F-NMR spectrum. DETAILED DESCRIPTION
[0042] The technical solution of the present invention is further described below with reference to the accompanying drawings and through specific implementation methods.
[0043] The invention provides a method for preparing a lithium bis(fluorosulfonyl)imide solution. The lithium bis(fluorosulfonyl)imide solution can be prepared by using cheap and readily available raw materials and reacting under mild conditions. The preparation method comprises: dispersing lithium chloride particles in a non-aqueous solvent under an inert gas atmosphere, adding bis(fluorosulfonyl)imide to carry out double decomposition reaction to obtain lithium bis(fluorosulfonyl)imide, and then degassing and concentrating the obtained lithium bis(fluorosulfonyl)imide solution, deacidifying the resin, and fine filtering to obtain a high-quality lithium bis(fluorosulfonyl)imide solution; the reaction equation is as follows: LiCl+HFSI→LiFSI+HCl.
[0044] To better illustrate the present invention and facilitate understanding of the technical solution of the present invention, typical but non-limiting embodiments of the present invention are as follows:
[0045] Example 1
[0046] This embodiment provides a method for preparing a lithium bis(fluorosulfonyl)imide solution, the preparation method comprising the following steps:
[0047] In a 100mL three-necked flask, under nitrogen protection, add 50mL of dimethyl carbonate and 1.017g (0.024mol) of lithium chloride, and slowly add 3.623g (0.02mol) of bis(fluorosulfonyl)imide acid (HFSI) under stirring at 25°C for about 10 minutes. After the reaction, continue the reaction for 2 hours under stirring at 25°C. After the reaction, maintain the same conditions, turn on the vacuum pump to vacuum the reaction bottle for degassing and concentration, control the degassing and concentration temperature to 25°C, and it takes about 4 hours to complete under a pressure of 0.50kPa. The degassed lithium bis(fluorosulfonyl)imide solution is then deacidified by an ion exchange resin, and the operating temperature of the resin deacidification is controlled to be 25°C. The matrix structure of the ion exchange resin used for the resin deacidification is styrene divinylbenzene copolymer, and the functional group is -N(CH3)2. The adsorption time of the resin deacidification is controlled to be 5 hours. After filtration, the concentration is adjusted with dimethyl carbonate to obtain a lithium bis(fluorosulfonyl)imide solution with a weight concentration of about 30%.
[0048] The test results of this embodiment are as follows: lithium bis(fluorosulfonyl)imide content is 29.95%, free acid (calculated as HCl) is 41 ppm, moisture (Karl Fischer method) is 14 ppm, alkali metal ion content (calculated as K) is 1 ppm, chloride ion content is 121 ppm, heavy metal ion content (calculated as Fe) is 1 ppm, and insoluble matter content is 80 ppm.
[0049] Example 2
[0050] This embodiment provides a method for preparing a lithium bis(fluorosulfonyl)imide solution, the preparation method comprising the following steps:
[0051] In a 100mL three-necked flask, under nitrogen protection, add 50mL of dimethyl carbonate and 0.8478g (0.02mol) of lithium chloride, and slowly add 4.347g (0.024mol) of bis(fluorosulfonyl)imide (HFSI) under stirring at 25°C for about 10 minutes. After the reaction, maintain the temperature at 25°C and continue stirring to react for 2 hours. After the reaction, maintain the same conditions, turn on the vacuum pump to slowly evacuate the reaction bottle for degassing and concentration, control the degassing and concentration temperature to 80°C, and complete it at a pressure of 0.50kPa for about 2 hours. Then the degassed lithium bis(fluorosulfonyl)imide solution is deacidified by ion exchange resin, and the operating temperature of the resin deacidification is controlled to 60°C. The matrix structure of the ion exchange resin used for the resin deacidification is a styrene resin, and the functional groups are -N(CH3)2, -N + (CH3)3, control the resin deacidification adsorption time to 1h, and after filtration, adjust the concentration with dimethyl carbonate to obtain a lithium bis(fluorosulfonyl)imide solution with a weight concentration of about 30%.
