Monomer containing pyrrolidone ring, degradable long-chain random copolyester and preparation method

By introducing pyrrolidone ring monomer and aliphatic dibasic acid into long-chain aliphatic polyester, combined with the esterification-melt polycondensation process, high molecular weight degradable long-chain random copolyester was prepared, and the performance and degradation rate were solved. The conflict has achieved widespread application of materials.

CN119080666AActive Publication Date: 2024-12-06NINGBO INST OF MATERIALS TECH & ENG CHINESE ACAD OF SCI
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411247904.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-12-06
Estimated Expiration
2044-09-05

AI Technical Summary

Technical Problem

The existing long-chain aliphatic polyesters have conflicts between performance and degradation rate in improving biodegradability, and the conditions for preparing high-molecular-weight polymers are harsh, which affects the wide range of applications of materials.

Method used

The monomer containing pyrrolidone ring is synthesized by Michael addition reaction, combined with aliphatic dibasic acid and long-chain diol, and prepared degradable long-chain random copolyester through an esterification-melt polycondensation process to regulate its biodegradation rate. and physical properties.

Benefits of technology

The preparation of high molecular weight copolyester has been achieved, with excellent crystallinity, high Young's modulus and water vapor barrier properties, and can regulate the biodegradation rate within a wide range. It is suitable for film products such as agricultural mulching and shopping bags.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119080666A_ABST
    Figure CN119080666A_ABST
Patent Text Reader

Abstract

The invention provides a pyrrolidone ring-containing monomer, a degradable long-chain random copolyester and a preparation method of the degradable long-chain random copolyester. The copolyester has a structure as shown in the following formula: # imgabs0 #, R1 comprises an ether bond or a thioether bond, R2 and R3 comprise straight-chain alkyl groups containing 10-30 carbon atoms, x and y are integers in a range of 1-10, and m is an integer in a range of 20-100. The degradable long-chain random copolyester provided by the invention is high in molecular weight, not only has excellent crystallinity, high Young modulus and water vapor gas barrier property, but also has better hydrolytic sensitivity, the biodegradation rate can be regulated and controlled in a wide range, the degradable long-chain random copolyester can be widely applied to preparation of agricultural plastic mulching films, shopping bags and other products, meanwhile, the preparation process is simple and easy to operate, and the degradable long-chain random copolyester is suitable for industrial production. The reaction conditions are mild, and the yield is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application specifically relates to a pyrrolidone ring-containing monomer, a degradable long-chain random copolyester and a preparation method, and belongs to the technical field of polymer materials. Background Art

[0002] Aliphatic polyesters with 10 or more methylene groups between ester bonds are usually called long-chain aliphatic polyesters or polyethylene-like aliphatic polyesters. As the length of the aliphatic chain increases, the repeating units form stable crystalline regions through van der Waals interactions between the methylene segments, and the polyester properties gradually approach those of polyethylene with high melting point, high crystallinity, and high water vapor barrier properties. By selecting the length of the monomer raw material, the properties of long-chain aliphatic polyesters can be modulated between flexible LDPE and more rigid HDPE to meet different application requirements: the presence of ester bonds also gives long-chain aliphatic polyesters the property of chemical recycling. Therefore, this type of long-chain aliphatic polyester with customizable properties and recyclability has become one of the most promising polyethylene substitutes. However, highly crystalline and highly hydrophobic materials are usually difficult to degrade, and the biodegradability of long-chain aliphatic polyesters also decreases with the chain length between ester bonds, which leads to a conflict between their application properties and degradation rates, and the recycling method of the materials is single and the application scenarios are limited. When leaked into the natural environment, long-chain aliphatic polyesters with slow degradation rates will still cause environmental pollution problems caused by waste accumulation.

[0003] By copolymerizing with polar dibasic acids, hydrophilic units are introduced into the polyester structure, which is beneficial to improve the hydrophilicity of copolyesters and enhance the biodegradability of materials. Pyrrolidone cyclic dibasic acids are synthesized by the Michael addition reaction of itaconic acid and aliphatic diamines, and polar CN can be introduced into the main chain of copolyesters by copolymerization. However, due to the hydrophobicity of the methylene chain segment, the hydrophilicity of the pyrrolidone ring structure obtained by aliphatic diamines is limited; in addition, the steric hindrance effect of the pyrrolidone ring will affect the close stacking of the molecular chain, and the addition of too many pyrrolidone units will destroy the crystallinity of the polyester and affect the thermal and mechanical properties of the polyester. Therefore, aliphatic pyrrolidone dibasic acids still cannot effectively enhance the biodegradability of long-chain aliphatic polyesters while taking into account the application performance of copolyesters.

[0004] Long-chain aliphatic polyesters prepared by melt polycondensation need to strictly control the alkyd-acid feed ratio of 1:1. The purity of the monomers and the deviation of the feed will cause an imbalance in the alkyd-acid ratio, making it difficult to increase the molecular weight of the polymerization. However, by using the excessive feeding method of diol, the diol can be removed as much as possible under high temperature and high vacuum conditions during the polycondensation stage to increase the molecular weight of the polymer. However, the boiling point of long-chain diols is relatively high, and the synthesis of high molecular weight products requires higher polymerization temperature and reaction time. For example, the atmospheric boiling point of decanediol is 297°C, and the boiling point of long-chain diols increases with the increase of carbon chain, and the preparation conditions are more demanding. Some researchers have proposed a method of introducing low-boiling diols into the polymerization system to assist the polycondensation ester exchange to solve the above problem, that is, firstly, low-boiling ethylene glycol and high-boiling hexanediol are mixed with oxalic acid diesters to obtain hydroxyl-terminated oligomers, and then the two oligomers are mixed and further polycondensed under reduced pressure at 150-220°C for 0.5-6h to obtain high molecular weight polyoxalate hexanediol ester. This low-boiling-point volatile diol-assisted polymerization process can obtain high-molecular-weight long-chain diol-containing polyester at a lower polymerization temperature and a shorter polymerization time. However, short-chain ethylene glycol may form diethylene glycol with a higher boiling point (boiling point 245°C at normal pressure) during the reaction, which is difficult to completely remove, resulting in residual chain segments that affect material properties. Summary of the invention

[0005] The main purpose of the present application is to provide a pyrrolidone ring-containing monomer, a degradable long-chain random copolyester, and a preparation method and application thereof, so as to overcome the deficiencies in the prior art.

[0006] In order to achieve the above-mentioned invention objectives, this application adopts the technical solution described below.

[0007] The first aspect of the present application provides a pyrrolidone ring-containing monomer having a structure shown in Formula 1,

[0008]

[0009] Here, R contains an ether bond or a thioether bond.

