Silicon carbide powder, preparation method thereof and preparation method of silicon carbide green body
By adding phenolic resin-based curing agent and nanocarbon black to silicon carbide powder, printing with sand-type additive manufacturing equipment and drying and impregnating, the problem of low silicon carbide blank in the existing technology is solved, and high The preparation of silicon carbide products with density and low residual carbon enhances mechanical properties and temperature resistance, and is suitable for the production of complex structures and large-size materials.
Patent Information
- Application Number
- CN202411204088.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-06
AI Technical Summary
The prior art is difficult to prepare large-size silicon carbide ceramic products with high density and complex structures, and the silicon carbide blanks sprayed by binder are low in density and low carbon content, resulting in poor mechanical properties and temperature resistance, which is difficult to meet the aerospace, Application requirements in energy and chemical fields.
A mixture of silicon carbide powder with a particle size of 10μm-135μm is used, combined with phenolic resin-based curing agent and nanocarbon black, and printed through sand-type additive manufacturing equipment and binder jetting technology. After drying and impregnation, silicon carbide powder is improved. The humidity and density of the silicon carbide green body with high density and low residual carbon is formed.
It realizes high-density, low residual carbon silicon carbide products, improves mechanical properties and temperature resistance, simplifies production processes, reduces costs and production difficulties, and reduces free silicon content. It is suitable for complex structures and large-size silicon carbide materials. Preparation.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of silicon carbide, and in particular to a silicon carbide green body. Background Art
[0002] As an important ceramic material, silicon carbide is not only used in traditional industrial fields such as high-temperature kiln tools, combustion nozzles, heat exchangers, sealing rings, and sliding bearings, but also as bulletproof armor materials, space reflectors, semiconductor wafer preparation components, and nuclear fuel cladding materials due to its excellent high-temperature mechanical strength, high hardness, high elastic modulus, high wear resistance, high thermal conductivity, and corrosion resistance. At present, simple silicon carbide products are mostly made by mold forming, which is suitable for the preparation of simple structures such as silicon carbide tubes and silicon carbide rods, but cannot be used to prepare complex structures, large sizes, and special-shaped silicon carbide products.
[0003] At present, for heterogeneous silicon carbide ceramic products with complex structures, they are mainly prepared and formed by 3D printing. There are two actual industrial application technologies, namely selective laser sintering technology and binder jetting technology. The selective laser sintering technology has low printing efficiency, low density of printed green bodies, long post-processing cycle, high cost, and is not suitable for printing large-size silicon carbide bodies; the silicon carbide ceramic body printed by binder jetting 3D printing has low density. After reaction sintering, the gaps in the body are filled with silicon to form free residual silicon. The silicon carbide ceramics prepared in this way have poor mechanical properties, temperature resistance and corrosion resistance. Compared with silicon carbide, silicon has a low melting point, low density, and is easily dissolved by strong acids. It is difficult to meet the application requirements of aerospace, energy and chemical, and mechanical industries. Summary of the invention
[0004] In view of the problems of poor mechanical properties, poor temperature resistance and poor corrosion resistance of silicon carbide products caused by low body density and low carbon content in the silicon carbide body made by the binder injection technology, it is necessary to propose a silicon carbide powder and a preparation method thereof and a preparation method of silicon carbide green body to prepare silicon carbide products with high density, low residual carbon and excellent mechanical properties.
[0005] A silicon carbide powder is a mixture of two or three of silicon carbide powder with a particle size of 10μm-15μm and a purity of ≥99.5%, silicon carbide powder with a particle size of 28μm-35μm and a purity of ≥99.5%, silicon carbide powder with a particle size of 45μm-50μm and a purity of ≥99.5%, silicon carbide powder with a particle size of 90μm-110μm and a purity of ≥99.5%, and silicon carbide powder with a particle size of 120μm-135μm and a purity of ≥99.5%. Specifically, silicon carbide powder with a particle size of 90μm-110μm and silicon carbide powder with a particle size of 120μm-135μm are set as coarse-particle silicon carbide powder; silicon carbide powder with a particle size of 10μm-15μm, silicon carbide powder with a particle size of 28μm-35μm and silicon carbide powder with a particle size of 45μm-50μm are set as fine-particle silicon carbide powder.
[0006] Preferably, in order to make the density of the silicon carbide powder product denser and the pores between particles smaller, the silicon carbide powder is silicon carbide shaping powder.
