Fireproof magnesium oxide board

By combining modified urea formaldehyde resin and foaming carbon catalyst, a fire-resistant and heat-retardant flame retardant with water absorption and expansion properties was prepared, which solved the problem of moisture absorption, halogenation and poor fire-retardant and heat-retardant properties of magnesium oxide sheets, and achieved Efficient and low-cost fire-resistant magnesium oxide sheet preparation significantly improves flame retardant and waterproof performance.

CN119080471APending Publication Date: 2024-12-06BEIJING GANGAN TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411295209.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-16
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing magnesium oxide sheets have poor moisture absorption, halogenation, embrittlement and fire insulation performance, which limits their application in the high-end market. Moreover, the compatibility and hygroscopic and hygroscopic properties of traditional phosphorus-nitrogen-type expanded flame retardant materials are insufficient. It affects the use and processing properties of materials.

Method used

The modified urea-formaldehyde resin is used to prepare a fire-resistant and heat-resistant flame retardant with water absorption and expansion properties. The chemical coating of the modified urea-formaldehyde resin and the combination of the carbon catalyst is used to prepare a particulate fire-resistant heat-resistant filler and pass through a screw Extrusion granulation and spray drying technology produce a granular flame retardant, which is blended with an appropriate amount of water and a water retention agent to form a fire-resistant magnesium oxide plate.

Benefits of technology

The long-term stable fire-resistant performance of fire-resistant magnesium oxide sheets is achieved, which reduces the preparation cost, simplifies process steps, improves production efficiency, and significantly improves the flame retardant and waterproof performance, avoiding the expensive and complex use of traditional emulsions.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a fireproof magnesium oxide board, which is prepared by mixing the following raw materials in parts by weight: 80-100 parts of magnesium oxide; 20 to 30 parts of anhydrous magnesium chloride; 10-20 parts of a fireproof heat-insulating flame retardant with water absorption performance and expansion performance; 20 to 30 parts of aluminum silicate fiber; 5 to 10 parts of sawdust; 10 to 15 parts of fly ash; 8-12 parts of glass magnesium board crushed powder; 1.5-5 parts of a non-woven fabric; 10 to 50 parts of water; wherein the fireproof heat-insulating flame retardant with the water absorption performance and the expansion performance is prepared from the following components: a component A: modified urea resin, a carbon source, a char forming catalyst, a foaming agent, titanium dioxide and a proper amount of water; the component B comprises a water-retaining agent and modified urea-formaldehyde resin, and the modified urea-formaldehyde resin is obtained by carrying out chemical coating modification on melamine modified urea-formaldehyde resin by utilizing polyacrylate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a plate material, in particular to a magnesium oxide plate material and a manufacturing process thereof. Background Art

[0002] Magnesium oxide board is a new type of multifunctional building material. Because it has the lightness, flexibility and reprocessing performance of wood-based organic boards, and the fire resistance and water resistance of inorganic boards, it is used in the decoration of walls, ceilings, floor linings and other parts with fire protection requirements. The main components of the current magnesium oxide board are glass fiber mesh cloth (the main source of the strength of the board), magnesium oxide, magnesium chloride, perlite, filling fiber and modified additives. However, the magnesium oxide board currently used has problems such as moisture absorption and halogen return of the board and embrittlement of the board, which affects the quality of the product, and the fireproof and heat-insulating performance is also poor, which limits the wide application of the product. Chinese patent application CN201310232377 attempts to use an expanded foaming material composed of melamine, pentaerythritol and ammonium polyphosphate, and obtains a certain flame retardant effect, but the flame retardant performance is difficult to meet the stringent requirements of the high-end market for flame retardant performance, such as a fire resistance limit value of greater than or equal to 4 hours.

[0003] Phosphorus-nitrogen intumescent flame retardant (IFR) is a new type of flame retardant material developed on the basis of flame retardant coatings, with phosphorus and nitrogen as the main components and no halogen. When the polymer material containing IFR is heated and burned, a carbon foam layer is formed on the surface, which can insulate heat, isolate oxygen, suppress smoke, and prevent molten droplet behavior, and has good resistance to long-term or repeated exposure to flames.

[0004] However, the IFR, like other flame retardant materials, has the disadvantages of poor compatibility with polymer materials and high hygroscopicity, which affects the performance and processing properties of the material. Therefore, how to perform surface treatment on the material, such as microencapsulation and surface coating of the material, is a topic of great concern to relevant personnel.

