Composite inorganic terrace material
By using micro-expanding agents made of industrial solid waste and modified blast furnace iron slag in inorganic grinding stone floors, the problem of easy cracking of floor materials during molding and hardening is solved, and the compressive strength and Tensile strength, and micro-expansion performance is improved through sintering and modification treatment, significantly improving the crack resistance and aesthetics of the floor.
Patent Information
- Application Number
- CN202411572245.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-06
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-11-06
AI Technical Summary
Inorganic grinding stone floors are prone to shrinking and cracking during molding and hardening, and are insufficient in strength, resulting in crack problems and poor aesthetics and durability.
Using micro-expanding agents made of industrial solid waste, modified blast furnace iron sludge and crack-resistant fibers, combined with silicate cement, aggregates and activators, a composite with high compressive strength and tensile strength is prepared. Inorganic floor materials, the micro-expansion properties and crack resistance of the material are improved by sintering and modification of the micro-expansion agent.
The high compressive strength, tensile strength and good micro-expansion properties of floor materials are achieved, the micro-expansion rate during the maintenance period is reduced, the crack resistance is significantly improved, and the actual use needs are met.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of concrete, and in particular to a composite inorganic floor material. Background Art
[0002] Inorganic terrazzo floor is an excellent floor, which is better than existing terrazzo floor in terms of strength, early strength, etc. At the same time, inorganic terrazzo floor can be paved seamlessly as a whole, and the overall shape is more beautiful; while the existing terrazzo floor usually needs to be separated by strips to prevent cracking, which leads to a large number of gaps and relatively poor appearance.
[0003] However, for inorganic terrazzo floors, cement is usually used as the cementitious material, and cement is prone to shrinkage and cracking during the molding and hardening process; at the same time, when the strength of the floor material is not enough, cracking is also prone to occur. Summary of the invention
[0004] In view of the above technical problems, the purpose of the present invention is to provide a composite inorganic floor material to address the defects of the prior art.
[0005] The present invention adopts the following technical scheme: a composite inorganic floor material, calculated by weight, includes: 30-50 parts of silicate cement, 80-120 parts of aggregate, 15-25 parts of blast furnace iron smelting slag, 0.5-2 parts of anti-cracking fiber, 5-10 parts of glass powder, 4-10 parts of activator, and 10-15 parts of micro-expansion agent; The preparation method of the micro-expanding agent comprises the following steps: taking 50-55 parts of lithium slag and 38-45 parts of red mud, crushing them, adding 20-25 parts of water, stirring them evenly, then granulating them, and then sintering them at 700-800°C for 2-4h, naturally cooling them to room temperature after the sintering, and then crushing them.
[0006] In the present invention, a new micro-expansion agent is proposed to solve the problem that conventional inorganic floors are prone to cracking. The micro-expansion agent is made of industrial solid waste. For lithium slag, it contains a large amount of silicon dioxide, aluminum oxide and calcium oxide, among which silicon dioxide and aluminum oxide exist in amorphous form. The main components of red mud are aluminum oxide, silicon dioxide, iron oxide and calcium oxide, and also contain a certain amount of non-ferrous metals. After the two are crushed, granulated and sintered, the final product has good micro-expansion performance. And compared with conventional calcium oxide and magnesium oxide expansion agents, the micro-expansion time of the expansion agent of the present invention is long, and the expansion multiple is relatively low in a short time, which will not affect the floor.
[0007] Aggregate is also called aggregate. The aggregate in the present invention is conventional aggregate in the floor field. Generally speaking, aggregate is divided into fine sand, medium sand and fine sand, all of which can be applied to the present invention.
[0008] Blast furnace iron smelting slag is a kind of cementitious material, and it is also a kind of solid waste, and it can also be used as an aggregate. Compared with cement, its advantage is that the particle size can be freely adjusted. According to the different particle sizes, the products after gelation and solidification have different micropores, which makes the floor material have certain air permeability; at the same time, when added to cement, it can also serve as a condensation nucleus for the initial hydration of cement, thereby accelerating the hydration process of cement. Generally speaking, it needs to be used together with an activator to quickly promote the hydration and gelation of blast furnace iron smelting slag.
