Lithium fluorosulfonyl difluorophosphoramide as well as preparation method and application of lithium fluorosulfonyl difluorophosphoramide

By reacting lithium fluorophosphate and [(fluorosulfonyl)imino]methone in a non-aqueous solvent, combining resin deacidification and degassing and concentration technology, high-purity lithium fluorosulfonyl difluorophosphimide was prepared, and the solution The problems of complex preparation process, low efficiency and high cost in the prior art are achieved, and the production of high yield and low impurities of lithium fluorosulphonyl difluorophosphimide is ensured, ensuring the performance of lithium-ion batteries.

CN119079944APending Publication Date: 2024-12-06HANGZHOU WANLIDA NEW ENERGY TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311180497.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-09-13
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing preparation process of lithium fluorosulfonyldifluorophosphimide is complicated, has low efficiency and high cost, making it difficult to meet the demand for high purity and low impurities of lithium-ion batteries.

Method used

Lithium fluorosulfonyl difluorophosphate is prepared by reacting with [(fluorosulfonyl)imino]methoketone in a non-aqueous solvent through simple process steps and gentle reaction conditions, and is prepared by resin Deacidification and degassing concentration technology improves product purity.

Benefits of technology

Achieve high yield (90.8-91.2%) and low impurity content of lithium fluorosulfonyl difluorophosphimide, reducing production costs, simplifying process steps, suitable for industrial production, and effectively ensuring the working performance of lithium-ion batteries .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004447144430000111
    Figure BDA0004447144430000111
  • Figure BDA0004447144430000141
    Figure BDA0004447144430000141
Patent Text Reader

Abstract

The invention provides lithium fluorosulfonyl difluorophosphoramide as well as a preparation method and application thereof, and belongs to the technical field of electrolyte. The preparation method comprises the following steps: mixing fluorine-containing lithium phosphate, [(fluorosulfonyl) imino] ketone and a non-aqueous solvent, and reacting to obtain the fluorosulfonyl difluorophosphoramide lithium. The preparation method provided by the invention is simple in process, convenient to operate and high in feasibility, reaction raw materials are cheap and easy to obtain, reaction conditions are mild, byproducts are few, and the cost can be greatly saved. The lithium fluorosulfonyl difluorophosphoramide prepared on the basis of the method is high in yield and can reach 90.8-91.2%, the impurity content is low, and the working performance of a battery can be effectively ensured when the lithium fluorosulfonyl difluorophosphoramide is used for a lithium ion battery electrolyte.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electrolytes, and in particular relates to lithium fluorosulfonyl difluorophosphoryl imide and a preparation method and application thereof. Background Art

[0002] Lithium-ion battery is a secondary battery (rechargeable battery) that mainly relies on the movement of lithium ions between the positive electrode and the negative electrode to work. Lithium fluorosulfonyl difluorophosphoryl imide can be used as an important electrolyte salt of non-aqueous electrolytes such as lithium-ion batteries. It is required to have a very high purity (usually not less than 99.5%), and the impurities such as water, alkali metals, heavy metals, chloride ions, sulfates, and free acids must be strictly controlled, otherwise it will lead to an increase in the internal resistance of the battery, a rapid decay of the battery capacity, a short cycle life, and even affect the safety of the battery. Therefore, obtaining a lithium fluorosulfonyl difluorophosphoryl imide product with high purity and low content of harmful impurities, used as an electrolyte material in lithium-ion batteries, has a high application value.

[0003] In the prior art, there is little research on lithium fluorosulfonyl difluorophosphoryl imide. For example, CN109705156A discloses a method for preparing lithium fluorosulfonyl difluorophosphoryl imide. Specifically, aminosulfonyl chloride and PCl are firstly reacted to obtain a fluorosulfonyl difluorophosphoryl imide. 5 As the starting material, the intermediate chlorosulfonyl trichlorophosphazene is prepared; secondly, the chlorosulfonyl trichlorophosphazene is reacted with hexamethyldisiloxane to prepare chlorosulfonyl trimethylsilyloxy dichlorophosphazene; then, the chlorosulfonyl trimethylsilyloxy dichlorophosphazene is reacted with triethylammonium trihydrofluoride to prepare fluorosulfonyl difluorophosphoramidite; finally, fluorosulfonyl difluorophosphoramidite is reacted with lithium carbonate to prepare lithium fluorosulfonyl difluorophosphoramidite. Although this method can prepare lithium fluorosulfonyl difluorophosphoramidite, the method has complicated procedures, low efficiency, poor feasibility and high cost.

