Method for preparing nanoscale carbonized steel slag cementing material
Through the accelerated reaction of magnesium chloride catalyzing and alcohol amine compounds, nanoscale carbonized steel slag gelling materials were prepared, which solved the problems of steel slag activity and particle size control, and improved the mechanical properties and industrial application value of cement-based materials.
Patent Information
- Application Number
- CN202411027718.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-12-06
AI Technical Summary
The prior art is difficult to effectively improve the specific surface area and activity of steel slag, and the preparation process is complex and the energy consumption is high. It is impossible to effectively control the CaCO3 crystal particle size of steel slag powder, which limits its wide application in the field of building materials.
The carbonization of steel slag powder is catalyzed by magnesium chloride to produce argon-type carbonization products, and the conversion of argon into calcite is accelerated by using alcohol amine compounds, so as to prepare nanoscale carbonized steel slag gelling materials within 10 to 60 minutes, and increase their specific surface area and active.
Nanocarbonized steel slag gelling material with significantly improved specific surface area was prepared in a short period of time, which improved the mechanical properties of cement-based materials, and adopted a simple operation method, low energy consumption, and had high industrial application value.
Smart Images

Figure CN119080413A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of bulk solid waste resource treatment, and in particular to a method for preparing a nano-scale carbonized steel slag cementitious material. Background Art
[0002] Steel slag is a solid waste discharged during the steelmaking process, accounting for about 10% to 15% of crude steel production. The main chemical component of steel slag is CaO, which accounts for about 40% to 50%, so it has a high theoretical CO2 fixation capacity. Due to the high temperature of steel slag formation, the silicate minerals are densely crystallized, and the steel slag has a high hardness, resulting in poor grindability and high cost in processing and preparing powders. C2S and C3S in steel slag can generate CSH gel and Ca(OH)2 after hydration, but the hydration reaction is very slow. Compared with silicate cement, the second hydration exothermic peak of steel slag appears later, and the exothermic heat flow peak is less than 10% of cement, so the activity of steel slag is poor.
[0003] Steel slag has a large discharge volume and large fluctuations in composition (mainly affected by the iron ore raw materials, the type of steel furnace, forging and pretreatment methods), and contains a large amount of free CaO and free MgO, which leads to poor stability of steel slag products and easily causes expansion damage to concrete structures. The large amount of steel slag accumulation occupies arable land and often causes secondary pollution to the environment.
[0004] At present, steel slag is mainly used as an admixture and aggregate in the field of building materials to replace part of cement and sand and gravel aggregates. However, the low activity and poor stability of steel slag limit the wide application of steel slag as an auxiliary cementitious material. Although related inventions use methods such as adding activators and mechanical grinding to increase the specific surface area of steel slag and improve the activity of steel slag, and use CO2 storage to improve the stability of steel slag. However, the above methods often require the use of sophisticated instruments and equipment, and the complicated operating steps consume more energy, and the addition of additional activators increases costs. Therefore, the above methods cannot effectively increase the specific surface area of steel slag and improve the activity of steel slag.
[0005] The Chinese patent application with publication number CN118063112A filed by the applicant recently discloses a method for improving the carbon dioxide storage rate of steel slag powder, comprising the following steps: in water, under the action of an alcohol amine compound, the steel slag powder and carbon dioxide undergo a carbonization reaction, and after the reaction is completed, the steel slag powder with carbon dioxide stored is obtained by post-treatment; the alcohol amine compound is one or a combination of N-methyldiethanolamine, triethanolamine, monoethanolamine, triisopropanolamine, diethanolisopropanolamine, glycerol phosphate, 2-methyl-2-methyl-propanol and piperazine; the steel slag powder has a specific surface area of 300~600m 2 / kg of converter steel slag powder. The above method adopts an appropriate method to improve the carbon dioxide sequestration method. The experimental conditions are simple, no specific pressure vessel and high concentration of CO2 are required, and the carbon dioxide sequestration rate of steel slag powder is greatly improved within 20 to 60 minutes. The carbon dioxide sequestration rate is increased by 70 to 120%, and nano-scale steel slag powder is obtained, and the problem of poor stability of steel slag powder is solved.
[0006] A Chinese patent with the authorization announcement number CN115557763B discloses a thermal insulation material formed by steel slag absorbing CO2 and a preparation method thereof. The method evenly mixes steel slag powder with calcium stearate, calcium hydroxide and silica fume, and then mixes and stirs with magnesium chloride solution and hydrogen peroxide solution in turn, and vibrates to form a blank, and the blank is placed in a reactor with CO2 gas, and the thermal insulation material is obtained after the carbonization reaction. The method uses the action of a regulating agent to form a mesh skeleton formed by aragonite-type CaCO3 crystals in the steel slag. However, the preparation process needs to control related complex factors such as ball milling, pressure, and humidity, has high energy consumption and long reaction time, and cannot control the particle size of the steel slag product, and does not fundamentally solve the problem of regulating the steel slag powder CaCO3 crystals.