[0010] The second aspect of the present application provides a method for preparing a monomer containing a pyrrolidone ring, comprising: subjecting itaconic acid and a diamine to a Michael addition reaction to obtain the monomer;

[0011] Wherein, the monomer has a structure shown in Formula 1, and the diamine has a structure shown in Formula 2,

[0012]

[0013] H2N-R-NH2

[0014] Formula 2

[0015] R contains an ether bond or a thioether bond;

[0016] The third aspect of the present application provides a degradable long-chain random copolyester having a structure shown in Formula 3,

[0017]

[0018] Among them, R1 contains an ether bond or a thioether bond, R2 and R3 include straight-chain alkyl groups containing 10-30 carbon atoms, x and y are both integers of 1-10, m is an integer of 20-100, and the molar ratio of R1 to R3 is 1:9-3:7.

[0019] The fourth aspect of the present application provides a method for preparing a degradable long-chain random copolyester, which comprises:

[0020] subjecting a first mixed system comprising monomer A, monomer B, monomer C, monomer D and an esterification catalyst to an esterification reaction or an ester exchange reaction to obtain an intermediate product;

[0021] subjecting the second mixed system comprising the intermediate product, a polycondensation catalyst and a stabilizer to a polycondensation reaction to obtain the degradable long-chain random copolyester;

[0022] Wherein, the monomer A includes an aliphatic dibasic acid containing R3 or its ester, the monomer B includes a long-chain diol containing R2, the monomer C includes the pyrrolidone ring-containing monomer, the monomer D includes propylene glycol, and R2 and R3 include alkyl groups containing 10-30 carbon atoms.

[0023] The fifth aspect of the present application provides the use of the pyrrolidone ring-containing monomer or the degradable long-chain random copolyester in the preparation of film products, wherein the film products include agricultural mulch films, shopping bags, etc., but are not limited thereto.

[0024] Compared with the prior art, this application has at least the following beneficial effects:

[0025] (1) The preparation process of the provided pyrrolidone ring-containing monomer and the degradable long-chain random copolyester is simple, easy to operate, has mild reaction conditions and high yield.

[0026] (2) The provided degradable long-chain random copolyester has a high molecular weight and not only has excellent crystallinity, high Young's modulus and water vapor gas barrier properties, but also has good hydrolysis sensitivity. The biodegradation rate can be regulated within a wide range and can be widely used in the preparation of film products such as agricultural mulch films and shopping bags. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0028] Figure 1 This is the H NMR spectrum of the SPA monomer containing pyrrolidone prepared in Example 1;

[0029] Figure 2 This is the infrared spectrum of the SPA monomer containing pyrrolidone prepared in Example 1;

[0030] Figure 3 This is the infrared spectrum of the degradable long-chain random copolyester prepared in Example 1;

[0031] Figure 4 This is a DSC secondary temperature rise curve of the degradable long-chain random copolyester prepared in Example 1;

[0032] Figure 5 This is a stress-strain curve of the degradable long-chain random copolyester prepared in Example 1;

[0033] Figure 6 This is the GPC curve of the degradable long-chain random copolyester prepared in Example 1;

[0034] Figure 7 This is a schematic diagram of the surface contact angle of the degradable long-chain random copolyester prepared in Example 1. DETAILED DESCRIPTION

[0035] As mentioned above, in view of the problems that the existing long-chain aliphatic polyesters have difficulty in balancing polyethylene-like properties and degradation properties, and the molecular weight of the condensation synthesis is not high, the present application provides a pyrrolidone ring-containing monomer, a degradable long-chain random copolyester, and a preparation method and application thereof. The present application first uses itaconic acid and a diamine containing an ether or thioether bond as raw materials, synthesizes a pyrrolidone ring-containing dibasic acid, that is, the pyrrolidone ring-containing monomer through a Michael addition reaction, and then the pyrrolidone ring-containing dibasic acid, aliphatic dibasic acid or its ester, long-chain diol, propylene glycol and a catalyst are mixed to obtain a polyester oligomer, and then the polyester oligomer is subjected to a condensation reaction under high temperature and high vacuum conditions to obtain the degradable long-chain random copolyester. The process is simple and easy to operate, the reaction conditions are mild and the yield is high, and the prepared copolyester has the advantages of easy crystallization, hydrolysis sensitivity, and adjustable biodegradation rate. At the same time, it has a fast crystallization rate, high crystallization enthalpy and melting enthalpy, high modulus, and excellent water vapor barrier properties. The technical solution of the present application will be further described as follows.

[0036] Some embodiments of the present application provide a pyrrolidone ring-containing monomer having a structure shown in Formula 1,

[0037]

[0038]

[0039] Some embodiments of the present application also provide a method for preparing the pyrrolidone ring-containing monomer, which comprises: subjecting itaconic acid and a diamine to a Michael addition reaction to obtain the monomer;

[0040] Wherein, the monomer has a structure shown in Formula 1, and the diamine has a structure shown in Formula 2,

[0041] H2N-R-NH2.

[0042] Formula 2

[0043] In the above formula 1 and II, R contains an ether bond or a thioether bond.

[0044] Furthermore, R may include at least one of the following structural units:

[0045]

[0046] In one embodiment, the preparation method specifically comprises: subjecting a mixed reaction system comprising itaconic acid, a diamine and water to the Michael addition reaction at 130-180° C. to obtain the monomer.

[0047] In one embodiment, the reaction time is 24-48 hours.

[0048] In one embodiment, the molar ratio of itaconic acid to diamine is 1.8-2.2:1.

[0049] In a more specific embodiment, the preparation method may include: dissolving itaconic acid and diamine in water, stirring, condensing and refluxing at a temperature of 130° C., then removing excess water, precipitating in cold methanol, and washing multiple times to obtain the pyrrolidone ring-containing monomer.

[0050] The method for preparing the monomer containing pyrrolidone ring provided in the present application has simple process, mild conditions and high yield, which can exceed 95%.

[0051] Some embodiments of the present application also provide a degradable long-chain random copolyester having a structure shown in Formula 3,

[0052]

[0053] Among them, R1 contains an ether bond or a thioether bond, R2 and R3 include straight-chain alkyl groups containing 10-30 carbon atoms, x and y are both integers of 1-10, m is an integer of 20-100, and the molar ratio of R1 to R3 is 1:9-3:7. Among them, if the R1 ratio is too small, the hydrophilicity of the copolyester will be insufficient and the degradation rate of the material will be slow; as the R1 ratio increases, the hydrophilicity of the material gradually increases and the degradation rate becomes faster, but when it exceeds 30%, the crystallization ability of the copolyester is seriously reduced, resulting in insufficient mechanical properties and barrier properties.

[0054] Preferably, R2 and R3 can be selected from long-chain alkyl groups containing 10-30 carbon atoms.