[0009] An implementation manner of the present invention is that the aggregate is medium sand.
[0010] An implementation manner of the present invention is that the aggregate is a mixture of medium sand and fine sand, and the mass ratio of the medium sand to the fine sand is 8:2-5.
[0011] One embodiment of the present invention is that the particle size of the blast furnace iron smelting slag is not greater than 2 mm. The larger the particle size, the lower the flatness of the floor, the lower the strength, the greater the difficulty of hydration, and the worse the crack resistance. The smaller the particle size, the higher the flatness of the floor, the greater the final strength, the lower the difficulty of hydration, and the better the crack resistance. In fact, when the specific surface area of blast furnace iron smelting slag reaches 300m 2 / kg, its hydration basically does not require an activator. However, in the actual production process, the larger the specific surface area, the higher the production cost. Therefore, after a large number of experiments, the inventor found that when the particle size of blast furnace iron smelting slag is not more than 2mm, the floor has a higher flatness and higher compressive strength, which can meet the actual use needs.
[0012] One embodiment of the present invention is that the anti-cracking fiber is basalt fiber. In fact, many fibers can be applied to the present invention, such as polypropylene fiber, glass fiber, etc. However, from the actual use effect, basalt fiber has a longer life than polypropylene fiber; and is less harmful to the human body than glass fiber.
[0013] An embodiment of the present invention is that the activator is at least one of sodium hydroxide, sodium carbonate and water glass.
[0014] One embodiment of the present invention is that the floor material includes: 30 to 35 parts of silicate cement, 80 to 95 parts of aggregate, 15 to 20 parts of blast furnace iron smelting slag, 0.5 to 0.8 parts of anti-cracking fiber, 5 to 10 parts of glass powder, and 10 to 12 parts of micro-expansion agent.
[0015] One embodiment of the present invention is that the floor material includes: 38 to 42 parts of silicate cement, 100 to 110 parts of aggregate, 18 to 22 parts of blast furnace iron smelting slag, 1 to 1.5 parts of anti-cracking fiber, 7 to 8 parts of glass powder, and 12 to 15 parts of micro-expansion agent.
[0016] An embodiment of the present invention is that the floor material further includes 15 to 25 parts of inorganic pigments, and the inorganic pigment is at least one of titanium dioxide, phthalocyanine green G, and iron oxide.
[0017] One embodiment of the present invention is that the blast furnace iron smelting slag is modified by the following method before use: 10 to 18 parts of pseudo-boehmite are taken and added to 40 to 70 parts of water, followed by adding acid and continuously stirring for at least 10 minutes to form a pseudo-boehmite sol, followed by adding 150 to 200 parts of blast furnace iron smelting slag and stirring at 200 to 1000 r / min and 50 to 80°C for at least 10 minutes, and drying after the stirring is completed; the amount of acid added is 0.5 to 3 parts. The blast furnace iron smelting slag after the modification has better performance and the strength of the final floor is higher.
[0018] The beneficial effects of the present invention are: the composite inorganic floor material of the present invention has high compressive strength and high tensile strength, and the concrete floor of the present invention has a certain micro-expansion performance, and the micro-expansion rate within the maintenance period (28d) of the floor is relatively gentle. These conditions make the floor material of the present invention have good crack resistance. DETAILED DESCRIPTION
[0019] In order to have a clearer understanding of the technical features, purposes and beneficial effects of the present invention, the technical scheme of the present invention is described in detail below in conjunction with embodiments, but it should not be construed as limiting the applicable scope of the present invention.
[0020] In the following embodiments, unless otherwise specified, the operations described are routine operations in the art.
[0021] In the following examples, unless otherwise specified, all raw materials used are conventional commercial products in the art.
[0022] In the following examples, unless otherwise specified, the parts are by mass.
[0023] Example 1: Preparation of micro-expanding agent: Take 51 parts of lithium slag and 40 parts of red mud, crush them, stir to mix them, then add 22 parts of water, continue to stir to mix them, and then use a granulator to granulate them. The formed particles are placed in a sintering furnace, heated to 750°C and kept warm for 3 hours. After the insulation is completed, the sintered particles are naturally cooled to room temperature and then crushed to pass through a 20-mesh sieve.