[0007] Mei Jieqiong, Lu Shijian and others mentioned in "Research Progress on Preparation of Polycrystalline Calcium Carbonate from Industrial Solid Waste by CO2 Indirect Mineralization (Clean Coal Technology, Vol. 30, No. 3)" that adjusting the mineralization reaction conditions such as temperature, pH, stirring rate and CO2 ventilation rate or adding crystal control agents can effectively control the crystal form, morphology and size of calcium carbonate. In the process of calcium carbonate formation, temperature, pressure, CO2 flow rate, CO2 concentration, Ca 2+ Parameters such as concentration, stirring rate, and solution pH are all important factors affecting the nucleation rate and crystal growth rate of calcium carbonate. Sodium dodecylbenzene sulfonate, docosanoic acid, MgCl2, Mg(OH)2, and alcoholamines can be used as calcium carbonate crystal form controllers. However, the document does not propose the use of multiple methods to compositely regulate the CaCO3 crystal form, and can only separate and treat the steel slag powder through the above method to obtain calcite crystal calcium carbonate with a particle size of 33.29μm or vaterite crystal calcium carbonate products with a particle size of 1~3μm. Summary of the invention
[0008] The problem to be solved by the present invention is to provide a method for preparing a carbonized steel slag cementitious material with a nanometer scale in view of the above-mentioned deficiencies existing in the prior art. The method firstly induces the carbonization of steel slag powder to produce aragonite by catalysis of magnesium chloride, and then accelerates the conversion of aragonite into calcite by an alcoholamine compound (instead of separating and obtaining nanometer-sized calcite crystalline calcium carbonate or micrometer-sized vaterite crystalline calcium carbonate products). The carbonized steel slag cementitious material with a nanometer scale can be prepared in about 10 to 60 minutes, and has the advantages of increasing the specific surface area of the carbonized steel slag, improving the activity of the carbonized steel slag, and enhancing the mechanical properties of cement-based materials.
[0009] The above-mentioned object of the present invention is achieved through the following technical solutions: A method for preparing a nano-scale carbonized steel slag cementitious material comprises the following steps: S1: mixing steel slag powder and magnesium chloride aqueous solution by stirring to obtain a first steel slag mixed solution; S2. introducing carbon dioxide into the first steel slag mixed liquid obtained in S1 to carry out a primary carbonization reaction to obtain an aragonite-type carbonized steel slag reaction liquid; S3: mixing the aragonite carbonized steel slag reaction liquid obtained in S2 with the alcoholamine compound by stirring to obtain a second steel slag mixed liquid; S4: introducing carbon dioxide into the second steel slag mixed liquid obtained in S3 to perform a secondary carbonization reaction to obtain a calcite-type carbonized steel slag reaction liquid; S5: post-treating the calcite-type carbonized steel slag reaction liquid obtained in S4 to obtain a nano-scale carbonized steel slag cementitious material.
[0010] Furthermore, in S1, the mass ratio of steel slag powder to magnesium chloride aqueous solution is controlled to be 0.05-0.30:1, and the steel slag powder has a specific surface area of 300-600m 2 / kg converter steel slag powder, the mass concentration of magnesium chloride in the aqueous solution is 0.05~5.00%. Among them, the concentration of magnesium chloride aqueous solution can be adjusted according to actual conditions (such as carbonized steel slag dosage, reaction time, yield, etc.), and within the above-mentioned ratio range, it can effectively catalyze and induce the carbonization reaction of steel slag powder.
[0011] Furthermore, in S1, the stirring and mixing temperature is controlled to be 20-40° C., the rotation speed is 100-500 r / min, and the magnetic stirring power is 20-50 W. The stirring and mixing time should be long enough to ensure that the steel slag powder and the magnesium chloride aqueous solution are fully mixed, thereby improving the reaction efficiency.
[0012] Further, in S2, the flow rate of carbon dioxide is controlled to be 0.1-1.0 L / min and the volume concentration is 20-50%. The introduction speed and amount of carbon dioxide have a great influence on the primary carbonization reaction. By controlling the introduction speed and amount of carbon dioxide, the generation of aragonite-type carbonized steel slag reaction liquid can be accurately controlled.
[0013] Furthermore, in S2, the first steel slag mixed liquid is continuously stirred and mixed under the same conditions as S1, and the time of the primary carbonization reaction is controlled to be 5 to 30 minutes. During the process of introducing carbon dioxide, stirring should be continued to ensure the uniformity of the reaction.
[0014] Further, in S3, the mass ratio of steel slag powder to alcoholamine compound is controlled to be 1:0.0050-0.0500, and the alcoholamine compound is one or a combination of N-methyldiethanolamine, triethanolamine, monoethanolamine, triisopropanolamine, diethanolisopropanolamine, glycerol phosphate, 2-methyl-2-methyl-propanol and piperazine. By adding alcoholamine compounds, the process of converting aragonite into calcite can be accelerated, thereby shortening the reaction time.
[0015] Furthermore, in S3, the stirring and mixing temperature is controlled to be 40-60° C., the rotation speed is 500-1000 r / min, and the magnetic stirring power is 20-50 W. The stirring and mixing time should be long enough to ensure that the aragonite carbonized steel slag reaction liquid and the alcoholamine compound are fully mixed, thereby improving the reaction efficiency.
[0016] Further, in the S4, the flow rate of carbon dioxide is controlled to be 1.0-3.0 L / min and the volume concentration is 50-99%. Carbon dioxide is introduced again for secondary carbonization reaction. The purpose of this step is to ensure the sufficient generation of calcite-type carbonized steel slag reaction liquid. Similar to the primary carbonization reaction, the introduction speed and amount of carbon dioxide should be accurately controlled to accurately control the generation of calcite-type carbonized steel slag reaction liquid.