[0004] Therefore, how to simplify the preparation process steps of lithium fluorosulfonyl difluorophosphoryl imide, improve efficiency, reduce costs and increase feasibility is the current research focus. Summary of the invention

[0005] In view of the deficiencies of the prior art, the object of the present invention is to provide a lithium fluorosulfonyl difluorophosphoryl imide and a preparation method and application thereof. The preparation method proposed by the present invention has simple process, convenient operation, high feasibility, and cheap and readily available reaction raw materials, mild reaction conditions, few by-products, and can greatly save costs. The lithium fluorosulfonyl difluorophosphoryl imide prepared by this method has a high yield of up to 90.8-91.2%, and a low impurity content, which can effectively ensure the working performance of the battery when used in lithium ion battery electrolyte.

[0006] To achieve this object, the present invention adopts the following technical solutions:

[0007] In a first aspect, the present invention provides a method for preparing lithium fluorosulfonyl difluorophosphoryl imide, the preparation method comprising:

[0008] The fluorine-containing lithium phosphate, [(fluorosulfonyl)imino]methanone and a non-aqueous solvent are mixed and reacted to obtain the lithium fluorosulfonyl difluorophosphoryl imide.

[0009] The preparation method proposed by the invention has simple process, convenient operation, high feasibility, and the reaction raw materials are cheap and easy to obtain, the reaction conditions are mild, the byproducts can be recycled, and the cost can be greatly saved. The lithium fluorosulfonyl difluorophosphoryl imide prepared by this method has a high yield of up to 90.8-91.2%, and has a low impurity content. When used in lithium ion battery electrolyte, it can effectively ensure the working performance of the battery.

[0010] In the present invention, the lithium fluorosulfonyl difluorophosphoryl imide prepared by this method can be directly used for the preparation of lithium ion battery electrolyte, and the method has cheap and readily available reaction raw materials, simple operation, few by-products, and is suitable for industrial production.

[0011] As a preferred technical solution of the present invention, the fluorine-containing lithium phosphate includes lithium difluorophosphate.

[0012] It should be noted that the reaction equation for the above reaction can be:

[0013] LiPO 2 F 2 +FSO 2 NCO→Li + (FSO 2 NPOF 2 ) - +CO 2 .

[0014] Preferably, the purity of the fluorine-containing lithium phosphate is greater than 99.5%, for example, it may be 99.6%, 99.7%, 99.8% or 99.9%.

[0015] Preferably, the water content of the fluorine-containing lithium phosphate is ≤50 ppm, for example, it may be 50 ppm, 40 ppm, 30 ppm or 20 ppm.

[0016] Preferably, the molar ratio of the fluorinated lithium phosphate to [(fluorosulfonyl)imino]methanone is (1-1.1):1, for example, 1:1, 1.02:1, 1.04:1, 1.06:1, 1.08:1 or 1.1:1.

[0017] In the present invention, if the molar ratio of fluorinated lithium phosphate to [(fluorosulfonyl)imino]methanone is too small, the [(fluorosulfonyl)imino]methanone remaining after the reaction needs to be removed, increasing the subsequent processing cost; if the molar ratio of fluorinated lithium phosphate to [(fluorosulfonyl)imino]methanone is too large, the time for processing the residual fluorinated lithium phosphate and the waste of raw materials will be increased.

[0018] As a preferred technical solution of the present invention, the non-aqueous solvent includes any one of dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethyl acetate, dimethylformamide, ethylene glycol dimethyl ether, acetonitrile or tetrahydrofuran, or a combination of at least two thereof.

[0019] Preferably, the water content of the non-aqueous solvent is less than 15 ppm, for example, it may be 10 ppm, 8 ppm, 5 ppm or 2 ppm.

[0020] As a preferred technical solution of the present invention, the mixing process is accompanied by stirring.

[0021] Preferably, the reaction temperature is 40-80°C, for example, 40°C, 50°C, 60°C, 70°C, 80°C, etc., preferably 50-70°C.

[0022] In the present invention, if the reaction temperature is too low, the reaction time will be prolonged, the time cost will be increased, and the yield will be low; if the reaction temperature is too high, coloration will occur, side reactions will occur, and the yield will be reduced.