[0007] Preferably, the humidity of the silicon carbide powder reaches a state where the silicon carbide powder can be easily kneaded into a ball, thereby ensuring that the silicon carbide powder does not generate dust during use and avoiding environmental problems of excessive suspended particles in the air caused by the powder entering the air.
[0008] A method for preparing silicon carbide powder, comprising:
[0009] S01, placing the selected coarse-grained silicon carbide powder into a preparation container, adding a curing agent into the preparation container, and stirring the two for 30s-90s. Preferably, the amount of the curing agent added is sufficient to ensure that dust does not appear during the stirring and mixing process, and the curing agent is used to react with the binder to form the product;
[0010] S02, selecting fine-grained silicon carbide powder and placing it in the preparation container, stirring for 60s-120s to uniformly mix the mixture in S01 and the fine-grained silicon carbide powder;
[0011] S03. According to the dust situation during the stirring process in S02, the curing agent is gradually added to the preparation container, and stirring is continued for 30s-90s to further increase the humidity of the silicon carbide powder, until the moisture content of the silicon carbide powder is 0.18%-0.25%, that is, the silicon carbide powder reaches a humidity state that can be squeezed into a ball by hand, and the preparation of the silicon carbide powder is completed.
[0012] The silicon carbide powder with a moisture content of 0.18%-0.25% is more suitable for sand-type additive manufacturing equipment, and can effectively ensure that the silicon carbide powder will not block the laying mechanism, thereby effectively improving the printing efficiency and printing quality.
[0013] Preferably, the curing agent may be a phenolic resin curing agent.
[0014] A method for preparing a green body of a silicon carbide product, comprising:
[0015] S11, printing, based on the sand-type additive manufacturing equipment, using the binder jetting technology to print the silicon carbide green body; specifically, adding the silicon carbide powder to the powder laying mechanism of the sand-type additive manufacturing equipment, using the silicon carbide powder to lay each layer of the product, and the laying time of each layer is 30min-60min to ensure the density of the powder laying surface; a phenolic resin binder is provided in the print head of the sand-type additive manufacturing equipment, and the phenolic resin is sprayed on the powder laying surface as a binder, and reacts with the curing agent mixed in the silicon carbide powder to solidify the contour of each layer of the powder laying surface product;
[0016] S12, drying, baking the printed silicon carbide green body at a temperature of 100° C.-200° C. for 1 h-4 h, so that the curing agent and the binder in the silicon carbide green body react completely, and the water in the pores of the green body evaporates completely, so that the pores of the green body are all opened and retained;
[0017] S13, impregnation, placing the baked silicon carbide green body into the prepared impregnation liquid, and ensuring that it is impregnated for 1h-5h at a pressure of 25kPa, and then drying again to obtain a silicon carbide green body with high residual carbon and high density.
[0018] Preferably, in S11, the amount of the binder added to each silicon carbide product is 5%-20% of the weight of the silicon carbide product, so that a firm bond can be achieved.
[0019] Preferably, in S11, the thickness of each powdering layer is 0.15mm-0.32mm, which ensures that each powdering layer can be penetrated by the adhesive spray to achieve full-thickness bonding without the powdering layer being unable to solidify due to excessive thickness.
[0020] The solid density of the silicon carbide green body printed in this way is ≥2.1g / cm 3 , effectively improving the printing density of silicon carbide green bodies.
[0021] Preferably, the preparation method of the impregnation liquid comprises first selecting 50%-80% of a phenolic resin having a carbon content higher than 50% and 50%-20% of ethanol for mixing, then adding 3%-10% of an organic dye dispersant accounting for the weight of the impregnation liquid, then adding 25%-60% of nano carbon black accounting for the weight of the impregnation liquid, and finally stirring for 3h-6h to obtain the impregnation liquid for standby use.
[0022] The beneficial effects of the technical solution of the present invention are as follows: the problems of low density and low carbon content of large-sized and complex-structured silicon carbide green bodies are solved, and the step of pre-adding a carbon source to silicon carbide powder is omitted, thereby simplifying the production process, improving production efficiency, and reducing production difficulty and production cost; at the same time, the content of free silicon in reaction-sintered silicon carbide products is effectively reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] none. DETAILED DESCRIPTION
[0024] In order to more clearly illustrate the technical solution of the present invention, the following description is some typical embodiments of the present invention. For ordinary technicians in this field, other solutions can be obtained based on these embodiments without paying any creative work.