[0017] Furthermore, in S4, the second steel slag mixture is continuously stirred and mixed under the same conditions as S3, and the time of the primary carbonization reaction is controlled to be 5 to 30 minutes. During the process of introducing carbon dioxide, stirring should be continued to ensure the uniformity of the reaction.
[0018] Furthermore, in S5, the post-treatment includes, after removing the supernatant of the calcite-type carbonized steel slag reaction solution, drying at 60-105° C. to obtain a carbonized steel slag gel material having a nanometer scale. The post-treatment process may also include steps such as centrifugation, washing, and drying to remove impurities in the reaction solution and improve the purity of the carbonized steel slag gel material.
[0019] In summary, the beneficial technical effects of the present invention are: 1. The present invention first induces carbonization of steel slag powder to produce aragonite through magnesium chloride catalysis, and then accelerates the conversion of aragonite into calcite through alcoholamine compounds, so that carbonized steel slag cementitious materials with nanometer scale can be obtained in a short time; at the same time, the preparation method of the present invention can significantly increase the specific surface area of carbonized steel slag, improve its activity, thereby improving the mechanical properties of cement-based materials, and uses environmentally friendly materials, and the reaction conditions are mild, which has high industrial application value; 2. The preparation method of the present invention can efficiently prepare nano-scale carbonized steel slag cementitious materials within 10 to 60 minutes. The prepared nano-carbonized steel slag cementitious materials have a specific surface area of 19 to 40.9 m2 / g, pore volume 0.032~0.0561cm 3 / g, and an average particle size of 5.50~6.86nm. Compared with the existing method, the specific surface area and pore volume of the nano-carbonized steel slag cementitious material are increased by 35~52 times and 45~51 times, respectively, and the average particle size is reduced by 1000~1200 times, achieving the purpose of increasing the specific surface area of the carbonized steel slag and improving the activity of the carbonized steel slag.
[0020] 3. The present invention adopts a pressure-free conventional instrument to prepare a nano-carbonized steel slag cementitious material with good stability at low energy consumption and high efficiency. The operation is extremely simple and the cost is extremely low.
[0021] 4. The nano-carbonized steel slag cementitious material prepared by the present invention is added to cement-based materials to replace part of the cement, thereby reducing the use of cement, improving the shrinkage cracking phenomenon of cement-based materials, and improving their crack resistance and mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 3 is a SEM image of the carbonized steel slag cementitious material of Example 1 of the present invention.
[0023] Figure 2 It is a graph showing the autogenous shrinkage data of cement paste of concrete specimens at different carbonized steel slag cementitious material dosages of Examples 18 to 24 of the present invention.
[0024] Figure 3 It is a data graph of crack area and crack width of concrete specimens at different carbonized steel slag cementitious material dosages of Examples 18 to 24 of the present invention.
[0025] Figure 4 It is a data diagram of particle size of carbonized steel slag cementitious material at different dosages of amine compounds in Examples 14 to 17 of the present invention.
[0026] Figure 5 It is a data graph of specific surface area of carbonized steel slag cementitious material at different dosages of amine compounds in Examples 14 to 17 of the present invention.
[0027] Figure 6 It is a pore volume data diagram of the carbonized steel slag cementitious material at different alcoholamine compound dosages of Examples 14 to 17 of the present invention.
[0028] Figure 7 It is a SEM picture of the carbonized steel slag cementitious material of Comparative Example 1 of the present invention.
[0029] Figure 8 It is a SEM picture of the carbonized steel slag cementitious material of Comparative Example 2 of the present invention.
[0030] Fig. 9 It is a SEM picture of the carbonized steel slag cementitious material of Comparative Example 3 of the present invention.
[0031] Fig.10 This is a SEM image of the carbonized steel slag cementitious material of Example 21 of the present invention.
[0032] Fig.11 It is the XDR diagram of the carbonized steel slag cementitious materials of Examples 18 to 24 of the present invention and Comparative Examples 1 to 3.
[0033] Fig.12 It is a phase analysis diagram of the carbonized steel slag cementitious materials of Examples 18 to 24 and Comparative Examples 1 to 3 of the present invention based on QXRD refinement technology. DETAILED DESCRIPTION
[0034] In order to make the technical means, creative features, objectives and functions achieved by the present invention clearer and easier to understand, the present invention is further explained below in conjunction with the accompanying drawings and specific implementation methods.
[0035] Embodiment 1: A method for preparing a nano-scale carbonized steel slag cementitious material disclosed in the present invention comprises the following steps: S1 First prepare a magnesium chloride aqueous solution with a mass concentration of 0.05% in a beaker, and add 30% of the total weight of the magnesium chloride aqueous solution and a specific surface area of 360m 2 / kg of converter slag powder, and then place the beaker in a magnetic stirrer (Hunan Frontier Technology Co., Ltd., photosynthetic DF-101S), and control the heating in a water bath at 20°C, the speed is 200r / min, the magnetic stirring power is 20W, and the first slag mixed liquid is obtained by stirring and mixing; S2 continues to stir and mix the first steel slag mixed liquid under the same conditions as S1, and introduces carbon dioxide into the first steel slag mixed liquid obtained in S1, controls the flow rate of carbon dioxide to be 0.1 L / min and the volume concentration to be 50%, and then performs a primary carbonization reaction for 30 min to obtain an aragonite-type carbonized steel slag reaction liquid; S3: first, adding 0.50% of the total weight of propylene glycol phosphate to the aragonite carbonized steel slag reaction liquid obtained in S2, and then placing the beaker in a magnetic stirrer (Hunan Frontier Technology Co., Ltd., photosynthetic DF-101S), and controlling the heating in a water bath at 40°C, the speed of 800 r / min, the magnetic stirring power of 30 W, and stirring and mixing to obtain a second steel slag mixed liquid; S4 continues to stir and mix the second steel slag mixed liquid under the same conditions as S3, and introduces carbon dioxide into the second steel slag mixed liquid obtained in S3, controlling the flow rate of carbon dioxide to be 1.0 L / min and the volume concentration to be 80%, and then performs a primary carbonization reaction for 20 minutes to obtain a calcite-type carbonized steel slag reaction liquid; In step S5, after removing the supernatant of the calcite-type carbonized steel slag reaction solution obtained in step 4, the remaining reaction solution is dried at 75° C. to obtain a carbonized steel slag cementitious material having a nanometer scale.
