Method for recovering battery-grade iron phosphate from sludge

By leaching acid liquid and synthesising hydrothermal synthesis of the sludge incineration ash, battery-grade iron phosphate is directly obtained, solving the problem of long process flow in the existing technology, and achieving process simplification and product performance improvement.

CN119079955AActive Publication Date: 2024-12-06HUAZHONG UNIV OF SCI & TECH

Patent Information

Application Number
CN202411205130.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

In the prior art, the process flow for recovering battery-grade iron phosphate from sludge is relatively long and needs to be simplified and shortened.

Method used

By incinerating the dried sludge, the sludge incineration ash is obtained, and the target acid liquid at a preset concentration is leaching to obtain a phosphorus-containing leaching solution. Then, the Fe source is added for hydrothermal synthesis, and the battery-grade iron phosphate is directly obtained. Simplified process flow.

Benefits of technology

The process flow for preparing battery-grade iron phosphate is shortened, the purity and electrochemical performance of iron phosphate is improved, and the processing cost and complexity is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119079955A_ABST
    Figure CN119079955A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of sludge resource utilization, in particular to a method for recycling battery-grade iron phosphate from sludge. The method comprises the following steps: incinerating dried sludge to obtain sludge incineration ash, leaching the sludge incineration ash by using a target acid solution with a first preset concentration, carrying out solid-liquid separation to obtain a phosphorus-containing leachate, adding a Fe source into the phosphorus-containing leachate to obtain a mixed solution, and carrying out hydrothermal synthesis on the mixed solution to obtain the phosphorus-containing iron-based composite material. The battery-grade iron phosphate is obtained. Therefore, according to the technical scheme, the phosphorus-containing leachate added with the Fe source is directly subjected to hydrothermal synthesis treatment, so that the technological process for preparing the battery-grade iron phosphate can be shortened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sludge resource utilization, and in particular to a method for recovering battery-grade iron phosphate from sludge. Background Art

[0002] Pollutants and nutrients in sewage are aggregated by the proliferation of bacteria and chemical agents, eventually forming sludge. With the rapid development of new energy vehicles, energy storage batteries and other industries, the output of battery-grade iron phosphate is also rising, resulting in an increase in the demand for its production raw materials (such as phosphorus).

[0003] In the related art, the method for recovering phosphorus from sludge and preparing battery-grade iron phosphate mainly adopts wet chemical method, but the process flow of this method is relatively long.

[0004] Therefore, there is an urgent need for a method for recovering battery-grade iron phosphate from sludge to solve this technical problem. Summary of the invention

[0005] The invention provides a method for recovering battery-grade iron phosphate from sludge, which can shorten the process flow of preparing battery-grade iron phosphate.

[0006] The present invention provides a method for recovering battery-grade iron phosphate from sludge, comprising:

[0007] Incinerating the dried sludge to obtain sludge incineration ash;

[0008] Leaching the sludge incineration ash with a target acid solution of a first preset concentration, and obtaining a phosphorus-containing leachate after solid-liquid separation;

[0009] adding an Fe source to the phosphorus-containing leaching solution to obtain a mixed solution;

[0010] The mixed solution is subjected to hydrothermal synthesis to obtain battery-grade iron phosphate.

[0011] As can be seen from the above scheme, the present invention provides a method for recovering battery-grade iron phosphate from sludge, by incinerating the dried sludge to obtain sludge incineration ash, then leaching the sludge incineration ash with a target acid solution of a first preset concentration, and obtaining a phosphorus-containing leaching solution after solid-liquid separation, and then adding an Fe source to the phosphorus-containing leaching solution to obtain a mixed solution, and hydrothermally synthesizing the mixed solution to obtain battery-grade iron phosphate. Therefore, the above technical scheme is a hydrothermal synthesis treatment directly performed on the phosphorus-containing leaching solution to which the Fe source is added, so that the process flow for preparing battery-grade iron phosphate can be shortened. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0013] Figure 1 A schematic diagram of a method for recovering battery-grade iron phosphate from sludge provided in an embodiment of the present invention;

[0014] Figure 2 A comparison chart of the iron phosphate recovered by the method provided in the embodiment of the present invention and commercial-grade iron phosphate;

[0015] Figure 3 A thermodynamic equilibrium calculation system diagram of the precipitation reaction between impurity components in the phosphorus-containing leachate and the target phosphorus-containing product provided in an embodiment of the present invention;

[0016] Figure 4 A Gibbs free energy change diagram of the iron phosphate precipitation reaction provided in an embodiment of the present invention;

[0017] Figure 5 A reaction equilibrium constant diagram for the iron phosphate precipitation reaction provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0018] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0019] See also Figure 1 One embodiment of the present invention provides a method for recovering battery-grade iron phosphate from sludge, the method comprising:

[0020] Step 100, incinerating the dried sludge to obtain sludge incineration ash;

[0021] Step 102: leaching the sludge incineration ash with a target acid solution of a first preset concentration, and obtaining a phosphorus-containing leaching solution after solid-liquid separation;

[0022] Step 104, adding an Fe source to the phosphorus-containing leaching solution to obtain a mixed solution;

[0023] Step 106: Perform hydrothermal synthesis on the mixed solution to obtain battery-grade iron phosphate.