[0023] Preferably, the reaction time is 6-10 h, for example, 6 h, 7 h, 8 h, 9 h or 10 h.

[0024] Preferably, the reaction is carried out in an inert atmosphere, and the gas in the inert atmosphere includes any one of nitrogen, argon or helium, or a combination of at least two of them.

[0025] As a preferred technical solution of the present invention, after the reaction is completed, the lithium fluorosulfonyl difluorophosphoryl imide is further subjected to a post-treatment step, and the post-treatment step specifically includes: resin deacidification of the lithium fluorosulfonyl difluorophosphoryl imide, and degassing and concentrating to obtain a lithium fluorosulfonyl difluorophosphoryl imide concentrated solution.

[0026] In the present invention, the resin used in the resin deacidification is a resin containing a basic group. The purpose of resin deacidification of lithium fluorosulfonyl difluorophosphoryl imide is to remove acidic impurities in the lithium hexafluorophosphate concentrate and improve product properties.

[0027] In the present invention, degassing and concentrating refers to a method of removing the acidic gas in the reaction solution by decompressing the gas phase containing the volatile components volatilized from the solution or by passing a carrier gas such as nitrogen gas, dry air, so that the gas phase is discharged outside the system. The present invention is concentrated by degassing, and the concentration of the solution is improved, and acidic impurities are discharged, thereby a highly purified liquid lithium fluorine sulfonyl difluoride phosphoryl imide concentrate can be manufactured. It should be noted that, when a carrier gas is passed, it can only be passed into the gas phase, but it is more effective when it is also passed into the liquid by bubbling, etc.

[0028] In the present invention, a highly purified concentrate can be obtained by degassing and concentrating without using a purifying agent, and a complicated device is not required, and production can be performed using a single reaction tank, thereby achieving a cost reduction effect.

[0029] As a preferred technical solution of the present invention, the pressure during degassing and concentration is 0.5-10KPa, for example, it can be 0.5KPa, 1KPa, 2KPa, 3KPa, 4KPa, 5KPa, 6KPa, 7KPa, 8KPa, 9KPa or 10KPa, etc., preferably 0.5-5KPa.

[0030] In the present invention, within this pressure range, the carbon dioxide gas present in the reaction solution can be effectively removed. If the pressure is too high, the carbon dioxide impurity cannot be removed to a desired concentration, or it takes a longer time to remove the impurity to a concentration below the desired concentration, which is not conducive to cost reduction.

[0031] Preferably, the temperature during degassing and concentration is 20-80°C, for example, it can be 20°C, 30°C, 40°C, 50°C, 60°C, 70°C or 80°C, etc., preferably 30-60°C.

[0032] In the present invention, if the temperature during degassing and concentration is too low, the non-aqueous solvent may solidify, making it difficult to remove acidic impurities, resulting in reduced product purity; if the temperature during degassing and concentration is too high, the obtained concentrated solution may be colored, or lithium fluorosulfonyl difluorophosphoryl imide may decompose, resulting in a reduced yield.

[0033] Preferably, the degassing and concentration time is 4-8 hours, for example, it can be 4 hours, 5 hours, 6 hours, 7 hours or 8 hours.

[0034] Preferably, the atmosphere during the degassing and concentration is an inert atmosphere, and the gas in the inert atmosphere includes any one of nitrogen, argon or helium, or a combination of at least two of them.

[0035] As a preferred technical solution of the present invention, the preparation method comprises the following steps:

[0036] (1) mixing lithium difluorophosphate and [(fluorosulfonyl)imino]methanone in a non-aqueous solvent, and reacting them in an inert atmosphere at 40-80° C. for 6-10 hours to obtain a reaction product;

[0037] wherein the molar ratio of lithium difluorophosphate to [(fluorosulfonyl)imino]ketone is (1-1.1):1;

[0038] (2) filtering the reaction product and performing resin deacidification, and then degassing and concentrating under reduced pressure to obtain a lithium fluorosulfonyl difluorophosphoryl imide concentrated solution;

[0039] The pressure during the reduced pressure degassing and concentration is 0.5-10KPa, the temperature is 20-80°C, and the time is 4-8h.

[0040] In a second aspect, the present invention provides lithium fluorosulfonyl difluoro phosphoramidite, which is prepared by the preparation method of lithium fluorosulfonyl difluoro phosphoramidite as described in the first aspect.