[0052] The test results of this embodiment are as follows: lithium bis(fluorosulfonyl)imide content is 30.04%, free acid (calculated as HCl) is 32 ppm, moisture (Karl Fischer method) is 16 ppm, alkali metal ion content (calculated as K) is 1 ppm, chloride ion content is 5 ppm, heavy metal ion content (calculated as Fe) is 1 ppm, and insoluble matter content is 76 ppm.
[0053] Example 3
[0054] This embodiment provides a method for preparing a lithium bis(fluorosulfonyl)imide solution, the preparation method comprising the following steps:
[0055] In a 100mL three-necked flask, under nitrogen protection, add 50mL of dimethyl carbonate and 0.8478g (0.02mol) of lithium chloride, and slowly add 3.623g (0.02mol) of bis(fluorosulfonyl)imide (HFSI) under stirring at 25°C for about 10 minutes. After the reaction, maintain 25°C and continue stirring to react for 2 hours. After the reaction, maintain the same conditions, turn on the vacuum pump to slowly evacuate the reaction bottle for degassing and concentration, control the degassing and concentration temperature to 50°C, and complete it at a pressure of 0.50kPa for about 4 hours. The degassed lithium bis(fluorosulfonyl)imide solution is then deacidified by an ion exchange resin, and the operating temperature of the resin deacidification is controlled to be 40°C. The matrix structure of the ion exchange resin used for the resin deacidification is styrene divinylbenzene copolymer, and the functional group is -N(CH3)2. The adsorption time of the resin deacidification is controlled to be 3h. After filtration, the concentration is adjusted with dimethyl carbonate to obtain a lithium bis(fluorosulfonyl)imide solution with a weight concentration of about 30%.
[0056] The test results of this example are as follows: the content of lithium bis(fluorosulfonyl)imide is 29.35%, the free acid (calculated as HCl) is 10ppm, the water content (Karl Fischer method) is 13ppm, the alkali metal ion content (calculated as K) is 2ppm, the chloride ion content is 4ppm, the heavy metal ion content (calculated as Fe) is 1ppm, and the insoluble matter content is 62ppm. Moreover, the nuclear magnetic fluorine spectrum of the product 19F-NMR (376MHz, CDCl3): δ50.9(s), as shown in FIG. Figure 1 shown.
[0057] Example 4
[0058] This embodiment provides a method for preparing a lithium bis(fluorosulfonyl)imide solution, the preparation method comprising the following steps:
[0059] In a 100mL three-necked flask, under nitrogen protection, add 50mL of dimethyl carbonate and 0.8478g (0.02mol) of lithium chloride, and slowly add 3.6953g (0.0204mol) of bis(fluorosulfonyl)imide (HFSI) under stirring at 25°C for about 10 minutes. After the reaction, maintain 25°C and continue stirring to react for 2 hours. After the reaction is completed, maintain the same conditions, turn on the vacuum pump to slowly vacuum and degas the reaction bottle, control the degassing and concentration temperature to 60°C, and complete it at a pressure of 0.30kPa for about 3 hours. Then the degassed lithium bis(fluorosulfonyl)imide solution is deacidified by ion exchange resin, and the operating temperature of the resin deacidification is controlled to be 50°C. The matrix structure of the ion exchange resin used for the resin deacidification is styrene divinylbenzene copolymer, and the functional group is -N + (C2H4OH)(CH3)2, control the resin deacidification adsorption time to 4h, after filtration, adjust the concentration with dimethyl carbonate to obtain a lithium bis(fluorosulfonyl)imide solution with a weight concentration of about 30%.
[0060] The test results of this embodiment are as follows: lithium bis(fluorosulfonyl)imide content is 29.42%, free acid (calculated as HF) is 18 ppm, moisture (Karl Fischer method) is 9 ppm, alkali metal ion content (calculated as K) is 1 ppm, chloride ion content is 5 ppm, heavy metal ion content (calculated as Fe) is 1 ppm, and insoluble matter content is 58 ppm.