[0005] In response to the above-mentioned technical defects and market demand, the inventors have successfully developed a microencapsulated phosphorus-nitrogen intumescent flame retardant with a simple preparation process, low cost and certain moisture resistance, and a fireproof board prepared using the above flame retardant. In 2023, they applied for patent CN117534428A, and specifically disclosed a fireproof magnesium oxide board, which is made by mixing the following raw materials. The names and weight proportions of the raw materials are as follows: 80-100 parts of magnesium oxide; 20-30 parts of anhydrous magnesium chloride; 10-20 parts of a fireproof and heat-insulating flame retardant with water absorption and expansion properties; 20-30 parts of aluminum silicate fiber; 5-10 parts of sawdust; 10-15 parts of fly ash; 8-12 parts of glass magnesium board crushed powder; 1 non-woven fabric .5-5; 10-50 parts of water; wherein, the fireproof and heat-insulating flame retardant with water absorption and expansion properties is prepared from the following components: component A: elastic waterproof emulsion A, carbon source, carbon-forming catalyst, foaming agent, titanium dioxide, elastic waterproof emulsion B and appropriate amount of water; component B: water retaining agent. The fireproof magnesium oxide sheet has excellent moisture resistance and good flame retardancy. However, in actual production, in order to best balance moisture resistance and fire resistance, the waterproof elastic emulsion A is preferably imported from Germany Wacker EZ3066 emulsion as a binder for flame retardant particles. The emulsion is a VAE emulsion specially developed by Wacker for intumescent fire retardant coatings. Compared with other waterproof elastic emulsions, it has good foam expansion and foam stability. Generally speaking, the waterproofness of VAE emulsion is significantly inferior to that of acrylic emulsion and polyurethane emulsion. Even if the waterproofness of EZ3066 is slightly inferior to that of acrylic emulsion and polyurethane emulsion, it is significantly better than the general similar EVA emulsion. In order to further improve the waterproofness and prevent the expansion of the flame retardant from being inhibited, an elastic waterproof emulsion B represented by Emultex FR 797 needs to be sprayed on the surface of the semi-finished granular flame retardant. The above technical improvements make the above flame retardant have both moisture resistance and flame retardancy, but it is necessary to use an expensive imported special emulsion for intumescent fire retardant coatings, which is costly and requires the use of the emulsion twice, and the preparation process is complicated. Therefore, the market is in urgent need of a fireproof magnesium oxide sheet with a simple preparation process, low cost, moisture resistance and flame retardancy. Summary of the invention

[0006] The invention provides a fireproof magnesium oxide plate, which has long-term stable fireproof performance and is characterized in that the fireproof magnesium oxide plate is prepared by mixing the following raw materials, the raw materials having the following names and weight proportions: 80-100 parts of magnesium oxide; 20-30 parts of anhydrous magnesium chloride; 10-20 parts of a fireproof heat-insulating flame retardant having water absorption performance and expansion performance; 20-30 parts of aluminum silicate fiber; 5-10 parts of sawdust; 10-15 parts of fly ash; 8-12 parts of glass magnesium plate crushed powder; 1.5-5 parts of non-woven fabric; and 10-50 parts of water, wherein the fireproof heat-insulating flame retardant having water absorption performance and expansion performance is prepared from the following components: Component A: modified urea-formaldehyde resin, carbon source, carbon-forming catalyst, foaming agent, titanium dioxide and appropriate amount of water; Component B: water retaining agent; wherein, in component A, the weight ratio of modified urea-formaldehyde resin, carbon source, carbon-forming catalyst, foaming agent and titanium dioxide is (1-2):(4-8):(1-3):(1-3):(1-3); the carbon source is pentaerythritol, dipentaerythritol or tripentaerythritol; the carbon-forming catalyst is ammonium polyphosphate; the foaming agent is dicyandiamide, ammonium oxalate, urea or hexamethylenetetramine; wherein the modified urea-formaldehyde resin is obtained by chemically coating and modifying melamine-modified urea-formaldehyde resin with polyacrylate; the flame retardant preparation method is: (1) Add the carbon source, carbon-forming catalyst, foaming agent and titanium dioxide into a grinder in proportion for grinding and dispersion; (2) adding the powder mixed in step (1), modified urea-formaldehyde resin and water into a high-speed mixer for mixing; (3) subjecting the mixture obtained in step (2) to screw extrusion granulation or spray drying granulation, and then drying to obtain a granular fireproof and heat-insulating filler A; (4) The fireproof and heat-insulating filler A obtained in step (3) is blended with a granular water-retaining agent to obtain a final product, a fireproof and heat-insulating flame retardant.