[0041] Preferably, the purity of the lithium fluorosulfonyl difluorophosphoryl imide is 99.1-99.3%, for example, 99.1%, 99.2% or 99.3%.

[0042] As a preferred technical solution of the present invention, the mass concentration of acidic impurities in the lithium fluorosulfonyl difluorophosphoryl imide is ≤80ppm, for example, it can be 70ppm, 60ppm, 50ppm, 40ppm or 30ppm, etc., preferably ≤50ppm.

[0043] In the present invention, the content of anions such as chloride ions and sulfate ions in the prepared lithium fluorosulfonyl difluorophosphoryl imide is below 1 ppm, and the concentration of free acid is below 50 ppm, so it can be directly used for the preparation of lithium ion battery electrolyte.

[0044] It should be noted that the acidic impurities include hydrogen fluoride or fluorosulfonic acid.

[0045] In a third aspect, the present invention provides a use of the lithium fluorosulfonyl difluorophosphoryl imide as described in the second aspect in a lithium ion battery electrolyte.

[0046] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0047] Compared with the prior art, the present invention has the following beneficial effects:

[0048] (1) The preparation method provided by the present invention has mild reaction conditions and a high yield of the obtained product, which is as high as 90.8-91.2%. The reaction raw materials are cheap and readily available, which can greatly save costs. In addition, there are few by-products, which can be recycled.

[0049] (2) The preparation method provided by the present invention has simple reaction steps, easy operation, and simple post-reaction treatment, which increases the feasibility of industrial production.

[0050] (3) The lithium fluorosulfonyl difluorophosphoryl imide prepared by the present invention can be used to prepare the electrolyte in lithium ion batteries, which can effectively ensure the working performance of the battery. DETAILED DESCRIPTION

[0051] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0052] Example 1

[0053] This embodiment provides a method for preparing lithium fluorosulfonyl difluorophosphoryl imide, the preparation method comprising the following steps:

[0054] (1) In a 500 mL three-necked flask, under nitrogen protection, add 200 mL of dimethyl carbonate and 118.7 g (1.1 mol) of lithium difluorophosphate, slowly raise the temperature while stirring, slowly dropwise add 125.08 g (1 mol) of [(fluorosulfonyl)imino]ketone at 60° C., and complete the dropwise addition over 2 hours. After the addition is completed, keep the temperature for 6 hours to react;

[0055] Wherein, the molar ratio of lithium difluorophosphate to [(fluorosulfonyl)imino]ketone is 1.1:1;

[0056] (2) The obtained reaction product is filtered and the resin is deacidified. Then, at a temperature of 60° C., the vacuum pump is slowly turned on to slowly evacuate the bottle to a pressure of 5 KPa, and degassing and concentrating is performed for 8 hours. The degassed and concentrated solution is then precisely filtered and the concentration is adjusted with dimethyl carbonate to obtain a lithium fluorosulfonyl difluorophosphorylimide concentrated solution with a weight concentration of 30%.

[0057] The obtained lithium fluorosulfonyl difluorophosphoryl imide concentrate was tested for content, and the test results were as follows: the yield of lithium fluorosulfonyl difluorophosphoryl imide was 90.8%, the purity was 99.1%, the content of lithium fluorosulfonyl difluorophosphoryl imide in the concentrate was 30.53%, the free acid (calculated as HF acid) was 18 ppm, the water content (Karl Fischer method) was 29 ppm, the alkali metal ion content (calculated as K) was 1 ppm, the chloride ion content was 1 ppm, the heavy metal ion content (calculated as Fe) was 1 ppm, and the insoluble matter content was 80 ppm.

[0058] Example 2

[0059] This embodiment provides a method for preparing lithium fluorosulfonyl difluorophosphoryl imide, the preparation method comprising the following steps:

[0060] (1) In a 2000 mL three-necked flask, under nitrogen protection, 1000 mL of ethyl methyl carbonate and 437.04 g (4.05 mol) of lithium difluorophosphate were added, the temperature was slowly raised with stirring, and 500.32 g (4 mol) of [(fluorosulfonyl)imino]ketone was slowly added dropwise at 80° C. The addition was completed over 3 hours, and the temperature was kept for 5 hours to react;

[0061] Wherein, the molar ratio of lithium difluorophosphate to [(fluorosulfonyl)imino]ketone is 1.01:1;

[0062] (2) The obtained reaction product is filtered and the resin is deacidified. Then, at a temperature of 80° C., the vacuum pump is slowly turned on to slowly evacuate the bottle to a pressure of 2 KPa, and degassing and concentrating is performed for 4 hours. The degassed and concentrated solution is then precisely filtered and the concentration is adjusted with ethyl methyl carbonate to obtain a lithium fluorosulfonyl difluorophosphorylimide concentrated solution with a weight concentration of 30%.