[0024] In this embodiment, the dried sludge is incinerated to obtain sludge incineration ash, and then the sludge incineration ash is leached with a target acid solution of a first preset concentration, and a phosphorus-containing leaching solution is obtained after solid-liquid separation, and then an Fe source is added to the phosphorus-containing leaching solution to obtain a mixed solution, and the mixed solution is hydrothermally synthesized to obtain battery-grade iron phosphate. Therefore, the above technical solution is a hydrothermal synthesis treatment directly performed on the phosphorus-containing leaching solution to which the Fe source is added, so that the process flow of preparing battery-grade iron phosphate can be shortened.

[0025] In some embodiments, the incineration temperature is 750-900° C. to ensure the incineration effect of the dried sludge.

[0026] In one embodiment of the present invention, the target acid solution includes at least one of sulfuric acid and nitric acid.

[0027] In this embodiment, the target acid solution can be used to better leach phosphorus in the sludge incineration ash, and can also inhibit the co-precipitation of synchronously leached metal impurities during the hydrothermal synthesis process, ensuring that only phosphorus and iron are precipitated.

[0028] In the related art, when leaching phosphorus, Fe, Ca, Mg, Al and other elements in the sludge will be leached synchronously with the P element. In order to avoid the formation of impurities, it is often necessary to remove them by adjusting the pH pre-precipitation method, cation exchange resin method, etc., and then adjust the pH to the optimal precipitation range of the target product to obtain the highest possible yield. This method often requires 6-8 subdivision steps to achieve leachate purification and pH adjustment, which greatly increases the complexity of the entire phosphorus recovery process. However, the target acid solution with the first preset concentration in this embodiment can recover phosphorus under the conditions of low extract concentration, without pH adjustment and filtrate purification, effectively simplifying the treatment process and reducing the treatment cost.

[0029] Thermodynamic calculations show that iron phosphate has an independent precipitation range under the concentration conditions of the strong target acid solution with a pH of 0.4 to 2.1. Figure 3 (The width of each substance bar represents the extent of its precipitation reaction under the corresponding pH conditions), that is, other phosphorus-containing products (such as AlPO 4 MgNH 4 PO 4 , Ca 5 (PO 4 ) 3 OH) and solid impurities (such as Fe(OH) 3 、Al(OH) 3 Mg(OH) 2 , Ca(OH) 2) In this range, no precipitation reaction can occur. Therefore, it is only necessary to control the first preset concentration of the target acid solution, that is, at least one of sulfuric acid and nitric acid, to ensure that the pH of the phosphorus-containing leachate is within this range to achieve the separate precipitation of iron phosphate, thereby also ensuring the purity of the iron phosphate.

[0030] In one embodiment of the present invention, the first preset concentration is 0.02-0.15 mol / L, which can ensure the leaching effect of the target acid solution of the first preset concentration on the phosphorus element.

[0031] In some embodiments, the solid-liquid ratio of sludge incineration ash to the target acid solution of the first preset concentration can be 1:50 to 1:200, the leaching time can be 2 to 4 hours, and the flipping oscillation rate can be 60 to 120 rpm to ensure the leaching effect of the target acid solution of the first preset concentration on the phosphorus element in the sludge incineration ash.

[0032] In some embodiments, the phosphorus-containing leachate may be filtered using a 0.45 μm filter head to remove solid particles that have not been separated.

[0033] In one embodiment of the present invention, the phosphorus-containing leaching solution is used for cyclic leaching of new sludge incineration ash.

[0034] In this embodiment, the phosphorus-containing leachate is recycled to the cyclic leaching of phosphorus in the sludge incineration ash, thereby reducing the reagent consumption.

[0035] In one embodiment of the present invention, the Fe source includes FeCl 3 、Fe(NO 3 ) 3 and Fe 2 (SO 4 ) 3 At least one of .

[0036] In this embodiment, the Fe source is an inorganic compound, which can make the mixed solution have a strong crystallization tendency and is conducive to the formation of crystals.

[0037] In one embodiment of the present invention, the molar ratio of the Fe source to the phosphorus element in the phosphorus-containing leaching solution is 1 to 1.05:1.