[0055] In one embodiment, R1 may include at least one of the following structural units:

[0056]

[0057] The degradable long-chain random copolyester of the present application has a relatively high molecular weight, with a weight average molecular weight higher than 120,000 g / mol, preferably 140,000-200,000 g / mol, a dispersity of 2.0-3.0, and an intrinsic viscosity of 1.15-1.35 dL / g.

[0058] In the degradable long-chain random copolyester of the present application, the molar fraction of repeating units containing aliphatic dibasic acids in the total repeating units is adjusted to be greater than or equal to 70%, so that the copolyester presents the crystalline structure of long-chain aliphatic polyester. The presence of repeating units containing aliphatic dibasic acids can ensure that the melt crystallization enthalpy and melting enthalpy of the copolyester are relatively high, and the obtained copolyester has a fast crystallization rate and high crystallinity. The higher crystallinity also ensures that the copolyester has a high Young's modulus and water vapor barrier property. Specifically, the melt crystallization enthalpy or melting enthalpy of the degradable long-chain random copolyester is above 50 J / g, the melting point is above 60°C, and the Young's modulus is 200-800 MPa, which can reach 2-8 times that of commercial PBAT; the water vapor barrier coefficient is 1.10×10 -13 -4.65×10 -14 g cm / cm 2 ·s·Pa, which can reach 3-8 times that of commercial PBAT.

[0059] At the same time, the degradable long-chain random copolyester of the present application contains ether bonds / ether-sulfide bonds and pyrrolidone ring structures, so the overall hydrophilicity of the copolyester is improved. Further, the synergistic effect of the two polar structures can effectively increase the rate at which water molecules diffuse into the interior of the copolyester, thereby increasing the hydrolysis rate of the ester bond and achieving rapid degradation under bioenzyme catalysis. Moreover, in the present application, the hydrophilicity of the polyester can be changed according to the content of the pyrrolidone unit containing the ether / sulfide bond, thereby regulating its biodegradation rate. Specifically, the water contact angle of the degradable long-chain random copolyester is 85°-70°, the mass loss rate after degradation in water for 6 months is 20%-60%, and the mass loss rate after degradation by Antarctic Candida lipase b (CALB enzyme) for 30 days is 30%-90%.

[0060] In summary, the degradable long-chain random copolyester of the present application is easy to crystallize and has an adjustable degradation rate. It has excellent degradation performance and physical and mechanical properties similar to polyethylene, including faster crystallization rate, high crystallization enthalpy and melting enthalpy, higher modulus and excellent water vapor barrier, etc. When used as agricultural mulch and other products, it has better stiffness and moisture retention, and when used as shopping bags and other products, it has higher load-bearing and deformation resistance. At the same time, the degradation rate of the degradable long-chain random copolyester of the present application can be regulated by the type and content of the main repeating unit and the secondary repeating unit, so it has a wider range of applications, especially for the preparation of agricultural mulch and other products whose degradation rate can be adjusted over a wide range according to the use environment.

[0061] Some embodiments of the present application provide a method for preparing the degradable long-chain random copolyester, which uses long-chain diols and aliphatic dibasic acids as main monomers, a small amount of diacid containing a pyrrolidone ring as a copolymerization monomer, and synthesizes the copolyester through esterification-melt polycondensation or ester exchange-melt polycondensation reaction.

[0062] In one embodiment, the preparation method specifically comprises:

[0063] subjecting a first mixed system comprising monomer A, monomer B, monomer C, monomer D and an esterification catalyst to an esterification reaction or an ester exchange reaction to obtain an intermediate product;

[0064] subjecting the second mixed system comprising the intermediate product, a polycondensation catalyst and a stabilizer to a polycondensation reaction to obtain the degradable long-chain random copolyester;

[0065] The monomer A comprises an aliphatic dibasic acid containing R3 or an ester thereof. The monomer A is used to make the copolyester have the advantages of fast crystallization speed and high crystallinity, and can improve its mechanical properties and gas barrier properties.

[0066] The monomer B includes a long-chain diol containing R2. The introduction of the long-chain diol can further improve the crystallization ability of the copolyester, increase its hydrophobicity, and help improve its melting point and water vapor barrier properties.

[0067] The monomer C includes the monomer containing a pyrrolidone ring. Since the longer the chain of the aliphatic dibasic acid and diol is, the weaker the degradability of the obtained polyester product is and the slower the degradation rate is, the polar pyrrolidone unit is introduced into the system of the present application to adjust the biodegradation rate of the polyester, and according to the length of the aliphatic dibasic acid and diol, different types and amounts of monomers can be selected to adjust their degradation rates to different degrees, while maintaining other excellent properties as much as possible; at the same time, polar ether bonds / ether-sulfur bonds are added between the pyrrolidone rings to give play to the synergistic effect of various polar structures such as CN and CO / CS, which can further improve the hydrophilicity of the chain segment, and achieve rapid improvement of the degradation performance of the polyester after the introduction of a small amount of pyrrolidone units.

[0068] The monomer D includes propylene glycol, and R2 and R3 include alkyl groups containing 10-30 carbon atoms. Since long-chain diols have a high boiling point and are difficult to remove at a low polymerization temperature, which is not conducive to the growth of molecular weight, the present application adds low-boiling-point, easily removable short-chain diols to the system to assist in the polycondensation. Compared with ethylene glycol with the same low boiling point, propylene glycol will not form difficult-to-remove by-products at high temperatures. Therefore, the present application selects propylene glycol to assist in the melt polycondensation, which is not only conducive to the preparation of high molecular weight polymers, but also very few residual propylene glycol segments will not affect the performance of the copolyester.

[0069] In one embodiment, in the first mixed system, the ratio of the sum of the molar amounts of the monomer A and the monomer C to the sum of the molar amounts of the monomer B and the monomer D is 1:m, the molar ratio of the monomer A to the monomer C is 1:9-3:7, and the molar ratio of the monomer B to the monomer D is n:(mn), wherein m=1.4-1.6, n=0.9-1.1.

[0070] In the present application, by introducing the pyrrolidone ring-containing monomer and controlling the relative content change between the pyrrolidone ring and the aliphatic dibasic acid and the monomer within the above range, the hydrophilicity and degradation ability of the copolyester can be more accurately regulated and improved with less influence on the thermal and mechanical properties of the copolyester, thereby maintaining or improving its excellent degradation ability in water and biological enzyme environments.

[0071] In one embodiment, the esterification reaction or transesterification reaction is carried out under a protective atmosphere, and the reaction temperature is 175-200° C. If the temperature is too high, the diol will volatilize, resulting in a mismatch in the ratio of raw acid to alcohol and reaction failure, and if the temperature is too low, the reaction efficiency will be low.