[0063] The obtained lithium fluorosulfonyl difluorophosphoryl imide concentrate was tested for content, and the test results were as follows: the yield of lithium fluorosulfonyl difluorophosphoryl imide was 91.0%, the purity was 99.2%, the content of lithium fluorosulfonyl difluorophosphoryl imide in the concentrate was 30.08%, the free acid (calculated as HF acid) was 60 ppm, the water content (Karl Fischer method) was 35 ppm, the alkali metal ion content (calculated as K) was 1 ppm, the chloride ion content was 1 ppm, the heavy metal ion content (calculated as Fe) was 1 ppm, and the insoluble matter content was 102 ppm.

[0064] Example 3

[0065] This embodiment provides a method for preparing lithium fluorosulfonyl difluorophosphoryl imide, the preparation method comprising the following steps:

[0066] (1) In a 500 mL three-necked flask, under nitrogen protection, add 200 mL of ethyl acetate and 56.11 g (0.52 mol) of lithium difluorophosphate, slowly raise the temperature while stirring, slowly add 62.54 g (0.5 mol) of [(fluorosulfonyl)imino]methanone dropwise at 60° C., and complete the addition over 2 hours. After the addition is completed, keep the temperature for 4 hours to react;

[0067] Wherein, the molar ratio of lithium difluorophosphate to [(fluorosulfonyl)imino]ketone is 1.04:1;

[0068] (2) The obtained reaction product is filtered and the resin is deacidified. Then, at a temperature of 60° C., the vacuum pump is slowly turned on to slowly evacuate the bottle to a pressure of 10 KPa, and degassing and concentrating is performed for 6 hours. The degassed and concentrated solution is then precisely filtered and the concentration is adjusted with ethyl acetate to obtain a lithium fluorosulfonyl difluorophosphoryl imide concentrated solution with a weight concentration of 30%.

[0069] The obtained lithium fluorosulfonyl difluorophosphoryl imide concentrate was tested for content, and the test results were as follows: the yield of lithium fluorosulfonyl difluorophosphoryl imide was 90.9%, the purity was 99.2%, the content of lithium fluorosulfonyl difluorophosphoryl imide in the concentrate was 30.12%, the free acid (calculated as HF acid) was 16 ppm, the water content (Karl Fischer method) was 25 ppm, the alkali metal ion content (calculated as K) was 1 ppm, the chloride ion content was 1 ppm, the heavy metal ion content (calculated as Fe) was 1 ppm, and the insoluble matter content was 86 ppm.

[0070] Example 4

[0071] This embodiment provides a method for preparing lithium fluorosulfonyl difluorophosphoryl imide, the preparation method comprising the following steps:

[0072] (1) In a 500 mL three-necked flask, under argon protection, add 200 mL of tetrahydrofuran and 107.9 g (1 mol) of lithium difluorophosphate, slowly raise the temperature while stirring, slowly dropwise add 125.08 g (1 mol) of [(fluorosulfonyl)imino]methanone at 40° C., and complete the dropwise addition over 2 hours. After the completion of the dropwise addition, keep the temperature for 10 hours to react;

[0073] wherein the molar ratio of lithium difluorophosphate to [(fluorosulfonyl)imino]ketone is 1:1;

[0074] (2) The obtained reaction product is filtered and the resin is deacidified. Then, at a temperature of 40° C., the vacuum pump is slowly turned on to slowly evacuate the bottle to a pressure of 5 KPa, and degassing and concentrating is performed for 6 hours. The degassed and concentrated solution is then precisely filtered and the concentration is adjusted with tetrahydrofuran to obtain a lithium fluorosulfonyl difluorophosphoryl imide concentrated solution with a weight concentration of 30%.