[0024] Modification of blast furnace iron smelting slag: Take 15 parts of pseudo-boehmite and add it to 60 parts of water, stir to make it evenly dispersed, add 2.5 parts of concentrated hydrochloric acid under continuous stirring and continue stirring for 10 minutes. After the stirring is completed, add 180 parts of blast furnace iron smelting slag (passed through an 18-mesh sieve) and stir at 600r / min and 60°C for 15 minutes. After the stirring is completed, dry it.
[0025] The composition of the composite inorganic floor material: 40 parts of Portland cement (grade 42.5), 105 parts of aggregate (medium sand and fine sand in a mass ratio of 8:3.5), 20 parts of modified blast furnace iron smelting slag, 1.4 parts of basalt fiber, 7.5 parts of glass powder, 18 parts of titanium dioxide, and 14 parts of micro-expansion agent.
[0026] Example 2: Compared with Example 1, the difference is that the blast furnace iron smelting slag is not modified, and 6 parts of activator sodium hydroxide are added to the floor material, and the rest are the same.
[0027] Example 3: Preparation of micro-expanding agent: Take 54 parts of lithium slag and 44 parts of red mud, crush them, stir to mix them, then add 24 parts of water, continue to stir to mix them, and then use a granulator to granulate them. The formed particles are placed in a sintering furnace, heated to 780°C and kept warm for 3 hours. After the insulation is completed, the sintered particles are naturally cooled to room temperature and then crushed to pass through a 20-mesh sieve.
[0028] Modification of blast furnace iron smelting slag: Take 12 parts of pseudo-boehmite and add it to 60 parts of water, stir to make it evenly dispersed, add 1 part of concentrated sulfuric acid under continuous stirring and continue stirring for 15 minutes. After the stirring is completed, add 160 parts of blast furnace iron smelting slag and stir at 400r / min and 55°C for 30 minutes. After the stirring is completed, dry it.
[0029] The composition of the composite inorganic floor material: 32 parts of Portland cement (grade 42.5), 90 parts of aggregate (medium sand), 16 parts of modified blast furnace iron slag, 0.7 parts of basalt fiber, 6 parts of glass powder, and 11 parts of micro-expansion agent.
[0030] Example 4: Compared with Example 1, the difference is that the basalt fiber is replaced by polypropylene fiber, and the rest is the same.
[0031] Example 5: Compared with Example 1, the difference is that the particle size of blast furnace iron smelting slag is 2~5mm, and the rest is the same.
[0032] Comparative Example 1: Compared with Example 1, the difference is that SRM high performance concrete expansion agent (calcium oxide type) is used instead of the micro expansion agent, and the rest are the same.
[0033] Comparative Example 2: Compared with Example 1, the difference is that 14 parts of the micro-expansion agent are replaced by a mixture of 7.8 parts of lithium slag and 6.2 parts of red mud, and the rest are the same.
[0034] In order to further illustrate the advantages of the embodiments of the present invention, they are described below in conjunction with specific experimental data.
[0035] 1. Strength and water absorption test The floor compositions of Examples 1 to 7 and Comparative Examples 1 to 2 were added with water to prepare concrete floors, which were then cured at room temperature. The compressive strength and water absorption were measured at regular intervals. The final results are shown in Table 1. The test method is described in GB / T50081-2019 "Test Methods for Physical and Mechanical Properties of Concrete". When the concrete floor was prepared, the water-cement ratio was 0.33.
[0036] Table 1 Strength change and water absorption test results at different times
[0037] It can be seen from comparative document 1 that the floor composition of the embodiment of the present invention has high compressive strength, high tensile strength and low water absorption; at the same time, the concrete floor made from the floor composition of the embodiment of the present invention still has a considerable increase in strength after the curing age (28d).
[0038] 2. Micro expansion performance test Referring to GB50119-2013 "Technical Specifications for Application of Concrete Admixtures", the micro-expansion performance of the floor material compositions of Examples 1 to 5 and Comparative Examples 1 to 2 was tested, and the final results are shown in Table 2. Among them, when configured as a concrete floor, the water-cement ratio is 0.33; blank refers to a floor configured without adding a micro-expansion agent material.