[0036] Furthermore, the performance of the prepared carbonized steel slag cementitious material was tested: First, the specific surface area of the carbonized steel slag cementitious material was 35.6 m 2 / g, pore volume is 0.0368cm 3 / g, average particle size is 5.81nm; wherein, reference Figure 1 , SEM verification shows that the carbonized steel slag cementitious material with nanometer scale is prepared by the above method, and the transformation from aragonite to calcite is completed. If the reaction sequence or reaction conditions are changed, the above material cannot be obtained; Secondly, the prepared nano-carbonized steel slag cementitious material was used to replace 30% of the total weight of P•O 42.5 grade ordinary Portland cement to obtain a mixed cementitious material, and the mass ratio of the mixed cementitious material to water in the following specimens was controlled to be 1:0.35; The test specimens were prepared according to GB / T1346-2011 "Test Methods for Water Consistency, Setting Time and Stability of Cement Standard Consistency", and their stability was good; According to the bellows method recorded in ASTM C1698-2009, Standard Test Method for Autogenous Strain of Cement Paste and Mortar, the specimens were prepared and subjected to autogenous shrinkage test. The autogenous shrinkage inhibition rate of cement paste reached 23.4%. According to GB / T17671-1999 "Test method for strength of cement mortar (ISO method)", specimens were prepared and their mechanical properties were tested. Compared with blank specimens with 0% replacement rate, the compressive strength of cement mortar after 28 days increased by 21.5%, and the flexural strength after 28 days increased by 8.7%.
[0037] Embodiment 2: A method for preparing a nano-scale carbonized steel slag cementitious material disclosed in the present invention comprises the following steps: S1 First prepare a magnesium chloride aqueous solution with a mass concentration of 2.50% in a beaker, and add a 5% by weight magnesium chloride aqueous solution with a specific surface area of 516m 2 / kg of converter slag powder, and then place the beaker in a magnetic stirrer (Hunan Frontier Technology Co., Ltd., photosynthetic DF-101S), and control the heating in a water bath at 30°C, the speed is 100r / min, the magnetic stirring power is 50W, and the first slag mixed liquid is obtained by stirring and mixing; S2 continues to stir and mix the first steel slag mixed liquid under the same conditions as S1, and introduces carbon dioxide into the first steel slag mixed liquid obtained in S1, controlling the flow rate of carbon dioxide to 0.5 L / min and the volume concentration to 20%, and then performs a primary carbonization reaction for 10 min to obtain an aragonite-type carbonized steel slag reaction liquid; S3: first, add 2.00% of propylene glycol phosphate to the total weight of the converter slag powder in the aragonite carbonized slag reaction liquid obtained in S2, then place the beaker in a magnetic stirrer (Hunan Frontier Technology Co., Ltd., photosynthetic DF-101S), and control the heating in a water bath at 50°C, the speed at 500r / min, the magnetic stirring power at 40W, and stir and mix to obtain a second slag mixture; S4 continues to stir and mix the second steel slag mixed liquid under the same conditions as S3, and introduces carbon dioxide into the second steel slag mixed liquid obtained in S3, controlling the flow rate of carbon dioxide to 2.0 L / min and the volume concentration to 99%, and then performs a primary carbonization reaction for 5 minutes to obtain a calcite-type carbonized steel slag reaction liquid; In step S5, after removing the supernatant of the calcite-type carbonized steel slag reaction solution obtained in step 4, the remaining reaction solution is dried at 105° C. to obtain a carbonized steel slag cementitious material having a nanometer scale.
