Preparation method of food additive calcium hydroxide

The described method enhances calcium hydroxide production by digesting kiln-burned quicklime with water and ethanol, then drying, to achieve high purity and safety for food additives, addressing particle size and surfactant-related issues.

CN119080406APending Publication Date: 2024-12-06HUZHOU ZHEBAO METALLURGY AUX MATERIALS +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411297886.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing methods for producing calcium hydroxide with high specific surface area face issues such as particle size limitations, impurity contamination, and the use of surfactants that can introduce organic matter, posing safety concerns for food additive applications.

Method used

A method involving the digestion of kiln-burned quicklime with deionized water, followed by ethanol treatment and vacuum drying, without using surfactants, to produce calcium hydroxide with improved purity and safety for food use, while recycling ethanol.

Benefits of technology

The method produces calcium hydroxide with enhanced specific surface area and purity, ensuring food safety by eliminating organic impurities and optimizing raw material utilization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119080406A_ABST
    Figure CN119080406A_ABST
Patent Text Reader

Abstract

The embodiment of the invention provides a preparation method of food additive calcium hydroxide, and relates to the technical field of food additives. The preparation method of the food additive calcium hydroxide comprises the following steps: obtaining a heat preservation container, and selecting kiln calcined lime as a raw material; the method comprises the following steps: putting selected kiln calcined quicklime into a heat-insulating container, adding deionized water, and sealing the heat-insulating container for digestion reaction; after the digestion reaction is finished, spraying ethanol to a digestion product; and drying the digestion product in a vacuum oven. Calcium hydroxide is produced from commercially available kiln-fired calcium oxide, and the raw materials are cheap and easy to obtain; no surfactant is used in the production process, no organic matter is attached to the surface of the prepared calcium hydroxide, the purity of the calcium hydroxide is improved, and the calcium hydroxide can be safely used as a food additive; after gas escaping from the vacuum drying oven is condensed and collected, ethanol is recovered through rectification for cyclic utilization, the ethanol utilization rate is high and is fully utilized, the raw material utilization rate is increased, and the cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of food additives, and in particular, to a method for preparing calcium hydroxide, a food additive. Background Art

[0002] At present, calcium hydroxide, commonly known as slaked lime, has a wide range of uses due to its properties. For example, calcium hydroxide is alkaline and easily reacts with acidic gases such as sulfur oxides and nitrogen oxides. It is a cheap and efficient desulfurizer and denitrifier. Calcium hydroxide can decompose and release water when heated. As a filler for polymer materials, it can improve the flame retardant properties of composite materials. Calcium hydroxide can also be used as a food additive to act as an acidity regulator and increase the calcium content of food. Calcium hydroxide with a high specific surface area can better exert these properties. The most common method for preparing calcium hydroxide is to digest calcium oxide with water. In order to produce calcium hydroxide with a high specific surface area, two methods are used. One is to grind the raw calcium oxide finely. The smaller the calcium oxide particle size, the more conducive it is to quickly complete the digestion reaction, thereby avoiding the growth of calcium hydroxide grains [Huadian Technology, 2010, 32(5):74. Paper Science and Technology, 2016, 35(3):82.]; the other is to use a mixed solution of surfactant and water to carry out the digestion reaction and improve the dispersion of calcium hydroxide particles. Liu Yue et al. [Inorganic Salt Industry, 2023, 55(10):42.] selected 1-5 mm calcium oxide and water added with polyethylene glycol 400 for digestion reaction. Through three digestion methods, a specific surface area of ​​52.62 m was obtained. 2 / g of calcium hydroxide. Hao Zhifei et al. [Inorganic Salt Industry, 2015, 47(12):19.] made calcium oxide into 1-5 mm particles and digested them with aqueous solutions of propylene glycol, triethanolamine or polyethylene glycol. The specific surface area of ​​the obtained calcium hydroxide can reach 47.4 m 2 / g. Some preparation methods are to first modify calcium oxide and then perform a digestion reaction. For example, calcium oxide with a particle size of about 1 mm is first mixed with isopropanol and then added with water for digestion [Inorganic Salt Industry, 2008, 40(9):32.], and the patent [CN 202311807768.5] is to first mix and modify calcium oxide obtained by roasting calcium carbonate with a size of 15 to 1500 mesh (about 0.01 to 1.2 mm) with a digestion promoter and a dispersant, and then add water for digestion reaction; The above-mentioned prior art solutions have the following defects: the particle size of calcium oxide is too small during the grinding process, and it will mix with impurities such as coal slag and calcium carbonate left over from the calcined limestone, making it difficult to separate, thereby reducing the purity of calcium hydroxide [Refractory and Lime, 2015, 40(4):15.]; the surfactant used is adsorbed on the surface of calcium hydroxide to prevent grain growth and particle agglomeration. The results of infrared spectroscopy analysis confirmed that isopropyl alcohol [Inorganic Salt Industry, 2008, 40(9):32.] and polyethylene glycol [Inorganic Salt Industry, 2023, 55(10):42.] are attached to the surface of calcium hydroxide. The surfactant attached to the surface of calcium hydroxide is not conducive to the use of calcium hydroxide in food, because the organic matter such as the surfactant brought in may constitute a food safety problem. Summary of the invention