[0039] Table 2 Compressive strength test table
[0040] It can be seen from Table 2 that the composite inorganic floor material according to the embodiment of the present invention has good micro-expansion performance.
[0041] Referring to Examples 1 to 5, it can be seen that the composite inorganic floor material of the embodiments of the present invention has a certain micro-expansion performance in the hardening stage of the floor, and the degree of micro-expansion is low, and it can continue to expand, which is manifested in that the difference in expansion rate after 14 days in water and after 14 days in water and then turning into air for 28 days is small, indicating that the composite inorganic floor material of the embodiments of the present invention can still continue to micro-expand in the air.
[0042] Referring to Example 1 and Comparative Example 1, it can be seen that compared with conventional expansion agents on the market, the expansion agent of the embodiment of the present invention has better performance, and the volume change rate of the floor in water and air is lower, thereby making the probability of micro cracks in the floor caused by shrinkage lower.
[0043] Referring to Example 1 and Comparative Example 2, it can be seen that although the lithium slag and red mud used alone have certain micro-expansion properties, the performance is relatively poor.
[0044] The above is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the embodiments of the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A composite inorganic floor material, characterized in that: In parts by mass, it includes: 30-50 parts of Portland cement, 80-120 parts of aggregate, 15-25 parts of blast furnace iron smelting slag, 0.5-2 parts of anti-cracking fiber, 5-10 parts of glass powder, and 10-15 parts of micro expansion agent; The preparation method of the micro-expanding agent comprises the following steps: taking 50-55 parts of lithium slag and 38-45 parts of red mud, crushing them, adding 20-25 parts of water, stirring them evenly, then granulating them, and then sintering them at 700-800°C for 2-4h, naturally cooling them to room temperature after the sintering, and then crushing them.
2. The composite inorganic floor material according to claim 1, characterized in that: The aggregate is medium sand.
3. The composite inorganic floor material according to claim 1, characterized in that: The aggregate is a mixture of medium sand and fine sand, and the mass ratio of the medium sand to the fine sand is 8:2-5.
4. The composite inorganic floor material according to claim 1, characterized in that: The particle size of the blast furnace iron smelting slag is not greater than 2 mm, and the floor material also includes 4 to 10 parts of an activator.
5. The composite inorganic floor material according to claim 1, characterized in that: The anti-cracking fiber is basalt fiber.
6. The composite inorganic floor material according to claim 4, characterized in that: The activator is at least one of sodium hydroxide, sodium carbonate and water glass.
7. The composite inorganic floor material according to claim 1, characterized in that: The floor material includes: 30-35 parts of silicate cement, 80-95 parts of aggregate, 15-20 parts of blast furnace iron smelting slag, 0.5-0.8 parts of anti-cracking fiber, 5-10 parts of glass powder, and 10-12 parts of micro-expansion agent.
8. The composite inorganic floor material according to claim 1, characterized in that: The floor material includes: 38 to 42 parts of silicate cement, 100 to 110 parts of aggregate, 18 to 22 parts of blast furnace iron smelting slag, 1 to 1.5 parts of anti-cracking fiber, 7 to 8 parts of glass powder, and 12 to 15 parts of micro-expansion agent.
9. The composite inorganic floor material according to claim 1, characterized in that: The floor material also includes 15 to 25 parts of inorganic pigments, and the inorganic pigment is at least one of titanium dioxide, phthalocyanine green G, and iron oxide.
10. The composite inorganic floor material according to claim 1, characterized in that: The blast furnace iron smelting slag is modified by the following method before use: 10-18 parts of pseudo-boehmite are taken and added to 40-70 parts of water, followed by adding acid and continuously stirring for at least 10 minutes to prepare pseudo-boehmite sol, followed by adding 150-200 parts of blast furnace iron smelting slag and stirring at 200-1000r / min and 50-80°C for at least 10 minutes, and drying after the stirring is completed; the amount of acid added is 0.5-3 parts.
Citation Information
Patent Citations
Compound concrete expanding agent
CN106348644A
Concrete expansion agent based on industrial waste and preparation method of concrete expansion agent
CN108793798A
Lithium slag concrete expansive agent
CN108911565A
Inorganic composite gel system
CN113372899A
Self-compacting terrace material
CN117466609A