[0075] The obtained lithium fluorosulfonyl difluorophosphoryl imide concentrate was tested for content, and the test results were as follows: the yield of lithium fluorosulfonyl difluorophosphoryl imide was 91.2%, the purity was 99.1%, the content of lithium fluorosulfonyl difluorophosphoryl imide in the concentrate was 29.7%, the free acid (calculated as HF acid) was 37 ppm, the water content (Karl Fischer method) was 20 ppm, the alkali metal ion content (calculated as K) was 1 ppm, the chloride ion content was 1 ppm, the heavy metal ion content (calculated as Fe) was 1 ppm, and the insoluble matter content was 69 ppm.

[0076] Example 5

[0077] The difference between this embodiment and embodiment 1 is that in step (1), the molar ratio of lithium difluorophosphate to [(fluorosulfonyl)imino]methanone is 0.8:1.

[0078] The rest of the preparation methods and parameters were the same as those in Example 1.

[0079] Example 6

[0080] The difference between this embodiment and embodiment 1 is that in step (1), the molar ratio of lithium difluorophosphate to [(fluorosulfonyl)imino]methanone is 1.5:1.

[0081] The rest of the preparation methods and parameters were the same as those in Example 1.

[0082] Example 7

[0083] The difference between this embodiment and embodiment 1 is that the reaction temperature in step (1) is 25°C.

[0084] The rest of the preparation methods and parameters were the same as those in Example 1.

[0085] Example 8

[0086] The difference between this embodiment and embodiment 1 is that the reaction temperature in step (1) is 90°C.

[0087] The rest of the preparation methods and parameters were the same as those in Example 1.

[0088] Example 9

[0089] The difference between this embodiment and embodiment 1 is that the temperature during degassing and concentration in step (2) is 10°C.

[0090] The rest of the preparation methods and parameters were the same as those in Example 1.

[0091] Example 10

[0092] The difference between this embodiment and embodiment 1 is that the temperature during degassing and concentration in step (2) is 90°C.

[0093] The rest of the preparation methods and parameters were the same as those in Example 1.

[0094] Comparative Example 1

[0095] This comparative example provides a lithium difluorophosphate.

[0096] Performance Testing

[0097] (I) The lithium fluorosulfonyl difluorophosphoryl imide concentrated solution prepared in Examples 1-10 was tested to detect the contents of different components in the concentrated solution.

[0098] Test method: Use gas chromatography, moisture meter, acid-base titrator, and turbidity method to determine the purity of the concentrate, as well as the impurities, moisture, acidity, and chloride ion content of each component.

[0099] The test results are shown in Table 1.

[0100] Table 1

[0101]

[0102] (ii) A lithium ion battery was prepared based on the lithium fluorosulfonyl difluorophosphoryl imide concentrate provided in Examples 1-10 and the lithium difluorophosphate provided in Comparative Example 1, the specific steps comprising:

[0103] Ⅰ: Production of positive plate:

[0104] The mass ratio of LiNi is 100:1:0.9. 0.85 Co 0.12 Al 0.03 O 2 , acetylene black as a conductive agent, and polyvinylidene fluoride as a binder are mixed, the mixture is put into N-methyl-2-pyrrolidone as a dispersion medium, and kneaded to form a positive electrode slurry, the positive electrode slurry is applied to both sides of a positive electrode collector formed of aluminum foil, and dried to form a positive electrode material layer, the positive electrode material layer is compressed in a manner to achieve a specified thickness, and the compressed electrode plate is cut into a specified size, and finally, a positive electrode connector is joined to an exposed portion of the positive electrode collector where no positive electrode material layer is formed, thereby making a positive electrode plate.

[0105] Ⅱ: Production of negative plate:

[0106] A negative electrode active material graphite, a binder styrene, and a thickener carboxymethyl cellulose are mixed in a mass ratio of 96:2:2, and the mixture is put into water as a dispersion medium and kneaded to form a negative electrode slurry. The negative electrode slurry is applied to both sides of a negative electrode collector formed of copper foil, and dried to form a negative electrode material layer. The negative electrode material layer is compressed in a manner to achieve a specified thickness, and the compressed electrode plate is cut into a specified size. Finally, a negative electrode connector is joined to an exposed portion of the negative electrode collector where the negative electrode material layer is not formed, thereby making a negative electrode plate.

[0107] III: Preparation of electrode body:

[0108] The positive electrode plate and the negative electrode plate were wound with a separator formed of a microporous film made of polyethylene interposed therebetween to produce an electrode body, and the end of the separator at the winding end of the electrode body was fixed with an adhesive tape.