[0007] The manufacturing process of the modified urea-formaldehyde resin adopts an alkali-acid-alkali process, which specifically includes the following steps: (1) Add a certain mass of formaldehyde solution into the reactor, add a certain amount of deionized water, then adjust the pH to 7.5-9.0 with sodium hydroxide aqueous solution, and heat to 40-55°C, then add the first batch of urea and the first batch of melamine under stirring conditions, heat to 85-95°C and keep the temperature for 20-40 minutes or heat to 70-75°C and keep the temperature for 50-80 minutes; (2) Adjust the pH to 5.0-5.5 with formic acid, raise the temperature to 80-95°C, continue to keep the temperature for a period of time, and finally cool the reactants to 65-75°C, adjust the pH to 7.0-7.5 with sodium hydroxide aqueous solution, add the second batch of urea and the second batch of melamine, stir evenly, and keep the temperature for 20-40 minutes; (3) After cooling to a certain temperature, add the third batch of urea, keep the temperature at 70-90°C for 10-40 minutes, and then adjust the pH value to 8.0-9.0 to obtain a basic modified urea-formaldehyde resin; (4) adding a pre-prepared mixture of isocyanate acrylate, acrylate and ester solvent while stirring, and reacting for 15-25 minutes; wherein the sum of the amounts of isocyanate acrylate and acrylate is 5-10wt% based on the basic modified urea-formaldehyde resin; (5) Add 5-10wt% of tris(2-hydroxyethyl)isocyanurate triacrylate (THEICTA) and acrylate mixture with stirring, the mass ratio of the two is (2-4):1; (6) Add initiator solution, raise the temperature to 50-90°C, and react for 0.4-3.5 hours to obtain modified urea-formaldehyde resin.

[0008] In steps (1) to (3), the cumulative molar ratio of formaldehyde to (urea + melamine) is 1.05-1.15; In step (2), the reaction is continued at a temperature of 16 to 20 seconds (Tu-4 cup, 30°C test) and then the reactants are cooled to 65 to 75°C. The weight ratio of isocyanate acrylate to acrylate in step (4) is (3-5): 1 In step (4), the isocyanate acrylate may be ethyl isocyanate acrylate or ethyl isocyanate methacrylate; The ester solvent in step (4) includes one or more of ethyl acetate, octyl acetate, and n-butyl acetate.

[0009] In step (4), the acrylate may be methyl (meth)acrylate, ethyl (meth)acrylate, or butyl (meth)acrylate; In step (5), the acrylate may be methyl (meth)acrylate, ethyl (meth)acrylate, or butyl (meth)acrylate; In step (6), the initiator is one or more of sodium persulfate, azobisisobutyronitrile, dibenzoyl peroxide, tert-butyl perbenzoate, di-tert-butyl peroxide, diisopropylbenzene peroxide, and di-tert-amyl peroxide; The manufacturing process of the fireproof magnesium oxide sheet material is characterized by comprising the following steps: (1) Put magnesium oxide, anhydrous magnesium chloride, flame retardant, and glass magnesium board powder into a blender according to the weight of the magnesium oxide board, and stir. At the same time, fill the blender with gas to form bubbles, and stir for 15 minutes; (2) Add aluminum silicate fiber, fly ash, sawdust and the magnesium oxide board in the same weight proportion into a mixer, continue to stir and mix, and stir evenly for 30 minutes to make a slurry. (3) Introduce the prepared template into the press and lay the non-woven fabric; (4) Take out the slurry in step (2) and add it to the hopper of the press, then fill the slurry into the template seamless cloth, press it to the required size, and demold it after drying for 8-10 hours; (5) Place the cured sheet together with the template in reverse, gently lift one corner of the mold with your hand, and the cured sheet will fall off when pressed by your hand. Then, start from this corner to remove one side and lift up the mold; (6) Stack the plates after forming the mold together, cure them in the curing room for 3 days, and then place the products in a dry room for 10 days; (7) Then cut the four sides of the dried board according to the specifications.