[0072] Furthermore, the protective atmosphere includes an atmosphere formed by an inert gas such as argon, nitrogen, etc. or a mixed gas thereof.

[0073] In one embodiment, the reaction time of the esterification reaction or the transesterification reaction is 4h-6h.

[0074] In one embodiment, the preparation method comprises: preparing the intermediate product when the esterification reaction or the transesterification reaction is carried out until the yield of the byproduct water or methanol is greater than or equal to 90% of the theoretical yield.

[0075] In one embodiment, in the first mixed system, the ratio of the esterification catalyst to the sum of the molar amounts of the monomer A and the monomer C is 0.5:1000-2.0:1000, wherein if the catalyst is too little, the esterification efficiency is low and the reaction is incomplete, and if the catalyst is too much, the product color is yellow.

[0076] In a more specific implementation case, the preparation method may include the following steps:

[0077] (1) Esterification stage: monomers A, B, C, D and an esterification catalyst are mixed to form a first mixed system, and the intermediate product is obtained by esterification or transesterification reaction until the yield of byproduct water or methanol is at least 90%;

[0078] (2) Polycondensation stage: The intermediate product, polycondensation catalyst and stabilizer are subjected to vacuum melt polycondensation to obtain the copolyester.

[0079] In one embodiment, the esterification catalyst includes but is not limited to any one or more combinations of titanium-based catalysts, antimony-based catalysts, tin-based catalysts, acetic acid-based catalysts, and the like.

[0080] Among them, the titanium catalyst includes any one or more combinations of tetrabutyl titanate, isopropyl titanate, isobutyl titanate, propylene glycol titanium, and titanium dioxide, and is not limited to this. The antimony catalyst includes any one or more combinations of antimony trioxide, antimony acetate, and propylene glycol antimony, and is not limited to this. The tin catalyst includes any one or more combinations of butyl stannic acid, dibutyl tin oxide, stannous isooctanoate, stannous oxalate, dibutyl tin diacetate, dibutyl tin dilaurate, and dioctyl tin oxide, and is not limited to this. The acetic acid catalyst includes any one or more combinations of lithium acetate, potassium acetate, calcium acetate, magnesium acetate, barium acetate, zinc acetate, cobalt acetate, antimony acetate, lead acetate, and manganese acetate, and is not limited to this.

[0081] In one embodiment, the ratio of the polycondensation catalyst to the sum of the molar amounts of the monomer A and the monomer C is 0.1:1000-0.5:1000.

[0082] In one embodiment, the ratio of the stabilizer to the sum of the molar amounts of the monomer A and the monomer C is 0.5:1000-2.0:1000, wherein if the stabilizer is too little, the reaction product is easily thermally degraded, and if the stabilizer is too much, the remaining stabilizer will remain as an impurity, affecting the quality of the final product.

[0083] In one embodiment, the reaction temperature of the polycondensation reaction is 200-230° C. If the temperature is too low, the reaction time will be greatly prolonged, and if the temperature is too high, side reactions such as thermal decomposition may occur.

[0084] In one embodiment, the reaction time of the polycondensation reaction is 8h-24h.

[0085] In one embodiment, the polycondensation reaction is carried out under a vacuum degree of less than 5 Pa.

[0086] In one embodiment, the polycondensation catalyst includes, but is not limited to, any one or more combinations of titanium catalysts, antimony catalysts, tin catalysts, and acetic acid catalysts. Among them, the titanium catalyst includes any one or more combinations of tetrabutyl titanate, isopropyl titanate, isobutyl titanate, propylene glycol titanium, and titanium dioxide, and is not limited thereto. The antimony catalyst includes any one or more combinations of antimony trioxide, antimony acetate, and propylene glycol antimony, and is not limited thereto. The tin catalyst includes any one or more combinations of butyl stannic acid, dibutyl tin oxide, stannous isooctanoate, stannous oxalate, dibutyl tin diacetate, dibutyl tin dilaurate, and dioctyl tin oxide, and is not limited thereto. The acetic acid catalyst includes one or more combinations of lithium acetate, potassium acetate, calcium acetate, magnesium acetate, barium acetate, zinc acetate, cobalt acetate, antimony acetate, lead acetate, and manganese acetate, and is not limited thereto.

[0087] In one embodiment, the stabilizer can inhibit the breakage of ester bonds, fatty chains, etc. during the reaction process, and can include antioxidant 1010, antioxidant 1076, antioxidant 1500, antioxidant 425, thermal stabilizer 330, thermal stabilizer 1178, thermal stabilizer 618, thermal stabilizer 626, thermal stabilizer 168, trimethyl phosphite, triethyl phosphite, triisooctyl phosphite, triisodecyl phosphite, trilauryl phosphite, tritridecyl phosphite, trioctadecyl phosphite, triphenyl phosphite, tri-p-tolyl phosphite, di-tridecyl phosphite, tri-p-tolyl ... The invention may include any one or more combinations of tris(2,4-di-tert-butylbenzene) phosphate, di(2,4-di-p-isopropylphenyl) pentaerythritol bisphosphite phosphoric acid, pentaerythritol tetraphenyl tridecyl phosphite, pentaerythritol tridecyl diphosphite, pentaerythritol diisodecyl diphosphite, tetraphenyl dipropylene glycol diphosphite, phosphoric acid, phosphorous acid, polyphosphoric acid and triethyl phosphonoacetate, light stabilizer 791, light stabilizer 700, light stabilizer 783, light stabilizer 119, light stabilizer 770, light stabilizer 622, light stabilizer 944 and light stabilizer 1164, and is not limited thereto.

[0088] In the present application, when the esterification catalyst is a titanium-based catalyst or an antimony-based catalyst, the esterification catalyst can also be used as the polycondensation catalyst. In this case, the esterification product can be directly subjected to subsequent polycondensation reaction. However, considering that the esterification catalyst will be partially ineffective after the esterification reaction, when the esterification catalyst and the polycondensation catalyst are the same, part of the esterification catalyst can be added to the esterification product before the polycondensation reaction. The ratio of the added esterification catalyst to the sum of the molar amounts of the monomer A and the monomer C can be 0.5:1000-1:1000.

[0089] The method for preparing the copolyester provided in the present application has the advantages of simple process, mild conditions, high yield, etc.

[0090] The technical solution of the present application is described in detail below in conjunction with specific embodiments so that those skilled in the art can better understand and implement the technical solution of the present application. The specific functional details disclosed herein should not be interpreted as being restrictive, but only as the basis for the claims and as a representative basis for teaching those skilled in the art to adopt the present application in different ways in any appropriate detailed embodiment.

[0091] In the following examples and comparative examples, unless otherwise specified, all raw materials are commercially available or prepared by conventional methods in the art.