[0061] Example 5
[0062] This embodiment provides a method for preparing a lithium bis(fluorosulfonyl)imide solution, the preparation method comprising the following steps:
[0063] In a 100mL three-necked flask, under nitrogen protection, add 50mL of dimethyl carbonate and 0.8478g (0.02mol) of lithium chloride, and slowly add 3.7677g (0.0208mol) of bis(fluorosulfonyl)imide (HFSI) under stirring at 25°C for about 10 minutes. After the reaction, maintain 25°C and continue stirring to react for 2 hours. After the reaction, maintain the same conditions, turn on the vacuum pump to slowly evacuate the reaction bottle for degassing and concentration, control the degassing and concentration temperature to 70°C, and complete it at a pressure of 0.50kPa for about 4 hours. The degassed lithium bis(fluorosulfonyl)imide solution is then deacidified by an ion exchange resin, and the operating temperature of the resin deacidification is controlled to be 50°C. The matrix structure of the ion exchange resin used for the resin deacidification is styrene divinylbenzene copolymer, and the functional group is -N(CH3)2. The adsorption time of the resin deacidification is controlled to be 2h. After filtration, the concentration is adjusted with dimethyl carbonate to obtain a lithium bis(fluorosulfonyl)imide solution with a weight concentration of about 30%.
[0064] The test results of this embodiment are as follows: lithium bis(fluorosulfonyl)imide content is 29.07%, free acid (calculated as HF) is 20 ppm, moisture (Karl Fischer method) is 8 ppm, alkali metal ion content (calculated as K) is 1 ppm, chloride ion content is 5 ppm, heavy metal ion content (calculated as Fe) is 1 ppm, and insoluble matter content is 87 ppm.
[0065] Example 6
[0066] This embodiment provides a method for preparing a lithium bis(fluorosulfonyl)imide solution, the preparation method comprising the following steps:
[0067] In a 100mL three-necked flask, under nitrogen protection, add 50mL of dimethyl carbonate, 0.8648g (0.0204mol) of lithium chloride, and slowly add 3.623g (0.02mol) of bis(fluorosulfonyl)imide (HFSI) under stirring at 25°C for about 10 minutes. After the reaction, maintain the temperature at 25°C and continue stirring to react for 2 hours. After the reaction is completed, maintain the same conditions, turn on the vacuum pump to slowly evacuate the reaction bottle for degassing and concentration, control the degassing and concentration temperature to 40°C, and complete it at a pressure of 0.40kPa for about 4 hours. Then the degassed lithium bis(fluorosulfonyl)imide solution is deacidified by ion exchange resin, and the operating temperature of the resin deacidification is controlled to be 30°C. The matrix structure of the ion exchange resin used for the resin deacidification is a styrene resin with a functional group of -N + (C2H4OH)(CH3)2, the adsorption time of resin deacidification is controlled to be 4h, and after filtration, the concentration is adjusted with dimethyl carbonate to obtain a lithium bis(fluorosulfonyl)imide solution with a weight concentration of about 30%.
[0068] The test results of this embodiment are as follows: lithium bis(fluorosulfonyl)imide content is 29.15%, free acid (calculated as HF) is 12ppm, moisture (Karl Fischer method) is 10ppm, alkali metal ion content (calculated as K) is 1ppm, chloride ion content is 25ppm, heavy metal ion content (calculated as Fe) is 1ppm, and insoluble matter content is 71ppm.
[0069] Example 7
[0070] This embodiment provides a method for preparing a lithium bis(fluorosulfonyl)imide solution, the preparation method comprising the following steps:
[0071] In a 100mL three-necked flask, under nitrogen protection, add 50mL of dimethyl carbonate, 0.8817g (0.0208mol) of lithium chloride, and slowly add 3.623g (0.02mol) of bis(fluorosulfonyl)imide (HFSI) under stirring at 25°C for about 10 minutes. After the reaction, maintain the temperature at 25°C and continue stirring to react for 2 hours. After the reaction is completed, maintain the same conditions, turn on the vacuum pump to slowly evacuate the reaction bottle for degassing and concentration, control the degassing and concentration temperature to 30°C, and complete it at a pressure of 0.20kPa for about 3 hours. Then the degassed lithium bis(fluorosulfonyl)imide solution is deacidified by ion exchange resin, and the operating temperature of the resin deacidification is controlled to be 25°C. The matrix structure of the ion exchange resin used for the resin deacidification is acrylic (ester) resin, and the functional group is -N + (C2H4OH)(CH3)2, control the resin deacidification adsorption time to 5h, after filtration, adjust the concentration with dimethyl carbonate to obtain a lithium bis(fluorosulfonyl)imide solution with a weight concentration of about 30%.