[0109] IV: Preparation of non-aqueous electrolyte:

[0110] Ethylene carbonate, ethyl methyl carbonate and dimethyl carbonate are mixed in a volume ratio of 4:3:3 (1 atmosphere, 25°C) to prepare a non-aqueous solvent, lithium hexafluorophosphate as an electrolyte salt is dissolved in the non-aqueous solvent at a concentration of 14.6 weight%, and 2 weight% of vinylene carbonate and 0.7 weight% of the lithium fluorosulfonyl difluorophosphorylimide concentrate provided by Examples 1-10 or the lithium difluorophosphate provided by Comparative Example 1 are added as additives to prepare a non-aqueous electrolyte.

[0111] V: Preparation of sealing body:

[0112] The terminal plate, valve core, annular insulating plate and terminal plate are stacked to form a sealing body, wherein the valve core and terminal plate are formed of aluminum plate, a plurality of vent holes are arranged on the terminal plate, and the valve core, insulating plate and terminal plate constitute a current blocking mechanism.

[0113] VI: Preparation of lithium-ion batteries:

[0114] An upper insulating plate and a lower insulating plate are respectively arranged at the upper and lower parts of the electrode body, the electrode body is inserted into an outer can, the negative electrode terminal is connected to the bottom of the outer can, the positive electrode terminal is connected to the sealing body, and after the non-aqueous electrolyte is injected into the interior of the outer can, the sealing body is embedded and fixed to the opening of the outer can with the help of a gasket, thereby obtaining a cylindrical non-aqueous electrolyte secondary battery.

[0115] Five lithium-ion batteries prepared in each embodiment and comparative example were manufactured under the same conditions, and then cycle performance tests and rate performance tests were performed, and the average value of the test results was taken.

[0116] Cycle performance test: Charge at a constant current of 1C, set the upper and lower limits of the charging voltage to 4.3V and 3V respectively, and measure the change in battery capacity at a temperature of 25°C.

[0117] Rate performance test: Charge at a constant current of 5C, set the upper and lower limits of the charging voltage to 4.35V and 3V respectively, and measure the change in battery capacity at a temperature of 25°C.

[0118] The test results are shown in Table 2.

[0119] Table 2

[0120]

[0121] analyze:

[0122] It can be seen from Table 1 and Table 2 that the preparation method provided by the present invention has high yield, few by-products, and high purity of lithium fluorosulfonyl difluorophosphoryl imide, which can be directly used in the preparation of electrolyte in lithium ion batteries, and can effectively ensure the working performance of the battery, thereby obtaining excellent cycle performance and rate performance.

[0123] From the data results of Example 1 and Example 5-6, it can be seen that if the molar ratio of lithium difluorophosphate to [(fluorosulfonyl)imino]ketone is too small, the [(fluorosulfonyl)imino]ketone remaining after the reaction needs to be removed, increasing the subsequent processing cost; if the molar ratio of lithium difluorophosphate to [(fluorosulfonyl)imino]ketone is too large, it will increase the time for processing the residual lithium difluorophosphate and the waste of raw materials. The lithium fluorosulfonyl difluorophosphoryl imide obtained when the molar ratio of lithium difluorophosphate to [(fluorosulfonyl)imino]ketone is too small or too large can improve the cycle performance and rate performance of the battery.

[0124] From the data results of Example 1 and Example 7-8, it can be seen that if the reaction temperature is too low, the reaction speed is slow, the reaction time is greatly increased, and the yield is reduced; if the reaction temperature is too high, coloring will occur, side reactions will occur, and the yield will be reduced. The lithium fluorosulfonyl difluorophosphoryl imide obtained when the reaction temperature is too low or too high can improve the cycle performance and rate performance of the battery, but the improvement is not large.

[0125] From the data results of Examples 1 and 9-10, it can be seen that if the temperature during degassing and concentration is too low, the non-aqueous solvent will solidify, making it difficult to remove acidic impurities, resulting in a decrease in product purity; if the temperature during degassing and concentration is too high, the resulting concentrated solution will be colored, and lithium fluorosulfonyl difluorophosphoryl imide may decompose, resulting in a decrease in yield. The lithium fluorosulfonyl difluorophosphoryl imide obtained when the temperature during degassing and concentration is too low or too high can improve the cycle performance and rate performance of the battery.