[0038] In one embodiment of the present invention, the reaction temperature of the hydrothermal synthesis is 150-210° C., and the reaction time is 1-24 h.

[0039] In one embodiment of the present invention, step 106 may specifically include:

[0040] Performing hydrothermal synthesis on the mixed solution to obtain a hydrothermal synthesis product;

[0041] Performing solid-liquid separation on the hydrothermal synthesis product to obtain a solid product;

[0042] Washing the solid product with a washing liquid, and freeze-drying the washed solid product;

[0043] The freeze-dried solid product is calcined under air atmosphere to obtain battery-grade iron phosphate.

[0044] In this embodiment, under the heating conditions of the target acid solution, the precipitation reaction of related impurities and other phosphorus-containing products except iron phosphate can be further suppressed. It should be noted that the precipitation reaction of iron phosphate is a reversible reaction at low temperature. In the reversible reaction, the equilibrium constant lgK<5, which will lead to a decrease in the yield of iron phosphate and a slow synthesis rate. The hydrothermal method can effectively increase the reaction equilibrium constant lgK at high temperature, making the synthesis reaction more thorough and faster. Figure 4 (When △G < 0, the reaction is considered to be spontaneous) and Figure 5 (When lgK>5, the precipitation reaction is considered to be more complete).

[0045] In addition, the hydrothermally produced iron phosphate presents a uniform micron-sized spherical structure, which has better electrochemical performance than the amorphous structure obtained by room temperature precipitation. At the same time, iron phosphate does not directly nucleate and grow in a liquid environment, but grows closely attached to the wall surface. This feature enables it to achieve a good thin layer deposition effect during the reaction process, which is also conducive to the improvement of its electrochemical performance.

[0046] In this embodiment, the iron phosphate is microscopically regular spherical, with a sphericity of >0.9 and an average particle size of <1 μm, and the Fe, P, and O elements are uniformly distributed (e.g. Figure 2 ) so that iron phosphate has better electrochemical properties and ion conduction effect.

[0047] exist Figure 2 In the figure, a and b are respectively the macroscopic morphology comparisons of the iron phosphate prepared by the method and the commercial grade iron phosphate, c and d are respectively the microscopic morphology comparisons of the iron phosphate prepared by the method and the commercial grade iron phosphate, e and f are respectively the crystal structure comparisons of the iron phosphate prepared by the method and the commercial grade iron phosphate. Figure 2 It can be seen that the iron phosphate prepared in the embodiment of the present invention has greatly improved uniformity.

[0048] In the embodiment of the present invention, the iron phosphate can meet the standard of HG / T4701-2021 iron phosphate for batteries, and the data are shown in Table 1 (showing the content of battery grade iron phosphate, analytical grade reagent grade and recovered product of this method).

[0049] Table 1 Comparison of ferric phosphate and standard limits

[0050]

[0051] In this embodiment, vacuum filtration is used to separate the hydrothermal synthesis product into solid and liquid, so that the hydrothermal synthesis product can be better separated into solid and liquid.

[0052] In some embodiments, the calcination temperature may be 500-800° C., so that the freeze-dried solid product can be fully calcined to remove crystal water from the solid product, thereby obtaining battery-grade iron phosphate.

[0053] In one embodiment of the present invention, the washing liquid includes a first washing liquid and a second washing liquid, the first washing liquid is dilute nitric acid or dilute sulfuric acid of a second preset concentration, and the second washing liquid is deionized water.

[0054] In this embodiment, the washing step in the hydrothermal process is mainly to remove the impurity ions carried by the residual water in the solid product. Experiments show that when the Al( element in the sludge is too high (for example, Al salt conditioner is added to the sludge during the front-end treatment process), the hydrothermal synthesis process may still produce Al element doping. At this time, washing with dilute nitric acid or dilute phosphoric acid can remove the impurity without causing the loss of iron phosphate. Here, the PO in iron phosphate is used. 4 3- Than NO 3 - It has strong coordination ability and is insoluble in dilute nitric acid.

[0055] In some embodiments, the second preset concentration is 1%, which can ensure the washing effect of the second preset concentration of dilute nitric acid or dilute sulfuric acid on the solid product.

[0056] In one embodiment of the present invention, washing the solid product with a washing liquid includes: washing the solid product with a first washing liquid and a second washing liquid in sequence.

[0057] In some embodiments, if the sludge is Al salt conditioned sludge, the solid product can be washed twice with 1% dilute nitric acid or 1% dilute phosphoric acid during the hydrothermal synthesis process, and then washed with deionized water. It should be noted that the washing liquid can be reused, thereby reducing the cost of the reagent.