[0003] The present application aims to solve at least one of the technical problems existing in the prior art. According to the preparation method of the food additive calcium hydroxide of the embodiment of the present application, the steps are as follows: S1. Obtain an insulation container and select kiln-burned quicklime as raw material; S2, the selected kiln-burned quicklime is placed in an insulated container, after adding deionized water, the insulated container is sealed for digestion reaction, wherein the water / calcium oxide mass ratio is 0.35-1.0, the temperature of the digestion water is 10-80° C., and the digestion reaction time is 30-80 minutes; S3. After the digestion reaction is completed, open the heat preservation container and spray ethanol on the digestion product, wherein the mass ratio of ethanol to calcium oxide is 0.04 to 0.6, and the contact time between ethanol and digestion product is 5 to 80 minutes; S4, then putting the digestion product into a vacuum oven for drying, the vacuum oven has an operating temperature of 90 to 140° C., and the digestion product is dried in the vacuum oven for 1 to 10 hours; S5. Take out the digestion product dried in the vacuum oven and grind it into powder to obtain calcium hydroxide, a food additive.

[0004] According to the preparation method of the food additive calcium hydroxide of the embodiment of the present application, commercially available kiln-fired calcium oxide is used to produce calcium hydroxide, and the raw materials are cheap and easily available; no surfactant is used in the production process, and there is no organic matter attached to the surface of the prepared calcium hydroxide, thereby improving the purity of the calcium hydroxide and making it safe to be used as a food additive; the gas escaping from the vacuum oven is condensed and collected, and then distilled to recover ethanol for recycling, so the utilization rate of ethanol is high and fully utilized, thereby improving the utilization rate of raw materials and reducing costs.

[0005] In addition, the preparation method of the food additive calcium hydroxide according to the embodiment of the present application also has the following additional technical features: In a preferred embodiment of the present invention, the temperature of the digestion water is 20-70°C.

[0006] In a preferred embodiment of the present invention, the water / calcium oxide mass ratio is 0.4 to 0.7.

[0007] In a preferred embodiment of the present invention, the digestion reaction time is 35 to 70 minutes.

[0008] In a preferred embodiment of the present invention, the mass ratio of ethanol to calcium oxide is 0.05 to 0.5.

[0009] In a preferred embodiment of the present invention, the contact time between the ethanol and the digestion product is 10 to 60 minutes.

[0010] In a preferred embodiment of the present invention, the operating temperature of the vacuum oven is 100-130°C.

[0011] In a preferred embodiment of the present invention, the digestion product is dried in the vacuum oven for 2 to 8 hours.

[0012] In a preferred embodiment of the present invention, the gas escaping from the vacuum oven is condensed and collected, and then distilled and recovered to obtain ethanol for recycling.

[0013] In a preferred embodiment of the present invention, the kiln-burned quicklime is calcium oxide, wherein the kiln-burned quicklime is screened according to the physical and chemical indicators of the national food safety standards and used in step S2; in step S4, a grinder is used to grind the digestion product.

[0014] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] In order to more clearly illustrate the technical solutions of the implementation methods of the present application, the drawings required for use in the implementation methods will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0016] Figure 1 is the X-ray diffraction analysis result of the example sample provided in the embodiment of the present application; Figure 2 X-ray diffraction analysis results of comparative example samples provided in the embodiments of the present application; Figure 3 A flowchart of the method steps provided for an implementation of the present application. DETAILED DESCRIPTION

[0017] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0018] The technical solutions in the embodiments of the present application will be described below in conjunction with the drawings in the embodiments of the present application.