[0092] In the following examples and comparative examples, a mixed solution of phenol and tetrachloroethane in a mass ratio of 1:1 was used to measure the Ubbelohde viscosity at 25°C; a gel permeation chromatograph (Agilent PL-GPC220) was used to measure the weight average molecular weight and dispersity according to a polystyrene standard, wherein the sample was dissolved in chloroform at a concentration of 1 m / mL, chloroform was used as the mobile phase, and the flow rate was 1 ml·min -1 , the temperature is 40℃.

[0093] In the following examples and comparative examples, a differential scanning calorimeter (Mettler Toledo DSC) was used to test thermal properties, wherein the heating rate was 10°C / min, the temperature range was -20°C-250°C, and the measurement was performed in a N2 atmosphere.

[0094] In the following examples and comparative examples, a Zwicki 1kN universal material testing machine was used to test the mechanical properties, wherein the sample strip dimensions were 15.0 mm in length, 2.0 mm in width, and 1.0 mm in thickness, and the tensile speed was 20 mm / min.

[0095] In the following examples and comparative examples, the surface contact angle of the samples was measured using a contact angle measuring instrument OCA25.

[0096] In the following examples and comparative examples, the water vapor transmission rate test system was used to test the water vapor barrier performance in a constant temperature and humidity chamber at 38°C and 90% relative humidity. The sample transmission area was 29.2 cm 2 .

[0097] In the following examples and comparative examples, a phosphate buffer solution was used as a degradation solvent, and a hydrolysis degradation test was performed at a constant temperature of 37° C., wherein the sample was 10 mm in length, 10 mm in width, and 0.5 mm in thickness.

[0098] In the following examples and comparative examples, a phosphate buffer solution containing 0.1 mg / ml lipase was used as a degradation solvent, and the enzyme degradation test was carried out at a constant temperature of 37° C., wherein the sample was 10 mm in length, 10 mm in width, and 0.5 mm in thickness.

[0099] Embodiment 1 The preparation method of a degradable long-chain random copolyester (hereinafter referred to as copolyester) provided in this embodiment comprises the following steps:

[0100] (1) Preparation of a pyrrolidone ring-containing monomer: 2.2 mol of itaconic acid and 1.0 mol of 1,1′-thiobis(methylamine) were dissolved in water, stirred, condensed and refluxed at 130° C. for 48 h, and then excess water was removed. The mixture was precipitated in cold methanol and washed several times to obtain a pyrrolidone ring-containing monomer named SPA. The NMR spectrum of the monomer is shown in FIG. Figure 1 As shown, the infrared spectrum is Figure 2 shown.

[0101] (2) Preparation of polyester oligomers by esterification reaction: First, 0.1 mol of pyrrolidone ring-containing monomer SPA, 0.9 mol of tetradecyl diacid, 1.05 mol of tetradecyl glycol, 0.55 mol of propylene glycol, and 170 mg of tetrabutyl titanate were added to the reactor. Under the protection of high-purity nitrogen, the temperature was gradually raised to 200° C. and reacted for 4 hours until the water content produced exceeded 90% of the theoretical yield, thereby obtaining a polyester oligomer as an intermediate product.

[0102] (3) Preparation of copolyester by melt polycondensation reaction: 145 mg of polycondensation catalyst antimony trioxide and 650 mg of stabilizer diphenyl phosphate were added to the oligomer obtained in step (2), and the pressure was gradually reduced and the temperature was increased. After 30 minutes, the vacuum degree of the reactor reached 5 Pa, and the reaction temperature was maintained at 220° C. After 18 hours, the polymerization reaction was terminated after the rated stirring torque reached 200 N·cm to obtain a copolyester. The structure of the copolyester was determined by infrared, nuclear magnetic resonance and other characterizations as shown in Formula 4-1. The infrared spectrum of the copolyester is shown in Figure 3 shown.

[0103]

[0104] Wherein, x and y are both integers of 1-10, m is an integer of 20-100, and x:y=1:9.

[0105] After testing, the copolyester has an intrinsic viscosity of 1.26 dL / g, a weight-average molecular weight of 185,500 g / moL, a dispersity of 2.1, a melting peak temperature of 91.4°C, a melting enthalpy of 95.6 J / g, a crystallization peak temperature of 64°C, and a crystallization enthalpy of 95.6 J / g.

[0106] After testing, the modulus of the copolyester reaches 550MPa, the strength exceeds 30MPa, and the elongation at break exceeds 1000%.

[0107] The DSC secondary heating curve, stress-strain curve and GPC curve of the copolyester are shown in Figure 2. Figure 4 , Figure 5 and Figure 6 shown.

[0108] The test showed that the surface contact angle of the copolyester with water was 83° and the water vapor barrier coefficient was 4.894×10 -14 g cm / cm 2 ·s·Pa, which is 7 times that of PBAT. The surface contact angle of the copolyester with water is Figure 7 shown.

[0109] According to the test, in deionized water, the mass of the copolyester decreased by 20% after 180 days of degradation in deionized water, and in PBS buffer containing CALB enzyme, the mass of the copolyester decreased by 30% after 30 days of degradation.

[0110] Embodiment 2 The preparation method of a degradable long-chain random copolyester (hereinafter referred to as copolyester) provided in this embodiment comprises the following steps:

[0111] (1) Preparation of a pyrrolidone ring-containing monomer: 1.8 mol of itaconic acid and 1.0 mol of 2,2'-thiobis(ethylamine) were dissolved in water, stirred, condensed and refluxed at 180°C for 24 h, and then excess water was removed, precipitated in cold methanol, and washed several times to obtain a pyrrolidone ring-containing monomer, named ESPA.

[0112] (2) Preparation of polyester oligomers by esterification reaction: First, 0.2 mol of pyrrolidone ring-containing monomer ESPA, 0.8 mol of dodecyl dimethyl ester, 1.03 mol of dodecyl glycol, 0.57 mol of propylene glycol, and 560 mg of isopropyl titanate were added to the reactor. Under the protection of high-purity nitrogen, the temperature was gradually raised to 200° C. and reacted for 6 hours until the content of the generated water and methanol mixture exceeded 90% of the theoretical value, thereby obtaining polyester oligomers.

[0113] (3) Preparation of copolyester by melt polycondensation reaction: 150 mg of polycondensation catalyst antimony acetate and 150 mg of stabilizer phosphorous acid were added to the oligomer obtained in step (2), and the pressure was gradually reduced and the temperature was increased. After 30 minutes, the vacuum degree of the reactor reached 5 Pa, and the reaction temperature was maintained at 220°C. After 12 hours, the polymerization reaction was terminated after reaching the rated stirring torque of 200 N·cm to obtain a copolyester. The structural formula was determined by infrared, nuclear magnetic resonance and other characterizations as shown in Formula 4-2.