[0058] In one embodiment of the present invention, after freeze-drying the washed solid product, the method further comprises:

[0059] adding a reducing agent and a Li source to the freeze-dried solid product;

[0060] The solid product to which a reducing agent and a Li source are added is heated under an inert atmosphere to obtain battery-grade lithium iron phosphate.

[0061] In this embodiment, the recovered product is battery-grade iron phosphate with high sphericity. After further thermochemical Li addition, high-purity lithium iron phosphate can be obtained, realizing resource utilization from sludge to high-value phosphorus-containing products.

[0062] In some embodiments, the solid product to which the reducing agent and the Li source are added is heated continuously at 600-800° C. for 10 h in an inert atmosphere to obtain battery-grade lithium iron phosphate.

[0063] In one embodiment of the present invention, the reducing agent comprises H 2 and at least one of a carbon source, the carbon source comprising at least one of glucose, sucrose, starch and carbon black, and the Li source comprising LiOH and Li 2 CO 3 At least one of .

[0064] In one embodiment of the present invention, when the reducing agent is H 2 When the reducing agent is used, the gas volume ratio of the inert gas in the solid product is 5%:95%.

[0065] In one embodiment of the present invention, when the reducing agent is a carbon source, the dosage of the reducing agent is 0.5-10% of the total mass of the solid product after freeze-drying.

[0066] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for recovering battery-grade iron phosphate from sludge, characterized in that: include: Incinerating the dried sludge to obtain sludge incineration ash; Leaching the sludge incineration ash with a target acid solution of a first preset concentration, and obtaining a phosphorus-containing leachate after solid-liquid separation; adding an Fe source to the phosphorus-containing leaching solution to obtain a mixed solution; The mixed solution is subjected to hydrothermal synthesis to obtain battery-grade iron phosphate.

2. The method according to claim 1, characterized in that The target acid solution includes at least one of sulfuric acid and nitric acid, and the first preset concentration is 0.02-0.15 mol / L.

3. The method according to claim 1, characterized in that The phosphorus-containing leaching solution is used for cyclic leaching of new sludge incineration ash.

4. The method according to claim 1, characterized in that: The Fe source includes at least one of FeCl3, Fe(NO3)3 and Fe2(SO4)3, and the molar ratio of the Fe source to the phosphorus element in the phosphorus-containing leaching solution is 1 to 1.05:

1.

5. The method according to claim 1, characterized in that The reaction temperature of the hydrothermal synthesis is 150-210° C., and the reaction time is 1-24 hours.

6. The method according to any one of claims 1 to 5, characterized in that The step of subjecting the mixed solution to hydrothermal synthesis to obtain battery-grade iron phosphate comprises: Performing hydrothermal synthesis on the mixed solution to obtain a hydrothermal synthesis product; Performing solid-liquid separation on the hydrothermal synthesis product to obtain a solid product; Washing the solid product with a washing liquid, and freeze-drying the washed solid product; The freeze-dried solid product is calcined under air atmosphere to obtain battery-grade iron phosphate.

7. The method according to claim 6, characterized in that The washing liquid comprises a first washing liquid and a second washing liquid, the first washing liquid is dilute nitric acid or dilute sulfuric acid of a second preset concentration, and the second washing liquid is deionized water; The step of washing the solid product with a washing liquid comprises: The solid product is washed sequentially with the first washing liquid and the second washing liquid.

8. The method according to claim 7, characterized in that After freeze-drying the washed solid product, the method further comprises: adding a reducing agent and a Li source to the freeze-dried solid product; The solid product to which a reducing agent and a Li source are added is heated under an inert atmosphere to obtain battery-grade lithium iron phosphate.

9. The method according to claim 8, characterized in that The reducing agent includes at least one of H2 and a carbon source, the carbon source includes at least one of glucose, sucrose, starch and carbon black, and the Li source includes at least one of LiOH and Li2CO3.

10. The method according to claim 9, characterized in that When the reducing agent is H2, the gas volume ratio of the reducing agent to the inert gas in the solid product is 5%:95%; and / or, When the reducing agent is a carbon source, the dosage of the reducing agent is 0.5-10% of the total mass of the solid product after freeze-drying; and / or, The molar ratio of the Fe source to the Li source in the solid product is 1:1.05.

Citation Information

Patent Citations

  • Method for preparing iron phosphate from municipal sludge incineration ash and battery-grade iron phosphate

    CN113401887A

  • Method and system for efficiently and selectively recovering iron phosphate product from sludge leachate

    CN116143094A

Cited By

  • Method for synergistically and efficiently recovering phosphorus from sludge incineration ash and waste masks

    CN121063985A