[0072] The test results of this embodiment are as follows: lithium bis(fluorosulfonyl)imide content is 30.23%, free acid (calculated as HF) is 8 ppm, moisture (Karl Fischer method) is 9 ppm, alkali metal ion content (calculated as K) is 1 ppm, chloride ion content is 31 ppm, heavy metal ion content (calculated as Fe) is 1 ppm, and insoluble matter content is 55 ppm.
[0073] Comparative Example 1
[0074] This comparative example provides a method for preparing a lithium bis(fluorosulfonyl)imide solution. Compared with Example 3, the only difference is that the temperature for the double decomposition reaction of lithium chloride and bis(fluorosulfonyl)imide is 0°C.
[0075] The test results of this comparative example are as follows: lithium bis(fluorosulfonyl)imide content is 30.31%, free acid (calculated as HF) is 52ppm, moisture (Karl Fischer method) is 9ppm, alkali metal ion content (calculated as K) is 1ppm, chloride ion content is 70ppm, heavy metal ion content (calculated as Fe) is 1ppm, and insoluble matter content is 88ppm.
[0076] Comparative Example 2
[0077] This comparative example provides a method for preparing a lithium bis(fluorosulfonyl)imide solution. Compared with Example 3, the only difference is that the temperature for the double decomposition reaction of lithium chloride and bis(fluorosulfonyl)imide is 40°C.
[0078] The test results of this comparative example are as follows: lithium bis(fluorosulfonyl)imide content is 30.51%, free acid (calculated as HF) is 8ppm, moisture (Karl Fischer method) is 9ppm, alkali metal ion content (calculated as K) is 1ppm, chloride ion content is 5ppm, heavy metal ion content (calculated as Fe) is 1ppm, and insoluble matter content is 48ppm.
[0079] Comparative Example 3
[0080] This comparative example provides a method for preparing a lithium bis(fluorosulfonyl)imide solution. Compared with Example 3, the only difference is that the temperature for the double decomposition reaction of lithium chloride and bis(fluorosulfonyl)imide is -5°C.
[0081] The test results of this comparative example are as follows: lithium bis(fluorosulfonyl)imide content is 25.13%, free acid (calculated as HF) is 117ppm, moisture (Karl Fischer method) is 202ppm, alkali metal ion content (calculated as K) is 15ppm, chloride ion content is 150ppm, heavy metal ion content (calculated as Fe) is 21ppm, and insoluble matter content is 108ppm.
[0082] Comparative Example 4
[0083] This comparative example provides a method for preparing a lithium bis(fluorosulfonyl)imide solution. Compared with Example 3, the only difference is that the temperature for the double decomposition reaction of lithium chloride and bis(fluorosulfonyl)imide is 45°C.
[0084] The test results of this comparative example are as follows: lithium bis(fluorosulfonyl)imide content is 28.70%, free acid (calculated as HF) is 98ppm, moisture (Karl Fischer method) is 139ppm, alkali metal ion content (calculated as K) is 43ppm, chloride ion content is 191ppm, heavy metal ion content (calculated as Fe) is 12ppm, and insoluble matter content is 142ppm.
[0085] The test results of the above embodiments and comparative examples are summarized in Table 1 for easy comparison.
[0086] Table 1
[0087]
[0088] It can be seen from Table 1 that:
[0089] Compared with Example 3, since Comparative Example 1 only lowered the temperature of the metathesis reaction to 0°C, the free acid and chloride ion contents increased;
[0090] Compared with Example 3, since Comparative Example 2 only raises the temperature of the metathesis reaction to 40° C., the free acid and chloride ion contents are reduced;
[0091] Compared with Example 3, since Comparative Example 3 only lowers the temperature of the metathesis reaction to -5°C, the LiFSI content in the reaction solution is reduced, and the free acid, water and chloride ion contents are all increased;
[0092] Compared with Example 3, since Comparative Example 4 only raises the temperature of the metathesis reaction to 45° C., the LiFSI content in the reaction solution is reduced, and the contents of free acid, water, chloride ions and alkali metal ions are all increased.