[0010] The grinding and dispersing time is 1-2 hours.

[0011] Wherein, the high-speed mixer in step (2) is a high-speed kneader or a high-speed disperser.

[0012] Wherein, the mass ratio of the thermal insulation filler A to the granular water-retaining agent in step (4) is (2-3):1.

[0013] Among them, the water retaining agent is a polyacrylic acid water retaining agent.

[0014] Wherein, the degree of polymerization of ammonium polyphosphate is greater than 600 and less than 1000.

[0015] After adopting the above technical solution, the present invention has at least the following beneficial effects: (1) The present invention adopts modified urea-formaldehyde resin to replace imported EZ3066 emulsion, Emultex FR 797, etc., to achieve excellent moisture-proof performance and relatively close flame retardant performance, greatly reducing the manufacturing cost of preparing fire-proof heat-insulating flame retardants and fire-proof magnesium oxide boards with water absorption and expansion properties.

[0016] (2) Due to the use of the special modified urea-formaldehyde resin of the present invention, it not only has excellent foaming performance, but also has excellent waterproof performance. Due to VAE emulsion, the inventors found that the step of spraying elastic waterproof emulsion B to coat the granular flame retardant to form a capsule structure can be omitted, while maintaining the original fireproof performance, simplifying the process steps, and improving the production efficiency and cost of the factory. At the same time, from the comparison of magnesium oxide plate A and magnesium oxide plate B, it can be seen that the flame retardant performance of the self-made modified urea-formaldehyde resin instead of EZ3066 emulsion has not decreased significantly even without coating. From the comparison of magnesium oxide plate A and magnesium oxide plate D, it can be seen that due to the excellent waterproofness of the modified urea-formaldehyde resin and its own self-expansion performance, its flame retardant performance is also quite excellent after omitting the overall coating step.

[0017] (3) When preparing modified urea-formaldehyde resin, among many types of acrylate monomers, tris(2-hydroxyethyl)isocyanurate triacrylate (THEICTA) was finally selected after a large number of experiments. While achieving the waterproofing effect of acrylic polymer coating, it also has the effect of foaming into carbon. It is speculated that this may be due to its nitrogen-containing characteristics, which avoids the acrylic resin with too low nitrogen content outside the urea-formaldehyde resin from inhibiting foaming into carbon.

[0018] (4) When preparing the modified urea-formaldehyde resin, the pre-prepared mixture of isocyanate acrylate, acrylate and ester solvent mixture is used in step (4). On the one hand, the slow side reaction of isocyanate acrylate with water is reduced. On the other hand, by dispersing the isocyanate acrylate in the acrylate and ester solvents, the local high cross-linking between the isocyanate acrylate and the urea-formaldehyde resin is avoided, which is conducive to the uniform coating of the isocyanate acrylate. Finally, the acrylate added together as a dispersion medium also increases the reaction response speed of the subsequent free radical copolymerization of the acrylate and the acrylic functional group in the isocyanate.

[0019] (5) When preparing the modified urea-formaldehyde resin, the outer coating is made of a mixture of tris(2-hydroxyethyl)isocyanuric acid triacrylate (THEICTA) and acrylates, which avoids the high cross-linking of THEICTA due to its three functional groups, which will increase the decomposition temperature and thus mismatch the decomposition and dehydration carbonization temperature of the intumescent flame retardant in the fireproof material, and even inhibit the early dehydration and foaming. Some acrylates can significantly reduce the cross-linking density, and while improving the bonding performance of the film-forming material, the effect of improving the foaming performance can be maintained.

[0020] (6) When preparing modified urea-formaldehyde resin, the amount of isocyanate acrylate should be appropriate. If it is too little, the coating effect is poor, and the effect of improving the waterproof effect and fire resistance is insufficient. If it is too much, isocyanate will consume a large amount of amino groups and even hydroxyl groups inside the urea-formaldehyde resin, and the hydroxyl content determines the dehydration and foaming rate of the urea-formaldehyde resin. Therefore, the amount of isocyanate acrylate should be appropriate.