[0025] In one embodiment, the silicon carbide powder can be used to make high-strength and high-density silicon carbide products, and its components include two or three of silicon carbide powder with a particle size of 10μm-15μm and a purity of ≥99.5%, silicon carbide powder with a particle size of 28μm-35μm and a purity of ≥99.5%, silicon carbide powder with a particle size of 45μm-50μm and a purity of ≥99.5%, silicon carbide powder with a particle size of 90μm-110μm and a purity of ≥99.5%, and silicon carbide powder with a particle size of 120μm-135μm and a purity of ≥99.5%. In this embodiment, silicon carbide powder with a particle size greater than or equal to 90μm is defined as coarse-grained silicon carbide powder, and silicon carbide powder with a particle size less than 90μm is defined as fine-grained silicon carbide powder.
[0026] As a supplement to the present embodiment, the silicon carbide powder with a particle size of 10 μm-15 μm and a purity of ≥99.5%, the silicon carbide powder with a particle size of 28 μm-35 μm and a purity of ≥99.5%, the silicon carbide powder with a particle size of 45 μm-50 μm and a purity of ≥99.5%, the silicon carbide powder with a particle size of 90 μm-110 μm and a purity of ≥99.5%, and the silicon carbide powder with a particle size of 120 μm-135 μm and a purity of ≥99.5% are all silicon carbide shaping powders, which effectively reduces the pore size of silicon carbide products and improves the density of silicon carbide products.
[0027] As a supplement to this embodiment, in order to prevent the silicon carbide powder of the present invention from raising dust into the environment during use, the moisture content of the silicon carbide powder is 0.18%-0.25%. Specifically, the silicon carbide powder is in a humidity state that can be easily kneaded into a ball. And the silicon carbide powder in this humidity state can also effectively ensure that the powder spreading device of the additive manufacturing equipment is not easily blocked, and dust and other problems will not occur during the powder spreading process.
[0028] In another embodiment, a method for preparing the silicon carbide powder having a high bulk density comprises:
[0029] S101, selecting 65 parts of coarse-grained silicon carbide powder with a particle size of 90 μm-110 μm and adding them to a sand mixing tank, then adding a curing agent with a mass ratio of 3% of the coarse-grained silicon carbide powder to the sand mixing tank, and stirring at a high speed for 60 seconds;
[0030] S102, selecting 35 parts of fine-grained silicon carbide powder with a particle size of 10 μm-15 μm, adding it to the sand mixing tank, and stirring at high speed for 120 seconds to ensure that the three components are fully and evenly mixed;
[0031] S103, according to the dust situation during the mixing process of S102, add a curing agent with a mass ratio of 3.5% of the silicon carbide powder with a particle size of 10μm-15μm to the sand mixing tank again, and stir at high speed for 60s to fully mix the added curing agent with the components in the sand mixing tank, and make the humidity of the available silicon carbide powder obtained in the sand mixing tank reach a humidity state that can be kneaded and agglomerated, thereby completing the preparation of the silicon carbide powder.
[0032] As a supplement to this embodiment, a method for preparing a silicon carbide product using the silicon carbide powder includes:
[0033] S111, printing, the silicon carbide product is printed by 3D printing sand mold additive manufacturing equipment in this embodiment; specifically, the prepared silicon carbide powder is added into the powder spreading mechanism of the sand mold additive manufacturing equipment, and the laying time of each layer is 40 minutes to ensure the density of the powder spreading surface; a phenolic resin binder is installed in the print head of the additive manufacturing equipment, and the binder is sprayed at the corresponding product position according to the layer information to solidify the contour of the product on each layer of the powder spreading surface;
[0034] S112, drying, baking the green body of the printed silicon carbide product at a temperature of 160° C. for 2 hours, so that the curing agent and the binder in the silicon carbide green body react completely, and the water in the pores of the green body evaporates completely, so that the pores of the green body are fully opened and retained;
[0035] S113, impregnation, placing the baked silicon carbide green body into the impregnation liquid, and ensuring that it is impregnated for 2 hours at a pressure of 25 kPa, and then drying again to obtain a silicon carbide green body with high residual carbon and high density.
[0036] As a further supplement to this embodiment, in S111, the amount of binder added to each silicon carbide product is 14% of the green body weight of the silicon carbide product, so that a firm bond can be achieved.
[0037] As a further supplement to the present embodiment, in S111, the thickness of each layer of the powdered surface is 0.15 mm, which ensures that each layer of the powdered surface can be completely cured by the adhesive and will not exceed the thickness and cannot be cured.