[0093] The present invention illustrates the detailed structural features of the present invention through the above embodiments, but the present invention is not limited to the above detailed structural features, that is, it does not mean that the present invention must rely on the above detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
[0094] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0095] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0096] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A method for preparing a lithium bis(fluorosulfonyl)imide solution, characterized in that: The preparation method comprises the following steps: (1) Lithium chloride suspended in a non-aqueous solvent is subjected to a double decomposition reaction with bis(fluorosulfonyl)imide to obtain a reaction system; (2) The reaction system of step (1) is sequentially degassed and concentrated, resin deacidified, and filtered to obtain a lithium bis(fluorosulfonyl)imide solution.
2. The preparation method according to claim 1, characterized in that: In step (1), the molar ratio of lithium chloride to bis(fluorosulfonyl)imide is (0.8-1.2):
1.
3. The preparation method according to claim 1, characterized in that: In step (1), the purity of lithium chloride and bis(fluorosulfonyl)imide is greater than 99.5 wt %, and the water content is less than 50 ppm.
4. The preparation method according to claim 1, characterized in that: In step (1), the water content of the non-aqueous solvent is less than 15 ppm, and the non-aqueous solvent includes at least one of dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethyl acetate, acetone, diethyl ether, dimethylformamide, ethylene glycol dimethyl ether, acetonitrile or tetrahydrofuran.
5. The preparation method according to claim 1, characterized in that: In step (1), the reaction temperature of the metathesis reaction is 0 to 40° C.; Preferably, in step (1), the reaction time of the metathesis reaction is 2 to 6 hours.
6. The preparation method according to claim 1, characterized in that: In step (1), the metathesis reaction is carried out under an inert gas atmosphere; Preferably, the inert gas is at least one of nitrogen, argon or helium.
7. The preparation method according to claim 1, characterized in that: In step (2), the degassing and concentration is degassing under reduced pressure, and the pressure range is 0.05 to 10 kPa; Preferably, in step (2), the temperature of the degassing and concentration is 20 to 80°C; Preferably, in step (2), the degassing and concentration time is 4 to 8 hours.
8. The preparation method according to claim 1, characterized in that: In step (2), the operating temperature of the resin deacidification is 20 to 60° C.; Preferably, in step (2), the matrix structure of the ion exchange resin used for resin deacidification is any one of styrene divinyl benzene copolymer, styrene resin or acrylic (ester) resin, and the functional groups are -N(CH3)2, -N + (CH3)3, -N + Any one of (C2H4OH)(CH3)2; Preferably, in step (2), the adsorption time of the resin deacidification is 1 to 5 hours.
9. A lithium bis(fluorosulfonyl)imide solution, characterized in that: The lithium bis(fluorosulfonyl)imide solution is prepared by the preparation method according to any one of claims 1 to 8, wherein the chloride ion content of the lithium bis(fluorosulfonyl)imide solution is below 5 ppm, and the acidity of the free acid is below 50 ppm.
10. An application of a lithium bis(fluorosulfonyl)imide solution, characterized in that: Using lithium bis(fluorosulfonyl)imide solution in lithium batteries; Wherein, the lithium bis(fluorosulfonyl imide) solution is prepared by the preparation method according to any one of claims 1 to 8, or the lithium bis(fluorosulfonyl imide) solution is the lithium bis(fluorosulfonyl imide) solution according to claim 9.
Citation Information
Patent Citations
Method for preparing bi-(sulfonyl fluoride) imine and (fluorinated alkyl sulfonyl fluorine sulfonyl) imine alkali metal salt
CN101747242A
Imidodisulfuryl fluoride lithium salt preparation method
CN107055493A
Preparation method of lithium bis (fluorosulfonyl) imide
CN116143086A
Lithium bis (fluorosulfonyl) imide composition and preparation method thereof
CN116495711A
Clean and waste-free method for preparing lithium bis (fluorosulfonyl) imide
CN116654882A