[0019] Example 1 like Figure 1-Figure 3 As shown, according to the preparation method of the food additive calcium hydroxide of the embodiment of the present application, commercially available kiln-burned quicklime (calcium oxide) is selected as a raw material according to the physical and chemical indicators of the national food safety standard (food additive-calcium oxide, GB 30614-2014), calcium oxide and 25°C deionized water are weighed according to the water / calcium oxide mass ratio = 0.4, and are put into an insulated container in turn, and the insulated container is sealed for digestion reaction for 40 minutes; ethanol is weighed according to the ethanol / calcium oxide mass ratio = 0.05, and is evenly sprayed on the digestion product. After 20 minutes, the digestion product is placed in a 120°C vacuum oven and dried for 2 hours; after cooling, the digestion product is ground into powder for standby use.

[0020] The powdered samples were subjected to N adsorption using a Micromeritics ASAP 2010 physical adsorption instrument. 2 The specific surface area of ​​the sample was calculated by low-temperature adsorption using the BET equation. The crystal form of the powdered sample was analyzed using an X'Pert PRO X-ray powder diffractometer from PANalytical.

[0021] Example 2 According to the physical and chemical indicators of the national food safety standard (food additive - calcium oxide, GB 30614-2014), commercially available kiln-burned quicklime (calcium oxide) was selected as the raw material. Calcium oxide and 65°C deionized water were weighed according to the water / calcium oxide mass ratio = 0.4, and put into an insulated container in turn. The insulated container was sealed for digestion reaction for 60 minutes; ethanol was weighed according to the ethanol / calcium oxide mass ratio = 0.05, and sprayed evenly on the digestion product. After 10 minutes, the digestion product was placed in a 110°C vacuum oven and dried for 3 hours; after cooling, the digestion product was ground into powder for later use.

[0022] The specific surface area and crystal form analysis methods of the powdered sample are the same as those in Example 1.

[0023] Example 3 According to the physical and chemical indicators of the national food safety standard (food additives - calcium oxide, GB 30614-2014), commercially available kiln-fired quicklime (calcium oxide) was selected as the raw material. Calcium oxide and 70°C deionized water were weighed according to the water / calcium oxide mass ratio of 0.5, and put into an insulated container in turn. The insulated container was sealed for digestion reaction for 65 minutes; ethanol was weighed according to the ethanol / calcium oxide mass ratio of 0.12, and sprayed evenly on the digestion product. After 10 minutes, the digestion product was placed in a 120°C vacuum oven and dried for 3 hours; after cooling, the digestion product was ground into powder for later use.

[0024] The specific surface area and crystal form analysis methods of the powdered sample are the same as those in Example 1.

[0025] Example 4 According to the physical and chemical indicators of the national food safety standard (food additive - calcium oxide, GB 30614-2014), commercially available kiln-burned quicklime (calcium oxide) was selected as the raw material. Calcium oxide and 50°C deionized water were weighed according to the water / calcium oxide mass ratio = 0.5, and put into an insulated container in turn. The insulated container was sealed for digestion reaction for 35 minutes; ethanol was weighed according to the ethanol / calcium oxide mass ratio = 0.44, and sprayed evenly on the digestion product. After 60 minutes, the digestion product was placed in a 130°C vacuum oven and dried for 2 hours; after cooling, the digestion product was ground into powder for later use.

[0026] The specific surface area and crystal form analysis methods of the powdered sample are the same as those in Example 1.

[0027] Example 5 According to the physical and chemical indicators of the national food safety standard (food additive - calcium oxide, GB 30614-2014), commercially available kiln-fired quicklime (calcium oxide) was selected as the raw material. Calcium oxide and 30°C deionized water were weighed according to the water / calcium oxide mass ratio = 0.6, and put into an insulated container in turn. The insulated container was sealed for digestion reaction for 45 minutes; ethanol was weighed according to the ethanol / calcium oxide mass ratio = 0.21, and sprayed evenly on the digestion product. After 30 minutes, the digestion product was placed in a 120°C vacuum oven and dried for 5 hours; after cooling, the digestion product was ground into powder for later use.