[0038] The green body density of the silicon carbide product printed in this way is ≥2.16g / cm 3 , effectively improving the printing density of silicon carbide green bodies.
[0039] As a supplement to the present embodiment, the preparation method of the impregnation liquid includes first selecting 60 parts of high residual carbon phenolic resin and 40 parts of ethanol and mixing them, then adding 10% of the weight of the impregnation liquid by weight of an organic dye dispersant HY-268 to the mixed solution, then adding 40% of the weight of nano carbon black to the impregnation liquid, and finally stirring for 4 hours to obtain the impregnation liquid for standby use.
[0040] At this time, the carbon density of the green silicon carbide product was 0.2 g / cm 3 -0.3g / cm 3 ; and the density of the silicon carbide product after reaction sintering is 2.95g / cm 3 -3.10g / cm 3 , the content of free silicon is 10%-20%, realizing the production of high residual carbon and high density silicon carbide products.
[0041] In another embodiment, a method for preparing the silicon carbide powder having a high bulk density comprises:
[0042] S201, selecting 76 parts of coarse-grained silicon carbide powder with a particle size of 120 μm-135 μm and adding them to a sand mixing tank, then adding a curing agent with a mass ratio of 3% of the coarse-grained silicon carbide powder to the sand mixing tank, and stirring at a high speed for 60 seconds;
[0043] S202, selecting 24 parts of fine-grained silicon carbide powder with a particle size of 28 μm-35 μm, adding it to the sand mixing tank, and stirring at high speed for 90 seconds to ensure that the three components are fully and evenly mixed;
[0044] S203, according to the dust situation during the mixing process of S202, add a curing agent with a mass ratio of 3.5% of the silicon carbide powder with a particle size of 28μm-35μm to the sand mixing tank again, and stir at high speed for 60s to fully mix the added curing agent with the components in the sand mixing tank, and make the humidity of the available silicon carbide powder obtained in the sand mixing tank reach a humidity state that can be kneaded and agglomerated, thereby completing the preparation of the silicon carbide powder.
[0045] As a supplement to this embodiment, a method for preparing a silicon carbide product using the silicon carbide powder includes:
[0046] S211, printing, the silicon carbide product is printed by 3D printing sand mold additive manufacturing equipment in this embodiment; specifically, the prepared silicon carbide powder is added into the powder spreading mechanism of the sand mold additive manufacturing equipment, and the laying time of each layer is 60 minutes to ensure the density of the powder spreading surface; a phenolic resin binder is installed in the print head of the additive manufacturing equipment, and the binder is sprayed at the corresponding product position according to the layer information to solidify the contour of the product on each layer of the powder spreading surface;
[0047] S212, drying, baking the green body of the printed silicon carbide product at a temperature of 200° C. for 1.5 hours, so that the curing agent and the binder in the silicon carbide green body react completely, and the water in the pores of the green body evaporates completely, so that the pores in the green body are all opened and retained;
[0048] S213, impregnation, placing the baked silicon carbide green body into the impregnation liquid, and ensuring that it is impregnated for 3 hours at a pressure of 25 kPa, and then drying again to obtain a silicon carbide green body with high residual carbon and high density.
[0049] As a further supplement to this embodiment, in S211, the amount of binder added to each silicon carbide product is 10% of the green body weight of the silicon carbide product, so that a firm bond can be achieved.
[0050] As a further supplement to the present embodiment, in S211, the thickness of each layer of powder coating is 0.2 mm, which ensures that each layer of powder coating can be completely cured by the adhesive and will not exceed the thickness and cannot be cured.
[0051] The green body density of the silicon carbide product printed in this way is ≥2.2g / cm 3 , effectively improving the printing density of silicon carbide green bodies.
[0052] As a supplement to the present embodiment, the preparation method of the impregnation liquid includes first selecting 50 parts of high residual carbon phenolic resin and 50 parts of ethanol and mixing them, then adding 7% of the weight of the impregnation liquid by weight of organic dye dispersant HY-268 to the mixed solution, then adding 37% of the weight of nano carbon black to the impregnation liquid, and finally stirring for 5 hours to obtain the impregnation liquid for standby use.
[0053] At this time, the carbon density of the green silicon carbide product was 0.2 g / cm 3 -0.3g / cm 3 ; and the density of the silicon carbide product after reaction sintering is 2.95g / cm 3 -3.10g / cm 3 , the content of free silicon is 10%-20%, realizing the production of high residual carbon and high density silicon carbide products.