[0114]

[0115] Wherein, x and y are both integers of 1-10, m is an integer of 20-100, and x:y=2:8.

[0116] After testing, the copolyester has an intrinsic viscosity of 1.28 dL / g, a weight-average molecular weight of 156783 g / moL, a dispersity of 2.3, a melting peak temperature of 90.1°C, a melting enthalpy of 83.7 J / g, a crystallization peak temperature of 64.7°C, and a crystallization enthalpy of 83.0 / g.

[0117] The test results show that the modulus of the copolyester reaches 300MPa, the strength exceeds 15MPa, and the elongation at break exceeds 700%. The test results show that the surface contact angle of the copolyester is 70°, and the water vapor barrier coefficient is 9.638×10 -14 g cm / cm 2 ·s·Pa, which is 3.6 times that of PBAT.

[0118] According to the test, in deionized water, the mass of the copolyester decreased by 26% after 190 days of degradation in deionized water, and in PBS buffer containing CALB enzyme, the mass of the copolyester decreased by 40% after 30 days of degradation.

[0119] Embodiment 3 The preparation method of a degradable long-chain random copolyester (hereinafter referred to as copolyester) provided in this embodiment comprises the following steps:

[0120] (1) Preparation of a pyrrolidone ring-containing monomer: 2.0 mol of itaconic acid and 1.0 mol of 1,8-diamine-3,6-dithiooctane were dissolved in water, stirred, condensed and refluxed at 160° C. for 36 h, and then excess water was removed, precipitated in cold methanol, and washed several times to obtain a pyrrolidone ring-containing monomer, named DSPA.

[0121] (2) Preparation of polyester oligomers by esterification reaction: First, 0.3 mol of pyrrolidone ring-containing monomer DSPA, 0.7 mol of 1,10-dimethyl sebacate, 1.0 mol of 1,10-decanediol, 0.4 mol of propylene glycol, and 210 mg of stannous isooctanoate were added to the reactor. Under the protection of high-purity nitrogen, the temperature was gradually raised to 175° C. and reacted for 4 hours until the content of the generated water and methanol mixture exceeded 90% of the theoretical value, thereby obtaining polyester oligomers.

[0122] (3) Preparation of copolyester by melt polycondensation reaction: 150 mg of polycondensation catalyst tetrabutyl titanate and 150 mg of stabilizer triisooctyl phosphite were added to the oligomer obtained in step (2), and the pressure was gradually reduced and the temperature was increased. After 30 minutes, the vacuum degree of the reactor reached 5 Pa, and the reaction temperature was maintained at 200°C. After 8 hours, the polymerization reaction was terminated after reaching the rated stirring torque of 200 N·cm to obtain a copolyester. Its structural formula was determined by infrared, nuclear magnetic resonance and other characterizations as shown in Formula 4-3.

[0123]

[0124]

[0125] Wherein, x and y are both integers of 1-10, m is an integer of 20-100, and x:y=3:7.

[0126] After testing, the copolyester has an intrinsic viscosity of 1.28 dL / g, a weight-average molecular weight of 140622 g / moL, a dispersity of 2.5, a melting peak temperature of 69.7°C, a melting enthalpy of 64.3 J / g, a crystallization peak temperature of 53.8°C, and a crystallization enthalpy of 63.4 / g.

[0127] After testing, the modulus of the copolyester reaches 250MPa, the strength exceeds 15MPa, and the elongation at break exceeds 800%. The surface contact angle of the copolyester is 70°, and the water vapor barrier coefficient is 1.10×10 -13 g cm / cm 2 ·s·Pa, which is 3.1 times that of PBAT.

[0128] According to the test, in deionized water, the mass of the copolyester decreased by 60% after 180 days of degradation in deionized water, and in PBS buffer containing CALB enzyme, the mass of the copolyester decreased by 90% after 30 days of degradation.

[0129] Embodiment 4 The preparation method of a degradable long-chain random copolyester (hereinafter referred to as copolyester) provided in this embodiment comprises the following steps:

[0130] (1) Preparation of a pyrrolidone ring-containing monomer containing an oxygen ether bond: 2.1 mol of itaconic acid and 1.0 mol of 1,1′-oxybis(methylamine) were dissolved in water, stirred, condensed and refluxed at 130° C. for 48 h, and then excess water was removed, precipitated in cold methanol, and washed several times to obtain a pyrrolidone ring-containing monomer, named OPA.

[0131] (2) Preparation of polyester oligomers by esterification reaction: 0.2 mol of pyrrolidone ring-containing monomer OPA, 0.8 mol of tetracosyl diacid, 0.9 mol of tetracosyl glycol, 0.6 mol of propylene glycol, and 360 mg of zinc acetate were first added to a reactor, and the temperature was gradually raised to 200° C. under the protection of high-purity nitrogen and reacted for 6 h until the water content produced exceeded 90% of the theoretical value, thereby obtaining a polyester oligomer.

[0132] (3) Preparation of copolyester by melt polycondensation reaction: 125 mg of polycondensation catalyst dibutyltin oxide and 250 mg of stabilizer triisooctyl phosphite were added to the oligomer obtained in step (2), and the pressure was gradually reduced and the temperature was increased. After 30 minutes, the vacuum degree of the reactor reached 5 Pa, and the reaction temperature was maintained at 230° C. After 24 hours, the polymerization reaction was terminated after the rated stirring torque reached 200 N·cm to obtain a copolyester. The structure 4-4 was determined by infrared, nuclear magnetic resonance and other characterizations as follows:

[0133]

[0134] Wherein, x and y are both integers of 1-10, m is an integer of 20-100, and x:y=2:8;

[0135] After testing, the copolyester has an intrinsic viscosity of 1.26 dL / g, a weight-average molecular weight of 198745 g / moL, a dispersity of 2.3, a melting peak temperature of 90.0°C, a melting enthalpy of 84.2 J / g, a crystallization peak temperature of 62.1°C, and a crystallization enthalpy of 84.0 / g.

[0136] The test results show that the modulus of the copolyester reaches 800MPa, the strength exceeds 28MPa, and the elongation at break exceeds 500%. The test results show that the surface contact angle of the copolyester is 85°, and the water vapor barrier coefficient is 4.6493×10 -14 g cm / cm 2 ·s·Pa, which is 8 times that of PBAT.

[0137] According to the test, in deionized water, the mass of the copolyester decreased by 21% after 180 days of degradation in deionized water, and in PBS buffer containing CALB enzyme, the mass of the copolyester decreased by 30% after 30 days of degradation.