[0028] The specific surface area and crystal form analysis methods of the powdered sample are the same as those in Example 1.

[0029] Example 6 According to the physical and chemical indicators of the national food safety standard (food additives - calcium oxide, GB 30614-2014), commercially available kiln-fired quicklime (calcium oxide) was selected as the raw material. Calcium oxide and 55°C deionized water were weighed according to the water / calcium oxide mass ratio of 0.6, and put into an insulated container in turn. The insulated container was sealed for digestion reaction for 50 minutes; ethanol was weighed according to the ethanol / calcium oxide mass ratio of 0.1, and sprayed evenly on the digestion product. After 20 minutes, the digestion product was placed in a 120°C vacuum oven and dried for 5 hours; after cooling, the digestion product was ground into powder for later use.

[0030] The specific surface area and crystal form analysis methods of the powdered sample are the same as those in Example 1.

[0031] Example 7 According to the physical and chemical indicators of the national food safety standard (food additive - calcium oxide, GB 30614-2014), commercially available kiln-burned quicklime (calcium oxide) was selected as the raw material. Calcium oxide and 25°C deionized water were weighed according to the water / calcium oxide mass ratio = 0.7, and put into an insulated container in turn. The insulated container was sealed for digestion reaction for 40 minutes; ethanol was weighed according to the ethanol / calcium oxide mass ratio = 0.15, and sprayed evenly on the digestion product. After 50 minutes, the digestion product was placed in a 130°C vacuum oven and dried for 6 hours; after cooling, the digestion product was ground into powder for later use.

[0032] The specific surface area and crystal form analysis methods of the powdered sample are the same as those in Example 1.

[0033] Example 8 According to the physical and chemical indicators of the national food safety standard (food additive - calcium oxide, GB 30614-2014), commercially available kiln-burned quicklime (calcium oxide) was selected as the raw material. Calcium oxide and 40°C deionized water were weighed according to the water / calcium oxide mass ratio of 0.7, and put into an insulated container in turn. The insulated container was sealed for digestion reaction for 50 minutes; ethanol was weighed according to the ethanol / calcium oxide mass ratio of 0.35, and sprayed evenly on the digestion product. After 30 minutes, the digestion product was placed in a 110°C vacuum oven and dried for 7 hours; after cooling, the digestion product was ground into powder for later use.

[0034] The specific surface area and crystal form analysis methods of the powdered sample are the same as those in Example 1.

[0035] Specifically, in order to further determine the effect of variables on the specific surface area and crystal form analysis of powdered samples, the following operations were performed: Comparative Example 1 (compared with Example 1, the operation of uniformly spraying the digestion product with ethanol was omitted to examine the effect of not using ethanol on the digestion product): calcium oxide and 25°C deionized water were weighed separately at a water / calcium oxide mass ratio of 0.4, and placed in an insulated container in turn, and the insulated container was sealed for digestion reaction for 40 minutes; then the digestion product was placed in a 120°C vacuum oven and dried for 2 hours; after cooling, the digestion product was ground into powder for later use.

[0036] The specific surface area and crystal form analysis methods of the powdered sample are the same as those in Example 1.

[0037] Comparative Example 2 (compared with Example 1, deionized water and ethanol are mixed and then used in the digestion reaction to examine the effect of the order of ethanol use on the digestion product): calcium oxide, 25°C deionized water and ethanol are weighed respectively according to the water / calcium oxide mass ratio = 0.4 and the ethanol / calcium oxide mass ratio = 0.05. After the deionized water and ethanol are evenly mixed, the calcium oxide and ethanol aqueous solution are put into an insulated container in turn, and the insulated container is sealed for digestion reaction for 40 minutes; the digestion product is then placed in a 120°C vacuum oven and dried for 2 hours; after cooling, the digestion product is ground into powder for later use.

[0038] The specific surface area and crystal form analysis methods of the powdered sample are the same as those in Example 1.

[0039] Comparative Example 3 (compared with Example 3, deionized water and ethanol are mixed for digestion reaction to examine the effect of the order of ethanol use on the digestion product): calcium oxide, 70°C deionized water and ethanol are weighed respectively according to the water / calcium oxide mass ratio = 0.5 and the ethanol / calcium oxide mass ratio = 0.12. After the deionized water and ethanol are evenly mixed, the calcium oxide and ethanol aqueous solution are put into an insulated container in turn, and the insulated container is sealed for digestion reaction for 65 minutes; the digestion product is then placed in a 120°C vacuum oven and dried for 3 hours; after cooling, the digestion product is ground into powder for later use.