[0038] Furthermore, the performance of the prepared carbonized steel slag cementitious material was tested: First, the specific surface area of the carbonized steel slag cementitious material was 22.1 m 2 / g, pore volume is 0.0465cm 3 / g, average particle size is 6.75nm; Secondly, the prepared nano-carbonized steel slag cementitious material replaced 60% of the total weight of P•O 42.5 grade ordinary Portland cement to obtain a mixed cementitious material, and the mass ratio of the mixed cementitious material in the following specimens was controlled as follows: polycarboxylate water reducer: machine-made sand: water was 1:0.015:2.5:0.50; According to ASTM C1581-04, Standard Test Method for Determining Age atCracking and Induced Tensile Stress Characteristics of Mortar and Concreteunder Restrained Shrinkage, the specimens were prepared and the crack area and crack width were tested. Compared with the blank specimens with 0% replacement rate, the crack area was reduced by 12.5% and the crack width was reduced by 46.3%. According to GB / T17671-1999 "Test Method for Cement Mortar Strength (ISO Method)", the specimens were prepared and their mechanical properties were tested. Compared with the blank specimens with 0% replacement rate, the 28-day cement paste compressive strength increased by 23.6%, and the 28-day flexural strength increased by 7.2%. Again, the prepared nano-carbonized steel slag cementitious material was used to replace 0, 5, 10, 15, 20, 25, and 30% of the total weight of P•O 42.5 grade ordinary Portland cement to obtain a mixed cementitious material, and the mass ratio of the mixed cementitious material in the following specimens was controlled as follows: polycarboxylate water reducer: machine-made sand: water was 1:0.015:2.5:0.50; According to the bellows method recorded in ASTM C1698-2009, Standard Test Method for Autogenous Strain of Cement Paste and Mortar, the specimens were prepared and subjected to autogenous shrinkage test. The test results are shown in Figure 2 As shown; According to ASTM C1581-04, Standard Test Method for Determining Age atCracking and Induced Tensile Stress Characteristics of Mortar and Concreteunder Restrained Shrinkage, the specimens were prepared and the crack area and crack width were tested. The test results are shown in the figure. Figure 3 shown.
[0039] Embodiment 3: A method for preparing a nano-scale carbonized steel slag cementitious material disclosed in the present invention comprises the following steps: S1 First prepare a magnesium chloride aqueous solution with a mass concentration of 5.00% in a beaker, and add a magnesium chloride solution with a specific surface area of 430m2 and a weight of 30% of the total weight of the magnesium chloride aqueous solution. 2 / kg of converter steel slag powder, and then place the beaker in a magnetic stirrer (Hunan Frontier Technology Co., Ltd., photosynthetic DF-101S), and control the heating in a water bath at 20°C, the speed is 100r / min, the magnetic stirring power is 50W, and the first steel slag mixed liquid is obtained by stirring and mixing; S2 continues to stir and mix the first steel slag mixed liquid under the same conditions as S1, and introduces carbon dioxide into the first steel slag mixed liquid obtained in S1, controls the flow rate of carbon dioxide to be 1.0 L / min and the volume concentration to be 50%, and then performs a primary carbonization reaction for 5 minutes to obtain an aragonite-type carbonized steel slag reaction liquid; S3: first, adding 5.00% of propylene glycol phosphate to the total weight of the converter slag powder into the aragonite carbonized slag reaction liquid obtained in S2, and then placing the beaker in a magnetic stirrer (Hunan Frontier Technology Co., Ltd., photosynthetic DF-101S), and controlling the heating in a water bath at 60°C, the speed at 1000 r / min, the magnetic stirring power at 50 W, and stirring and mixing to obtain a second slag mixture; S4 continues to stir and mix the second steel slag mixed liquid under the same conditions as S3, and introduces carbon dioxide into the second steel slag mixed liquid obtained in S3, controlling the flow rate of carbon dioxide to be 3.0 L / min and the volume concentration to be 99%, and then performs a primary carbonization reaction for 20 min to obtain a calcite-type carbonized steel slag reaction liquid; In step S5, after removing the supernatant of the calcite-type carbonized steel slag reaction solution obtained in step 4, the remaining reaction solution is dried at 60° C. to obtain a carbonized steel slag cementitious material having a nanometer scale.
[0040] Furthermore, the performance of the prepared carbonized steel slag cementitious material was tested: First, the specific surface area of the carbonized steel slag cementitious material was 28.9 m 2 / g, pore volume is 0.0408cm 3 / g, average particle size is 6.36nm; Secondly, the prepared nano-carbonized steel slag cementitious material replaced 40% of the total weight of P•O 42.5 grade ordinary Portland cement to obtain a mixed cementitious material, and the mass ratio of the mixed cementitious material in the following specimens was controlled to be 1:0.0035:1.6:2.3:0.49; The specimens were prepared according to JGJ55-2011 "Code for Design of Ordinary Concrete Mix", and their mechanical properties were tested according to GB / T50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete". Compared with the blank specimens with 0% replacement rate, the compressive strength of the cement paste at 28 days increased by 25.7%, and the flexural strength at 28 days increased by 9.6%.
[0041] Embodiment 4: A method for preparing a nano-scale carbonized steel slag cementitious material disclosed in the present invention comprises the following steps: S1 First prepare a magnesium chloride aqueous solution with a mass concentration of 3.50% in a beaker, and add 25% of the total weight of the magnesium chloride aqueous solution and a specific surface area of 600m 2 / kg of converter slag powder, and then placing the beaker in a magnetic stirrer (Hunan Frontier Technology Co., Ltd., photosynthetic DF-101S), and controlling the heating in a water bath at 40°C, the speed is 500r / min, the magnetic stirring power is 50W, and the first slag mixed liquid is obtained by stirring and mixing; S2 continues to stir and mix the first steel slag mixed liquid under the same conditions as S1, and introduces carbon dioxide into the first steel slag mixed liquid obtained in S1, controls the flow rate of carbon dioxide to be 1.0 L / min and the volume concentration to be 50%, and then performs a primary carbonization reaction for 10 min to obtain an aragonite-type carbonized steel slag reaction liquid; S3: first, adding 2.50% of the total weight of propylene glycol phosphate to the aragonite carbonized steel slag reaction liquid obtained in S2, and then placing the beaker in a magnetic stirrer (Hunan Frontier Technology Co., Ltd., photosynthetic DF-101S), and controlling the heating in a water bath at 40°C, the speed of 600 r / min, the magnetic stirring power of 50 W, and stirring and mixing to obtain a second steel slag mixed liquid; S4 continues to stir and mix the second steel slag mixed liquid under the same conditions as S3, and introduces carbon dioxide into the second steel slag mixed liquid obtained in S3, controlling the flow rate of carbon dioxide to be 1.5 L / min and the volume concentration to be 60%, and then performs a primary carbonization reaction for 20 min to obtain a calcite-type carbonized steel slag reaction liquid; In step S5, after removing the supernatant of the calcite-type carbonized steel slag reaction solution obtained in step 4, the remaining reaction solution is dried at 95° C. to obtain a carbonized steel slag cementitious material having a nanometer scale.