[0021] The technical solution of the invention is described in detail below in conjunction with specific embodiments. Example 1

[0022] The preparation method of fireproof and heat-insulating flame retardant A having water absorption and expansion properties comprises the following steps: (1) Add pentaerythritol as a carbon source, ammonium polyphosphate as a carbon-forming catalyst, dicyandiamide as a foaming agent, and titanium dioxide in a mass ratio of 4 kg: 2 kg: 2 kg: 2 kg into a grinder and grind and disperse for 1.5 hours.

[0023] (2) Add the powder mixed in step (1), the modified urea-formaldehyde resin and water into a high-speed mixer for mixing; the masses of the modified urea-formaldehyde resin and water are 1.5 kg and 0.5 kg respectively. The high-speed mixer is a high-speed kneading machine.

[0024] (3) subjecting the mixture obtained in step (2) to screw extrusion granulation, and then drying to obtain a granular fireproof and heat-insulating filler A; (4) the fireproof and heat-insulating filler obtained in step (3) was blended with a granular polyacrylic acid water-retaining agent in a mass ratio of 2:1 to obtain a final product, a fireproof and heat-insulating flame retardant A; The modified urea-formaldehyde resin used in step (2) is prepared by an alkali-acid-alkali process, comprising the following steps: (1) Add a certain mass of 4.05 kg (48.6 moles) of formaldehyde solution (36%) into the reactor, add a certain amount of deionized water, then adjust the pH to 8.0 with 30% sodium hydroxide aqueous solution, and heat to 50°C. Then, add the first batch of urea 0.8 kg and the first batch of melamine 0.315 kg under stirring conditions, raise the temperature to 95°C and keep the temperature for 30 minutes; (2) Adjust the pH to 5.0 with 10 wt% formic acid, raise the temperature to 95°C, and continue to keep the temperature to react until the system viscosity reaches 18s (apply 4 cups, test at 30°C). Finally, cool the reactants to 70°C, adjust the pH to 7.0 with sodium hydroxide aqueous solution, add 1.0 kg of the second batch of urea and 0.315 kg of the second batch of melamine, stir evenly, and keep the temperature to react for 30 minutes; (3) After cooling to a certain temperature, add 0.6 kg of the third batch of urea, keep the temperature at 70°C for 20 minutes, cool to 40°C, and then adjust the pH value to 8.0 to obtain a basic modified urea-formaldehyde resin; (4) Add 0.354 kg of a mixture of ethyl isocyanate acrylate and ethyl acrylate (5 wt % based on urea-formaldehyde resin) and 0.708 kg of ethyl acetate while stirring. The mass ratio of ethyl isocyanate acrylate to ethyl acrylate is 4:1.

[0025] (5) Add tris(2-hydroxyethyl)isocyanurate triacrylate (THEICTA) and ethyl acrylate (0.354 kg) in a mass ratio of 2:1. (6) Add initiator solution, raise the temperature to 70°C, and react for 2 hours to obtain modified urea-formaldehyde resin. Example 2

[0026] The preparation method of fireproof and heat-insulating flame retardant B comprises the following steps: (1) Add pentaerythritol as a carbon source, ammonium polyphosphate as a carbon-forming catalyst, dicyandiamide as a foaming agent, and titanium dioxide in a mass ratio of 4kg:2kg:2kg:2kg into a grinder and grind and disperse for 1.5 hours.

[0027] (2) The powder, elastic waterproof emulsion A and water mixed in step (1) are added into a high-speed mixer for mixing; the masses of the elastic waterproof emulsion A and water are 1 kg and 0.5 kg respectively, and the elastic waterproof emulsion A is EZ3066 emulsion. The high-speed mixer is a high-speed kneading machine.

[0028] (3) subjecting the mixture obtained in step (2) to screw extrusion granulation to obtain a granular flame retardant semi-finished product; (4) The granular flame retardant semi-finished product obtained in step (3) is placed in a disperser and stirred, and 0.5 kg of elastic waterproof emulsion B (Emultex FR 797) is sprayed on it, and then dried to obtain fireproof and heat-insulating filler A. The dispersion stirring speed is 400 r / min. (5) The fireproof and heat-insulating flame retardant obtained in step (4) is blended with a granular polyacrylic acid water-retaining agent in a mass ratio of 2:1 to obtain a final product, fireproof and heat-insulating flame retardant B. Example 3