[0040] The specific surface area and crystal form analysis methods of the powdered sample are the same as those in Example 1.

[0041] Comparative Example 4 (compared with Example 5, deionized water and ethanol are mixed for digestion reaction to examine the effect of the order of ethanol use on the digestion product): calcium oxide, 30°C deionized water and ethanol are weighed respectively according to the water / calcium oxide mass ratio = 0.6 and the ethanol / calcium oxide mass ratio = 0.21. After the deionized water and ethanol are evenly mixed, the calcium oxide and ethanol aqueous solution are put into an insulated container in turn, and the insulated container is sealed for digestion reaction for 45 minutes; the digestion product is then placed in a 120°C vacuum oven and dried for 5 hours; after cooling, the digestion product is ground into powder for later use.

[0042] The specific surface area and crystal form analysis methods of the powdered sample are the same as those in Example 1.

[0043] Comparative Example 5 (Compared with Example 7, the operation of uniformly spraying the digestion product with ethanol was omitted to examine the effect of not using ethanol on the digestion product): calcium oxide and 25°C deionized water were weighed separately at a water / calcium oxide mass ratio of 0.7, and placed in an insulated container in turn, and the insulated container was sealed for digestion reaction for 40 minutes; the digestion product was then placed in a 130°C vacuum oven and dried for 6 hours; after cooling, the digestion product was ground into powder for later use.

[0044] The specific surface area and crystal form analysis methods of the powdered sample are the same as those in Example 1.

[0045] In summary, the specific surface areas of the example samples and the comparative examples are summarized as shown in Table 1. The specific surface areas of the example samples are all larger than those of the corresponding comparative examples. The comparison results of Example 1 and Comparative Example 1, and Example 7 and Comparative Example 5 show that in the process of preparing calcium hydroxide, the use of ethanol can increase the specific surface area of ​​the calcium hydroxide sample; the comparison results of Example 1 and Comparative Example 2, Example 3 and Comparative Example 3, and Example 5 and Comparative Example 4 show that the order of ethanol use is a key factor, and it should be used after the calcium oxide is digested.

[0046] Table 1 Specific surface area of ​​samples of examples and comparative examples sample Specific surface area (m2 / g) Example 1 14.8 Example 2 16.0 Example 3 16.2 Example 4 15.8 Example 5 15.3 Example 6 15.4 Example 7 15.7 Example 8 15.5 Comparative Example 1 8.6 Comparative Example 2 9.1 Comparative Example 3 9.2 Comparative Example 4 10.2 Comparative Example 5 8.7 The crystal form analysis results of the samples in the examples are shown in Figure 1 The crystal form analysis results of the comparative samples are shown in Figure 2 The diffraction peak positions of all samples are the same as those of the calcium hydroxide standard sample (PDF 04-0733), indicating that all samples are high-purity calcium hydroxide crystals.

[0047] According to the physical and chemical indicators of the national food safety standards, commercially available kiln-burned quicklime is selected as the raw material, and after being digested with water, ethanol is sprayed on it, and then placed in a vacuum oven to dry, and ground into powder to obtain the food additive calcium hydroxide. At the same time, the gas escaping from the vacuum oven is condensed and collected, and then the ethanol is recovered by distillation for recycling. Because no surfactant is used in the production process, the obtained calcium hydroxide is free of impurities and can be safely used as a food additive.

[0048] Calcium hydroxide is produced using commercially available kiln-fired calcium oxide, and the raw materials are cheap and easily available; no surfactant is used in the production process, and the surface of the produced calcium hydroxide has no organic matter attached, so it can be safely used as a food additive; the gas escaping from the vacuum oven is condensed and collected, and then distilled to recover ethanol for recycling, with a high ethanol utilization rate.