[0126] It can be seen from the data results of Example 1 and Comparative Example 1 that if conventional lithium difluorophosphate is used as an additive in the preparation process of the non-aqueous electrolyte, the cycle performance and rate performance of the battery are poor.

[0127] The present invention can improve the cycle performance and rate characteristics of lithium ion batteries by adding lithium fluoride sulfonyl difluorophosphoryl imide to the original electrolyte. In addition, the present invention can provide a non-aqueous electrolyte secondary battery that takes into account both battery characteristics at high temperature and high voltage requirements and safety during overcharging, so it has great applicability in electric vehicles and energy storage applications.

[0128] The applicant declares that the present invention illustrates the technical solution of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing lithium fluorosulfonyl difluorophosphoryl imide, characterized in that: The preparation method comprises: The fluorine-containing lithium phosphate, [(fluorosulfonyl)imino]methanone and a non-aqueous solvent are mixed and reacted to obtain the lithium fluorosulfonyl difluorophosphoryl imide.

2. The preparation method according to claim 1, characterized in that: The fluorine-containing lithium phosphate includes lithium difluorophosphate; The molar ratio of the fluorine-containing lithium phosphate to [(fluorosulfonyl)imino]ketone is (1-1.1):

1.

3. The preparation method according to claim 1, characterized in that: The non-aqueous solvent includes any one of dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethyl acetate, dimethylformamide, ethylene glycol dimethyl ether, acetonitrile or tetrahydrofuran, or a combination of at least two thereof; The water content of the non-aqueous solvent is less than 15 ppm.

4. The preparation method according to claim 1, characterized in that: The mixing process is accompanied by stirring; The reaction temperature is 40-80°C; The reaction time is 6-10h; The reaction is carried out in an inert atmosphere, wherein the gas in the inert atmosphere comprises any one of nitrogen, argon or helium, or a combination of at least two of them.

5. The preparation method according to claim 1, characterized in that: The lithium fluorosulfonyl difluorophosphoryl imide is further subjected to a post-treatment step, which specifically includes: resin deacidification of the lithium fluorosulfonyl difluorophosphoryl imide, and then degassing and concentrating to obtain a lithium fluorosulfonyl difluorophosphoryl imide concentrated solution.

6. The preparation method according to claim 5, characterized in that: The pressure during degassing and concentration is 0.5-10KPa; The temperature during degassing and concentration is 20-80°C; The degassing and concentration time is 4-8h.

7. The preparation method according to any one of claims 1 to 6, characterized in that: The preparation method comprises the following steps: (1) mixing lithium difluorophosphate and [(fluorosulfonyl)imino]methanone in a non-aqueous solvent with stirring, and reacting in an inert atmosphere at 40-80° C. for 6-10 hours to obtain a reaction product; wherein the molar ratio of lithium difluorophosphate to [(fluorosulfonyl)imino]ketone is (1-1.1):1; (2) filtering the reaction product and performing resin deacidification, and then degassing and concentrating under reduced pressure to obtain a lithium fluorosulfonyl difluorophosphoryl imide concentrated solution; The pressure during the reduced pressure degassing and concentration is 0.5-10KPa, the temperature is 20-80°C, and the time is 4-8h.

8. A lithium fluorosulfonyl difluorophosphoryl imide, characterized in that: The lithium fluorosulfonyl difluorophosphoryl imide is prepared by the preparation method of lithium fluorosulfonyl difluorophosphoryl imide according to any one of claims 1 to 7; The purity of the lithium fluorosulfonyl difluorophosphoryl imide is 99.1-99.3%.

9. The lithium fluorosulfonyl difluorophosphoryl imide according to claim 8, characterized in that: The mass concentration of acidic impurities in the lithium fluorosulfonyl difluorophosphoryl imide is ≤80ppm.

10. Use of the lithium fluorosulfonyl difluorophosphoryl imide as claimed in claim 8 or 9 in a lithium ion battery electrolyte.

Citation Information

Patent Citations

  • Preparation method of lithium fluorosulfonyl bis(fluorophosphoryl)imide, product thereof and application

    CN109422252A

  • Liquid electrolyte for non-aqueous electrolyte cell, and non-aqueous electrolyte cell in which said liquid electrolyte for non-aqueous electrolyte cell is used

    WO2019111958A1