[0029] (1) Add carbon source pentaerythritol, carbon-forming catalyst ammonium polyphosphate, foaming agent dicyandiamide, and titanium dioxide in a mass ratio of 4kg:2kg:2kg:2kg into a grinder for grinding and dispersion for 1.5 hours, and then add 5kg of granular polyacrylic acid water-retaining agent for blending, with a mass ratio of 2:1 to obtain the final product, fireproof and heat-insulating flame retardant C; Example 4

[0030] On the basis of Example 2, step (4) is omitted to obtain a fireproof and heat-insulating flame retardant D. Example 5

[0031] On the basis of Example 2, in step (1), 8 kg of expandable graphite and 2 kg of titanium dioxide were added to a grinder for grinding and dispersion for 1.5 hours, and the other preparation steps were the same to obtain flame retardant E. Example 6

[0032] The fireproof magnesium oxide board is prepared from the following raw materials: 90kg magnesium oxide; 25kg anhydrous magnesium chloride; 15kg fireproof and heat-insulating flame retardant with water absorption and expansion properties; 25kg aluminum silicate fiber; 8kg sawdust; 12kg fly ash; 10 parts of glass magnesium board crushed powder; 5kg non-woven fabric; 30kg water. The specific preparation process is as follows: (1) Put magnesium oxide, anhydrous magnesium chloride, flame retardant, and glass magnesium board powder into a blender according to the weight of the magnesium oxide board, and stir. At the same time, fill the blender with gas to form bubbles, and stir for 15 minutes; (2) Add aluminum silicate fiber, fly ash and sawdust according to the weight of the magnesium oxide board into a mixer, continue to stir and mix, and stir evenly for 30 minutes to make a slurry. (3) Then introduce the prepared template into the press and lay the non-woven fabric; (4) Take out the slurry in step (2) and add it to the hopper of the press, then fill the slurry into the template seamless cloth, press it to the required size, and demold it after drying for 8-10 hours; (5) Place the cured sheet together with the template in reverse, gently lift one corner of the mold with your hand, and the cured sheet will fall off by pressing it. Then, start from this corner to remove one side and lift up the mold; (6) Stack the molded plates together, cure them in a curing room for 3 days, and then place the products in a dry room for 10 days; (7) Then cut the four sides of the dried board according to the specification requirements. Among them, the fireproof and heat-insulating flame retardants A, B, C, D and E with water absorption and expansion properties prepared in Examples 1-6 are used to obtain fireproof magnesium oxide boards A, B, C, D and E.

[0033] Fire performance test According to GB50045-95, the fire resistance limit (hours) is tested. If any of the following conditions occurs, the specimen reaches the fire resistance limit. Loss of stability: The axial deformation of the column member is greater than h / 100 (mm) or the axial deformation rate is greater than 3h / 1000 (mm / min). h is the initial fire height of the column member after loading and before the fire resistance test, unit: mm.

[0034] Sample type Flame retardant type Fire resistance Magnesium oxide sheet A Flame retardant A 5.0h Magnesium oxide sheet B Flame retardant B 5.4h Magnesium Oxide Sheet C Flame retardant C 3.6h Magnesium oxide sheet D Flame retardant D 4.5h Magnesium Oxide Sheet E Flame retardant E 3h It can be seen that the flame retardant properties of the fireproof magnesium oxide board with the addition of flame retardants modified by special processes have been greatly improved.