[0042] Furthermore, the performance of the prepared carbonized steel slag cementitious material was tested: First, the specific surface area of the carbonized steel slag cementitious material was 40.9 m 2 / g, pore volume is 0.0561cm 3 / g, average particle size is 5.50nm; Secondly, the prepared nano-carbonized steel slag cementitious material was used to replace 20% of the total weight of P•O 42.5 grade ordinary Portland cement to obtain a mixed cementitious material, and the mass ratio of the mixed cementitious material to water in the following specimens was controlled to be 1:0.40; The test specimens were prepared according to GB / T1346-2011 "Test Methods for Water Consistency, Setting Time and Stability of Cement Standard Consistency", and their stability was good; According to the bellows method recorded in ASTM C1698-2009, Standard Test Method for Autogenous Strain of Cement Paste and Mortar, the specimens were prepared and subjected to autogenous shrinkage test. The autogenous shrinkage inhibition rate of cement paste reached 60.2%. According to GB / T17671-1999 "Test method for strength of cement mortar (ISO method)", specimens were prepared and their mechanical properties were tested. Compared with blank specimens with 0% replacement rate, the compressive strength of cement mortar after 28 days increased by 50.1%, and the flexural strength after 28 days increased by 19.8%.
[0043] Example 5: A method for preparing a nano-scale carbonized steel slag cementitious material disclosed in the present invention comprises the following steps: S1 First prepare a magnesium chloride aqueous solution with a mass concentration of 4.50% in a beaker, and add 25% of the total weight of the magnesium chloride aqueous solution and a specific surface area of 600m 2 / kg of converter slag powder, and then place the beaker in a magnetic stirrer (Hunan Frontier Technology Co., Ltd., photosynthetic DF-101S), and control the heating in a water bath at 25°C, the speed is 300r / min, the magnetic stirring power is 30W, and the first slag mixed liquid is obtained by stirring and mixing; S2 continues to stir and mix the first steel slag mixed liquid under the same conditions as S1, and introduces carbon dioxide into the first steel slag mixed liquid obtained in S1, controlling the flow rate of carbon dioxide to 0.5 L / min and the volume concentration to 40%, and then performs a primary carbonization reaction for 25 min to obtain an aragonite-type carbonized steel slag reaction liquid; S3: first, add 2.50% of the total weight of propylene glycol phosphate to the aragonite carbonized steel slag reaction liquid obtained in S2, then place the beaker in a magnetic stirrer (Hunan Frontier Technology Co., Ltd., photosynthetic DF-101S), and control the heating in a water bath at 40°C, the speed is 500r / min, the magnetic stirring power is 50W, and stir and mix to obtain a second steel slag mixed liquid; S4 continues to stir and mix the second steel slag mixed liquid under the same conditions as S3, and introduces carbon dioxide into the second steel slag mixed liquid obtained in S3, controlling the flow rate of carbon dioxide to be 1.5 L / min and the volume concentration to be 80%, and then performs a primary carbonization reaction for 10 min to obtain a calcite-type carbonized steel slag reaction liquid; In step S5, after removing the supernatant of the calcite-type carbonized steel slag reaction solution obtained in step 4, the remaining reaction solution is dried at 105° C. to obtain a carbonized steel slag cementitious material having a nanometer scale.
[0044] Furthermore, the performance of the prepared carbonized steel slag cementitious material was tested: First, the specific surface area of the carbonized steel slag cementitious material was 21.7 m 2 / g, pore volume is 0.0351cm 3 / g, average particle size is 5.97nm; Secondly, the prepared nano-carbonized steel slag cementitious material replaced 20% of the total weight of P•O 42.5 grade ordinary Portland cement to obtain a mixed cementitious material, and the mass ratio of the mixed cementitious material in the following specimens was controlled as follows: polycarboxylate water reducer: machine-made sand: water was 1:0.02:3:0.35; The test specimens were prepared according to GB / T1346-2011 "Test Methods for Water Consistency, Setting Time and Stability of Cement Standard Consistency", and their stability was good; According to ASTM C1581-04, Standard Test Method for Determining Age atCracking and Induced Tensile Stress Characteristics of Mortar and Concreteunder Restrained Shrinkage, the specimens were prepared and the crack area and crack width were tested. Compared with the blank specimens with 0% replacement rate, the crack area was reduced by 18.6% and the crack width was reduced by 56.5%. According to GB / T17671-1999 "Test method for strength of cement mortar (ISO method)", specimens were prepared and their mechanical properties were tested. Compared with blank specimens with 0% replacement rate, the compressive strength of cement mortar after 28 days increased by 28.9%, and the flexural strength after 28 days increased by 10.3%.