[0138] Example 5 The preparation method of a degradable long-chain random copolyester (hereinafter referred to as copolyester) provided in this example comprises the following steps:

[0139] (1) Preparation of a pyrrolidone ring-containing monomer containing an oxygen ether bond: 2.0 mol of itaconic acid and 1.0 mol of 2,2′-oxybis(ethylamine) were dissolved in water, stirred, condensed and refluxed at 180° C. for 24 h, and then excess water was removed, precipitated in cold methanol, and washed several times to obtain a pyrrolidone ring-containing monomer, which was named EOPA.

[0140] (2) Preparation of polyester oligomers by esterification reaction: First, 0.3 mol of pyrrolidone ring-containing monomer EOPA, 0.7 mol of octadecyl diacid, 1.03 mol of tetradecyl glycol, 0.37 mol of propylene glycol, and 200 mg of stannous oxalate were added to the reactor. Under the protection of high-purity nitrogen, the temperature was gradually raised to 190° C. and reacted for 6 hours until the water content generated exceeded 90% of the theoretical value, thereby obtaining a polyester oligomer.

[0141] (3) Preparation of copolyester by melt polycondensation reaction: 185 mg of polycondensation catalyst zinc acetate and 250 mg of stabilizer triisooctyl phosphite were added to the oligomer obtained in step (2), and the pressure was gradually reduced and the temperature was increased. After 30 minutes, the vacuum degree of the reactor reached 5 Pa, and the reaction temperature was maintained at 210° C. After 12 hours, the polymerization reaction was terminated after the rated stirring torque reached 200 N·cm to obtain a copolyester. The structure of the copolyester was determined by infrared, nuclear magnetic resonance and other characterizations as shown in Formula 4-5;

[0142]

[0143] Wherein, x and y are both integers of 1-10, m is an integer of 20-100, and x:y=3:7;

[0144] After testing, the copolyester has an intrinsic viscosity of 1.15 dL / g, a weight-average molecular weight of 141917 / moL, a dispersity of 2.0, a melting peak temperature of 81.7°C, a melting enthalpy of 87.3 J / g, a crystallization peak temperature of 66.8°C, and a crystallization enthalpy of 87.1 J / g.

[0145] The test results show that the modulus of the copolyester reaches 300MPa, the strength exceeds 15MPa, and the elongation at break exceeds 700%. The test results show that the surface contact angle of the copolyester is 75°, and the water vapor barrier coefficient is 8.023×10 -14 g cm / cm 2 ·s·Pa, which is 4.4 times that of PBAT.

[0146] After testing, in deionized water, the mass of the copolyester decreased by 26% after 180 days of degradation in deionized water. In PBS buffer containing CALB enzyme, the mass of the copolyester decreased by 43% after 30 days of degradation.

[0147] Example 6 The preparation method of a degradable long-chain random copolyester (hereinafter referred to as copolyester) provided in this example comprises the following steps:

[0148] (1) Preparation of a pyrrolidone ring-containing monomer containing an oxygen ether bond: 1.8 mol of itaconic acid and 1.0 mol of 1,8-diamino-3,6-dioxaoctane were dissolved in water, stirred, condensed and refluxed at 145°C for 40 h, and then excess water was removed, precipitated in cold methanol, and washed several times to obtain a pyrrolidone diacid monomer, named DOPA.

[0149] (2) Preparation of polyester oligomers by esterification reaction: First, 0.1 mol of pyrrolidone ring-containing monomer DOPA, 0.9 mol of dimethyl arachidyl ester, 0.9 mol of dodecyl glycol, 0.7 mol of propylene glycol, and 145 mg of tetraisopropyl titanate were added to the reactor. Under the protection of high-purity nitrogen, the temperature was gradually raised to 175° C. and reacted for 6 hours until the content of the generated water and methanol mixture exceeded 90% of the theoretical value, thereby obtaining polyester oligomers.

[0150] (3) Preparation of copolyester by melt polycondensation reaction: 320 mg of polycondensation catalyst dibutyltin dilaurate and 330 mg of stabilizer triisooctyl phosphite were added to the oligomer obtained in step (2), and the pressure was gradually reduced and the temperature was increased. After 30 minutes, the vacuum degree of the reactor reached 5 Pa, and the reaction temperature was maintained at 200° C. After 8 hours, the polymerization reaction was terminated after the rated stirring torque reached 200 N·cm to obtain a copolyester. The structure of the copolyester was determined by infrared, nuclear magnetic resonance and other characterizations as shown in Formula 4-6;

[0151]

[0152] Wherein, x and y are both integers of 1-10, m is an integer of 20-100, and x:y=1:9;

[0153] After testing, the copolyester has an intrinsic viscosity of 1.19 dL / g, a weight-average molecular weight of 168293 / moL, a dispersity of 2.0, a melting peak temperature of 80.2°C, a melting enthalpy of 77.6 J / g, a crystallization peak temperature of 64.7°C, and a crystallization enthalpy of 76.1 J / g.

[0154] The test results show that the modulus of the copolyester reaches 400MPa, the strength exceeds 20MPa, and the elongation at break exceeds 700%. The test results show that the surface contact angle of the copolyester is 78°, and the water vapor barrier coefficient is 7.061×10 -14 g cm / cm 2 ·s·Pa, which is 5 times that of PBAT.

[0155] According to the test, in deionized water, the mass of the copolyester decreased by 24% after 180 days of degradation in deionized water, and in PBS buffer containing CALB enzyme, the mass of the copolyester decreased by 41% after 30 days of degradation.

[0156] Example 7 The preparation method of a degradable long-chain random copolyester (hereinafter referred to as copolyester) provided in this example comprises the following steps:

[0157] (1) Preparation of a pyrrolidone ring-containing monomer containing an oxygen ether bond: 1.9 mol of itaconic acid and 1.0 mol of 1,8-diamino-3,6-dioxaoctane were dissolved in water, stirred, condensed and refluxed at 150° C. for 40 h, and then excess water was removed, precipitated in cold methanol, and washed several times to obtain a pyrrolidone diacid monomer, named DOPA.

[0158] (2) Preparation of polyester oligomers by esterification reaction: First, 0.2 mol of pyrrolidone ring-containing monomer DOPA, 0.8 mol of dimethyl arachidyl ester, 0.9 mol of dodecyl glycol, 0.7 mol of propylene glycol, and 145 mg of tetraisopropyl titanate were added to the reactor. Under the protection of high-purity nitrogen, the temperature was gradually raised to 185° C. and reacted for 5 hours until the content of the generated water and methanol mixture exceeded 90% of the theoretical value, thereby obtaining polyester oligomers.