Claims

1. A fireproof magnesium oxide plate, characterized in that: The following raw materials are mixed and the names and weight proportions of the raw materials are as follows: 80-100 parts of magnesium oxide; 20-30 parts of anhydrous magnesium chloride; 10-20 parts of fireproof and heat-insulating flame retardant with water absorption and expansion properties; 20-30 parts of aluminum silicate fiber; 5-10 parts of sawdust; 10-15 parts of fly ash; 8-12 parts of glass magnesium board crushed powder; 1.5-5 parts of non-woven fabric; 10-50 parts of water, wherein the fireproof and heat-insulating flame retardant with water absorption and expansion properties is prepared from the following components: Component A: modified urea-formaldehyde resin, carbon source, carbon-forming catalyst, foaming agent, titanium dioxide and appropriate amount of water; Component B: water retaining agent; wherein, in component A, the weight ratio of modified urea-formaldehyde resin, carbon source, carbon-forming catalyst, foaming agent and titanium dioxide is (1-2):(4-8):(1-3):(1-3):(1-3); the carbon source is pentaerythritol, dipentaerythritol or tripentaerythritol; the carbon-forming catalyst is ammonium polyphosphate; the foaming agent is dicyandiamide, ammonium oxalate, urea or hexamethylenetetramine; wherein the modified urea-formaldehyde resin is obtained by chemically coating and modifying melamine-modified urea-formaldehyde resin with polyacrylate; the flame retardant preparation method is: (1) Add the carbon source, carbon-forming catalyst, foaming agent and titanium dioxide into a grinder in proportion for grinding and dispersion; (2) adding the powder mixed in step (1), modified urea-formaldehyde resin and water into a high-speed mixer for mixing; (3) subjecting the mixture obtained in step (2) to screw extrusion granulation or spray drying granulation, and then drying to obtain a granular fireproof and heat-insulating filler A; (4) blending the fireproof and heat-insulating filler A obtained in step (3) with a granular water-retaining agent to obtain a final product, a fireproof and heat-insulating flame retardant; The manufacturing process of the modified urea-formaldehyde resin adopts an alkali-acid-alkali process, which specifically includes the following steps: ① Add a certain mass of formaldehyde solution into the reactor, add a certain amount of deionized water, then adjust the pH to 7.5-9.0 with sodium hydroxide aqueous solution, and heat to 40-55°C, then add the first batch of urea and the first batch of melamine under stirring conditions, heat to 85-95°C and keep the temperature for 20-40 minutes or heat to 70-75°C and keep the temperature for 50-80 minutes; ② Use formic acid to adjust the pH to 5.0-5.5, raise the temperature to 80-95°C, continue to keep the temperature for a period of time, finally cool the reactants to 65-75°C, adjust the pH to 7.0-7.5 with sodium hydroxide aqueous solution, add the second batch of urea and the second batch of melamine, stir evenly, and keep the temperature for 20-40 minutes; ③ After cooling to a certain temperature, add the third batch of urea, keep the temperature at 70-90°C for 10-40 minutes, and then adjust the pH value to 8.0-9.0 to obtain a basic modified urea-formaldehyde resin; ④ Add the pre-made mixture of isocyanate acrylate, acrylate and ester solvent while stirring, and react for 15-25 minutes; wherein, based on the basic modified urea-formaldehyde resin, the sum of the amount of isocyanate acrylate and acrylate is 5-10wt%; ⑤ Add 5-10wt% of tris(2-hydroxyethyl)isocyanurate triacrylate (THEICTA) and acrylate mixture with a mass ratio of (2-4):1 to the basic modified urea-formaldehyde resin while stirring; ⑥ Add initiator solution, raise the temperature to 50-90°C, and react for 0.4-3.5 hours to obtain modified urea-formaldehyde resin.

2. The fireproof magnesium oxide sheet according to claim 1, characterized in that: In step (1), the grinding and dispersion time is 1-2 hours.

3. The fireproof magnesium oxide sheet according to claim 1, characterized in that: In step (2), the high-speed mixer is a high-speed kneader or a high-speed disperser.

4. The fireproof magnesium oxide sheet according to claim 1, characterized in that: In steps ①-③, the cumulative molar ratio of formaldehyde / (urea+melamine) is 1.05-1.

15.

5. The fireproof magnesium oxide sheet according to claim 1, characterized in that: The isocyanate acrylate is isocyanate ethyl acrylate or isocyanate ethyl methacrylate.

6. The fireproof magnesium oxide sheet according to claim 1, characterized in that: The mass ratio of the heat-insulating filler A to the granular water-retaining agent in step (4) is (2-3):

1.

7. The fireproof magnesium oxide sheet according to claim 1, characterized in that: The water retaining agent is a polyacrylic acid water retaining agent.

8. The fireproof magnesium oxide sheet according to claim 1, characterized in that: The degree of polymerization of ammonium polyphosphate is greater than 600 and less than 1000.

9. The fireproof magnesium oxide sheet according to claim 1, characterized in that: In step ②, the reaction was continued at a temperature of 16 to 20 seconds until the viscosity of the system reached 16 to 20 seconds, and the reactants were finally cooled to 65 to 75°C. The test conditions were 30°C and the Tu-4 cup test was used.

10. The fireproof magnesium oxide sheet according to claim 1, characterized in that: In step ④, the weight ratio of isocyanate acrylate to acrylate is (3-5):1.