[0054] Through the actual application of this technical solution in production, the problems of low density and low carbon content of the green body of large-sized and complex-structured silicon carbide products formed by binder jet 3D printing technology are solved, and the step of adding a carbon source before production of such products is simplified, making the step of post-processing carbon addition of the green body simpler, and effectively reducing the content of free silicon in the silicon carbide product after reaction sintering; on the other hand, the preparation method of the silicon carbide product described in the present invention is more conducive to environmental protection, and greatly reduces the risk of silicon carbide powder clogging the powder spreading mechanism and the risk of dust during printing.
[0055] The above embodiments are merely descriptions of a typical application of the technical solution of the present invention, and reasonable expansion can be carried out on a reasonable basis without requiring creative work.
Claims
1. A silicon carbide powder, characterized in that: The silicon carbide powder is a mixture, including two or three of silicon carbide powder with a particle size of 10μm-15μm and a purity of ≥99.5%, silicon carbide powder with a particle size of 28μm-35μm and a purity of ≥99.5%, silicon carbide powder with a particle size of 45μm-50μm and a purity of ≥99.5%, silicon carbide powder with a particle size of 90μm-110μm and a purity of ≥99.5%, and silicon carbide powder with a particle size of 120μm-135μm and a purity of ≥99.5%.
2. The silicon carbide powder according to claim 1, characterized in that The moisture content of the silicon carbide powder is 0.18%-0.25%.
3. The silicon carbide powder according to claim 1, characterized in that Silicon carbide powder with a particle size of 10μm-15μm and a purity of ≥99.5%, silicon carbide powder with a particle size of 28μm-35μm and a purity of ≥99.5%, silicon carbide powder with a particle size of 45μm-50μm and a purity of ≥99.5%, silicon carbide powder with a particle size of 90μm-110μm and a purity of ≥99.5%, and silicon carbide powder with a particle size of 120μm-135μm and a purity of ≥99.5% are all in the shape of silicon carbide shaped powder.
4. The method for preparing silicon carbide powder according to claim 2, characterized in that: include, S01, placing the selected coarse-grained silicon carbide powder into a preparation container, adding a curing agent into the preparation container, and stirring the two for 30s-90s; S02, selecting fine-grained silicon carbide powder and placing it in the preparation container, stirring for 60s-120s to uniformly mix the mixture in S01 and the fine-grained silicon carbide powder; S03, according to the dust situation during the stirring process of S02, gradually add curing agent into the preparation container, and continue stirring for 30s-90s.
5. A method for preparing a product made of silicon carbide material using the silicon carbide powder according to claim 2, characterized in that: include, S11, printing, using additive manufacturing equipment to print the green body of the product made of silicon carbide, and the laying time of each layer is 30min-60min; S12, drying, baking the printed silicon carbide green body at a temperature of 100° C.-200° C. for 1 h-4 h, so that the curing agent and the binder in the silicon carbide green body react completely, and the water in the pores of the green body evaporates completely, so that the pores of the green body are all opened and retained; S13, impregnation, placing the baked silicon carbide green body into the prepared impregnation liquid, and ensuring that it is impregnated for 1h-5h at a pressure of 25kPa, and then drying again to obtain a silicon carbide green body with high residual carbon and high density.
6. The method for preparing a product made of silicon carbide material according to claim 5, characterized in that: In S11, the amount of binder added to each silicon carbide product is 5%-20% of the weight of the silicon carbide product.
7. The method for preparing a product made of silicon carbide material according to claim 5, characterized in that: In S11, the thickness of each layer of powder surface is 0.15mm-0.32mm.
8. The method for preparing a product made of silicon carbide material according to claim 5, characterized in that: The impregnation liquid preparation method is: First, 50%-80% of high residual carbon phenolic resin and 50%-20% of ethanol are mixed; Then add 3% to 10% of the weight of the impregnation solution as an organic dye dispersant; Then add 25% to 60% of nano carbon black by weight of the impregnation solution; Finally, stirring is performed for 3 h to 6 h to obtain the impregnation solution.
Citation Information
Patent Citations
Silicon carbide composite powder for additive manufacturing and preparation method thereof
CN114230346A
Silicon carbide ceramic and preparation method thereof
CN114591085A
3D printing forming and curing method
CN116332652A
Silicon carbide composite ceramic and preparation method thereof
CN116409997A
Method for preparing high-thermal-conductivity and high-strength Si / SiC ceramic material through 3D printing
CN118184361A