[0045] Example 6: A method for preparing a nano-scale carbonized steel slag cementitious material disclosed in the present invention comprises the following steps: S1 First prepare a magnesium chloride aqueous solution with a mass concentration of 1.50% in a beaker, and add a 20% by weight magnesium chloride aqueous solution with a specific surface area of 480m 2 / kg of converter slag powder, and then placing the beaker in a magnetic stirrer (Hunan Frontier Technology Co., Ltd., photosynthetic DF-101S), and controlling the heating in a 40°C water bath, the speed is 400r / min, the magnetic stirring power is 40W, and the first slag mixed liquid is obtained by stirring and mixing; S2 continues to stir and mix the first steel slag mixed liquid under the same conditions as S1, and introduces carbon dioxide into the first steel slag mixed liquid obtained in S1, controlling the flow rate of carbon dioxide to 0.4 L / min and the volume concentration to 30%, and then performs a primary carbonization reaction for 20 min to obtain an aragonite-type carbonized steel slag reaction liquid; S3: first, add 2.00% of propylene glycol phosphate to the total weight of the converter slag powder into the aragonite carbonized steel slag reaction liquid obtained in S2, then place the beaker in a magnetic stirrer (Hunan Frontier Technology Co., Ltd., photosynthetic DF-101S), and control the heating in a water bath at 60°C, the speed is 500r / min, the magnetic stirring power is 50W, and stir and mix to obtain a second steel slag mixture; S4 continues to stir and mix the second steel slag mixed liquid under the same conditions as S3, and introduces carbon dioxide into the second steel slag mixed liquid obtained in S3, controlling the flow rate of carbon dioxide to be 2.0 L / min and the volume concentration to be 50%, and then performs a primary carbonization reaction for 15 min to obtain a calcite-type carbonized steel slag reaction liquid; In step S5, after removing the supernatant of the calcite-type carbonized steel slag reaction solution obtained in step 4, the remaining reaction solution is dried at 105° C. to obtain a carbonized steel slag cementitious material having a nanometer scale.
[0046] Furthermore, the performance of the prepared carbonized steel slag cementitious material was tested: First, the specific surface area of the carbonized steel slag cementitious material is 32.5m 2 / g, pore volume is 0.0476cm 3 / g, average particle size is 5.71nm; Secondly, the prepared nano-carbonized steel slag cementitious material replaced 30% of the total weight of P•O 42.5 grade ordinary Portland cement to obtain a mixed cementitious material, and the mass ratio of the mixed cementitious material in the following specimens was controlled to be 1:0.0045:1.5:2.5:0.47; The specimens were prepared according to JGJ55-2011 "Code for Design of Ordinary Concrete Mix", and their mechanical properties were tested according to GB / T50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete". Compared with the blank specimens with 0% replacement rate, the 28-day cement paste compressive strength increased by 28.6%, and the 28-day flexural strength increased by 11.5%.
[0047] Examples 7 to 10 are methods for preparing nanoscale carbonized steel slag cementitious materials disclosed in the present invention. The difference from Example 1 is that 1.50, 2.50, 3.50, and 4.50% (i.e., admixture dosage, wt%) of N-methyldiethanolamine (an alcohol amine compound) of the total weight of converter steel slag powder is added to S3, respectively.
[0048] According to the BET (nitrogen physical adsorption specific surface area) analysis test, the particle size, specific surface area and control volume of the carbonized steel slag cementitious material are as follows: Figures 4 to 6 shown.
[0049] Examples 11 to 17 are methods for preparing nanoscale carbonized steel slag cementitious materials disclosed in the present invention. The difference from Example 1 is that the alcoholamine compounds are N-methyldiethanolamine, triethanolamine, monoethanolamine, triisopropanolamine, diethanolisopropanolamine, 2-amino-2-methyl-propanol, and piperazine.
[0050] Examples 18 to 24 are methods for preparing nanoscale carbonized steel slag cementitious materials disclosed in the present invention. The difference from Example 7 is that the mass concentration of the magnesium chloride aqueous solution, the dosage of the alcoholamine compound, and the average particle size of the carbonized steel slag cementitious materials are as shown in Table 1.
[0051] Comparative Examples 1 to 3 are methods for preparing nano-scale carbonized steel slag cementitious materials disclosed in the present invention. The difference from Example 7 is that the mass concentration of the magnesium chloride aqueous solution, the amount of the alcoholamine compound, and the average particle size of the carbonized steel slag cementitious materials are shown in Table 1. The SEM test results of the carbonized steel slag cementitious materials are shown in Table 1. Figures 7 to 10 As shown in the figure, the XDR test results of carbonized steel slag cementitious materials are as follows Figures 11-12 shown.