[0049] Table 2 Comparison results of the examples and comparative examples Water / calcium oxide mass ratio Digestion water temperature / ℃ Digestion reaction time / min Ethanol / calcium oxide mass ratio Contact time / min Vacuum oven working temperature / ℃ Drying time / min Specific surface area (m2 / g) Example 1 0.4 25 40 0.05 20 120 120 14.8 Example 2 0.4 65 60 0.05 10 110 180 16.0 Example 3 0.5 70 65 0.12 10 120 180 16.2 Example 4 0.5 50 35 0.44 60 130 120 15.8 Example 5 0.6 30 45 0.21 30 120 300 15.3 Example 6 0.6 55 50 0.1 20 120 300 15.4 Example 7 0.7 25 40 0.15 50 130 360 15.7 Example 8 0.7 40 50 0.35 30 110 420 15.5 Comparative Example 1 0.4 25 40 - - 120 120 8.6 Comparative Example 2 0.4 25 40 0.05 - 120 120 9.1 Comparative Example 3 0.5 70 65 0.12 - 120 180 9.2 Comparative Example 4 0.6 30 45 0.21 - 120 300 10.2 Comparative Example 5 0.7 25 40 - - 130 360 8.7 Other structures and operations of the heat-insulating container and the vacuum oven according to the embodiments of the present application are known to those skilled in the art and will not be described in detail here.

[0050] It should be noted that the specific models and specifications of the heat preservation container, vacuum oven and grinder need to be selected and determined according to the actual specifications of the device, and the specific selection calculation method adopts the existing technology in this field, so it will not be described in detail.

[0051] The power supply and principles of the heat preservation container, vacuum oven and grinder are clear to those skilled in the art and will not be described in detail herein.

[0052] The above description is only an embodiment of the present application and is not intended to limit the scope of protection of the present application. For those skilled in the art, the present application may have various changes and variations. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application should be included in the scope of protection of the present application. It should be noted that similar reference numerals and letters represent similar items in the following drawings, so once an item is defined in one drawing, it does not need to be further defined and explained in the subsequent drawings.

Claims

1. A method for preparing a food additive calcium hydroxide, characterized in that: The steps include: S1. Obtain an insulation container and select kiln-burned quicklime as raw material; S2, the selected kiln-burned quicklime is placed in an insulated container, after adding deionized water, the insulated container is sealed for digestion reaction, wherein the water / calcium oxide mass ratio is 0.35-1.0, the temperature of the digestion water is 10-80° C., and the digestion reaction time is 30-80 minutes; S3. After the digestion reaction is completed, open the heat preservation container and spray ethanol on the digestion product, wherein the mass ratio of ethanol to calcium oxide is 0.04 to 0.6, and the contact time between ethanol and digestion product is 5 to 80 minutes; S4, then putting the digestion product into a vacuum oven for drying, the vacuum oven has an operating temperature of 90 to 140° C., and the digestion product is dried in the vacuum oven for 1 to 10 hours; S5. Take out the digestion product dried in the vacuum oven and grind it into powder to obtain calcium hydroxide, a food additive.

2. The method for preparing a food additive calcium hydroxide according to claim 1, wherein The temperature of the digestion water is 20-70°C.

3. A method for preparing a food additive calcium hydroxide according to claim 1, characterized in that, The water / calcium oxide mass ratio is 0.4 to 0.

7.

4. A method for preparing a food additive calcium hydroxide according to claim 1, characterized in that, The digestion reaction time is 35 to 70 minutes.

5. A method for preparing a food additive calcium hydroxide according to claim 1, characterized in that, The ethanol / calcium oxide mass ratio is 0.05-0.

5.

6. A method for preparing a food additive calcium hydroxide according to claim 1, characterized in that, The contact time between the ethanol and the digestion product is 10 to 60 minutes.

7. A method for preparing a food additive calcium hydroxide according to claim 1, characterized in that, The working temperature of the vacuum oven is 100-130°C.

8. A method for preparing a food additive calcium hydroxide according to claim 1, characterized in that, The digestion product is dried in the vacuum oven for 2 to 8 hours.

9. A method for preparing a food additive calcium hydroxide according to claim 1, characterized in that, The gas escaping from the vacuum oven is condensed and collected, and then recovered by distillation to obtain ethanol for recycling.

10. A method for preparing a food additive calcium hydroxide according to claim 1, characterized in that: The kiln-burned quicklime is calcium oxide, wherein the kiln-burned quicklime is screened according to the physical and chemical indicators of the national food safety standard and used in step S2; in step S4, a grinder is used to grind the digestion product.