[0052] Table 1 Comparative Example 1 Comparative Example 2 Comparative Example 3 Embodiment 18 Embodiment 19 Embodiment 20 Embodiment 21 Embodiment 22 Embodiment 23 Embodiment 24 <![CDATA[MgCl2 concentration]]> 0% 1% 0% 2% 3% 3% 4% 4% 5% 5% MDEA dosage 0% 0% 1% 1% 1% 2% 3% 4% 4% 5% Average particle size 20.6μm 8.4μm 5.6μm 5.53nm 5.75nm 6.12nm 6.46nm 6.96nm 5.97nm 6.04nm Figure 7 The SEM image of carbonized steel slag cementitious material when the addition amount of MgCl2 and MDEA is 0wt% shows that when MgCl2 and MDEA are not added, the steel slag powder generates hexagonal plate-like or flake-like Ca(OH)2. Figures 11-12 In the test, SS is the untreated steel slag powder raw material, ASS is the uncarbonized steel slag cementitious material, M0SS, M05SS, M15SS, M25SS, M35SS and M45SS are the carbonized steel slag cementitious materials with the alcohol amine compound dosage of 0, 0.5, 1.5, 2.5 and 4.5%, respectively. The XRD spectrum and phase analysis of the carbonized steel slag cementitious materials show that no CaCO3 is produced. Figure 8 This is the SEM image of the carbonized steel slag cementitious material when the MgCl2 dosage is 1wt% and the MDEA dosage is 0wt%. It shows that when only MgCl2 is added for single regulation, the CaCO3 crystal form generated by the steel slag powder is spherical vaterite and strip-shaped or needle-shaped aragonite. Fig. 9 This is the SEM image of the carbonized steel slag cementitious material when the MgCl2 dosage is 0wt% and the MDEA dosage is 1wt%, indicating that when only MDEA is added for single regulation, the CaCO3 crystal form generated by the steel slag powder is strip-shaped or needle-shaped aragonite. Fig.10 The SEM image of carbonized steel slag cementitious material with MgCl2 content of 4wt% and MDEA content of 3wt% shows that when the two-step method is used for composite regulation, the CaCO3 crystal form generated by the steel slag powder is coconut-shaped calcite, and Figure 1 The SEM test results showed that the particle size was nanometer. Figures 11-12 The XRD spectrum and phase analysis of medium-carbonized steel slag cementitious materials show that compared with single regulation, more CaCO3 calcite with coconut-like crystal form is generated during the two-step composite regulation.
[0053] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. A method for preparing a nano-scale carbonized steel slag cementitious material, characterized in that: The following steps are included: S1: mixing steel slag powder and magnesium chloride aqueous solution by stirring to obtain a first steel slag mixed solution; S2. introducing carbon dioxide into the first steel slag mixed liquid obtained in S1 to carry out a primary carbonization reaction to obtain an aragonite-type carbonized steel slag reaction liquid; S3: mixing the aragonite carbonized steel slag reaction liquid obtained in S2 with the alcoholamine compound by stirring to obtain a second steel slag mixed liquid; S4: introducing carbon dioxide into the second steel slag mixed liquid obtained in S3 to perform a secondary carbonization reaction to obtain a calcite-type carbonized steel slag reaction liquid; S5: post-treating the calcite-type carbonized steel slag reaction liquid obtained in S4 to obtain a nano-scale carbonized steel slag cementitious material.
2. The method for preparing a nanoscale carbonized steel slag cementitious material according to claim 1, characterized in that: In S1, the mass ratio of steel slag powder to magnesium chloride aqueous solution is controlled to be 0.05-0.30:1, and the steel slag powder has a specific surface area of 300-600m 2 / kg converter slag powder, the mass concentration of magnesium chloride in the aqueous solution is 0.05~5.00%.
3. The method for preparing a nano-scale carbonized steel slag cementitious material according to claim 1, characterized in that: In S1, the stirring and mixing temperature is controlled to be 20-40°C, the rotation speed is controlled to be 100-500 r / min, and the magnetic stirring power is controlled to be 20-50W.
4. The method for preparing a nano-scale carbonized steel slag cementitious material according to claim 1, characterized in that: In S2, the flow rate of carbon dioxide is controlled to be 0.1-1.0 L / min and the volume concentration is controlled to be 20-50%.
5. The method for preparing a nano-scale carbonized steel slag cementitious material according to claim 1, characterized in that: In S2, the first steel slag mixed liquid is continuously stirred and mixed under the same conditions as S1, and the time of the primary carbonization reaction is controlled to be 5 to 30 minutes.
6. The method for preparing a nano-scale carbonized steel slag cementitious material according to claim 1, characterized in that: In S3, the mass ratio of steel slag powder to alcohol amine compound is controlled to be 1:0.0050-0.0500, and the alcohol amine compound is one or a combination of several selected from N-methyldiethanolamine, triethanolamine, monoethanolamine, triisopropanolamine, diethanolisopropanolamine, glycerol phosphate, 2-methyl-2-methyl-propanol and piperazine.
7. The method for preparing a nano-scale carbonized steel slag cementitious material according to claim 1, characterized in that: In S3, the stirring and mixing temperature is controlled to be 40-60°C, the rotation speed is controlled to be 500-1000 r / min, and the magnetic stirring power is controlled to be 20-50W.
8. The method for preparing a nano-scale carbonized steel slag cementitious material according to claim 1, characterized in that: In S4, the flow rate of carbon dioxide is controlled to be 1.0-3.0 L / min and the volume concentration is controlled to be 50-99%.
9. The method for preparing a nano-scale carbonized steel slag cementitious material according to claim 1, characterized in that: In S4, the second steel slag mixed liquid is continuously stirred and mixed under the same conditions as S3, and the time of the primary carbonization reaction is controlled to be 5 to 30 minutes.
10. The method for preparing a nano-scale carbonized steel slag cementitious material according to claim 1, characterized in that: In the S5, the post-treatment includes removing the supernatant of the calcite-type carbonized steel slag reaction solution and drying it at 60-105°C to obtain a carbonized steel slag cementitious material having a nanometer scale.
Citation Information
Cited By
Application of amine auxiliary in accelerating carbonization of calcium-based solid waste
CN120055005A