[0159] (3) Preparation of copolyester by melt polycondensation reaction: 145 mg of tetraisopropyl titanate as a catalyst and 330 mg of triisooctyl phosphite as a stabilizer were added to the oligomer obtained in step (2), and the pressure was gradually reduced and the temperature was increased. After 30 minutes, the vacuum degree of the reactor reached 5 Pa, and the reaction temperature was maintained at 200° C. After 8 hours, the polymerization reaction was terminated after the rated stirring torque reached 200 N·cm to obtain a copolyester. The structure of the copolyester was determined by infrared, nuclear magnetic resonance and other characterizations as shown in Formula 4-7;

[0160]

[0161] Wherein, x and y are both integers of 1-10, m is an integer of 20-100, and x:y=2:8;

[0162] After testing, the copolyester has an intrinsic viscosity of 1.19 dL / g, a weight-average molecular weight of 175610 g / moL, a dispersity of 2.1, a melting peak temperature of 79.1°C, a melting enthalpy of 75.4 J / g, a crystallization peak temperature of 64.5°C, and a crystallization enthalpy of 75.4 J / g.

[0163] The test results show that the modulus of the copolyester reaches 400MPa, the strength exceeds 20MPa, and the elongation at break exceeds 700%. The test results show that the surface contact angle of the copolyester is 78°, and the water vapor barrier coefficient is 7.059×10 -14 g cm / cm 2 ·s·Pa, which is 5 times that of PBAT.

[0164] According to the test, in deionized water, the mass of the copolyester decreased by 23% after 180 days of degradation in deionized water, and in PBS buffer containing CALB enzyme, the mass of the copolyester decreased by 40% after 30 days of degradation.

[0165] Comparative Example 1 The preparation method of a homopolyester (defined as PTDD, hereinafter referred to as homopolyester) provided in this comparative example comprises the following steps:

[0166] (1) 1 mol of tetradecyl diacid, 1.05 mol of tetradecyl glycol, 0.55 mol of propylene glycol, and 100 mg of tetrabutyl titanate are placed in a reactor, and under the protection of high-purity nitrogen, the temperature is gradually raised to 200° C. for reaction for 4 hours until the water content generated exceeds 90% of the theoretical value, thereby obtaining a polyester oligomer.

[0167] (2) Add 145 mg of polycondensation catalyst antimony trioxide and 650 mg of stabilizer diphenyl phosphate to the above polyester oligomer, gradually increase the temperature to 220°C, gradually reduce the vacuum degree to 5 Pa, and react for 18 hours to obtain homopolyester PTDD. Characterized by IR, NMR, etc., its structure is determined as shown in Formula 5-1.

[0168]

[0169] After testing, the intrinsic viscosity of the homopolyester is 1.27dL / g, the weight-average molecular weight is 153525g / moL, the dispersity is 2.0, the melting peak temperature is 93.4°C, the melting enthalpy is 95.4J / g, the crystallization peak temperature is 71.9°C, and the crystallization enthalpy is 95.4J / g.

[0170] The test results show that the modulus of the homopolyester reaches 700MPa, the strength exceeds 35MPa, and the elongation at break exceeds 600%. The test results show that the surface contact angle of the homopolyester is 95°, and the water vapor barrier coefficient is 5.138×10 -14 g cm / cm 2 ·s·Pa.

[0171] After testing, in deionized water, the homopolyester had almost no mass loss after being degraded in deionized water for 180 days. In the PBS buffer of CALB enzyme, the homopolyester also had almost no mass loss after being degraded for 30 days.

[0172] Comparative Example 2 The preparation method of a copolyester provided in this comparative example is basically the same as that in Example 1, except that 1,1′-thiobis(methylamine) in step (1) is replaced by 1,3-propylenediamine to finally obtain a copolyester, and its structure is determined to be as shown in Formula 5-2 through characterization by infrared, nuclear magnetic resonance, etc.

[0173]

[0174] The test showed that the surface contact angle of the obtained copolyester with water was 88°, and the water vapor barrier coefficient was 4.763×10 -14 g cm / cm 2 ·s·Pa, which is 7.4 times that of PBAT. At the same time, in deionized water, the mass of the copolyester decreased by 13% after 180 days of degradation in deionized water, and in PBS buffer of CALB enzyme, the mass of the copolyester decreased by 15% after 30 days of degradation. Compared with Example 1, the polarity of the synthesized diacid monomer is reduced when it does not contain a thioether bond, resulting in a larger surface contact angle between the copolyester and water, an improved water vapor barrier, a poorer hydrophilicity of the material, and a reduced degradation performance.

[0175] Comparative Example 3 The preparation method of a copolyester provided in this comparative example is basically the same as that in Example 1, except that: 0.1 mole of the pyrrolidone ring-containing monomer SPA in step (2) is replaced with thiodiacetic acid, and finally a copolyester is obtained. The copolyester is characterized by infrared, nuclear magnetic resonance, etc., and its structure is determined as shown in Formula 5-3.

[0176]

[0177] The test results show that the surface contact angle of the obtained copolyester is 87° and the water vapor barrier coefficient is 4.797×10 -14 g cm / cm 2·s·Pa, which is 7.4 times that of PBAT. At the same time, in deionized water, the mass of the copolyester decreased by 14% after 180 days of degradation in deionized water, and in the PBS buffer of CALB enzyme, the mass of the copolyester decreased by 16% after 30 days of degradation. Compared with Example 1, the monomer used in this comparative example contains a thioether bond but no pyrrolidone structure, and its polarity is reduced, resulting in a larger surface contact angle between the copolyester and water, an improved water vapor barrier, a poorer hydrophilicity of the material, and a reduced degradation performance.

[0178] Comparative Example 4 The preparation method of a copolyester provided in this comparative example is basically the same as that in Example 1, except that propylene glycol in step (2) is replaced by ethylene glycol to finally obtain a copolyester.

[0179] After testing, the intrinsic viscosity of the obtained copolyester is 1.0dL / g, the weight average molecular weight is 103540g / moL, and the dispersity is 1.9. At the same time, the modulus of the copolyester reaches 550MPa, the strength exceeds 13MPa, and the elongation at break exceeds 450%. Compared with Example 1, in this comparative example, the low-boiling diol is replaced by propylene glycol with ethylene glycol, and the molecular weight of the copolyester is reduced within the same polycondensation time, and the mechanical properties are reduced. This is because ethylene glycol generates diethylene glycol at high temperature, which makes it difficult to remove the diol and reduces the efficiency of the polymerization reaction.

[0180] Comparative Example 5 The preparation method of a copolyester provided in this comparative example is basically the same as that in Example 1, except that: propylene glycol in step (2) is replaced by butanediol to finally obtain a copolyester.

[0181] After testing, the intrinsic viscosity of the obtained copolyester is 0.98dL / g, the weight average molecular weight is 95460g / moL, and the dispersity is 1.8. At the same time, the modulus of the copolyester reaches 550MPa, the strength exceeds 15MPa, and the elongation at break exceeds 490%. Compared with Example 1, the low boiling point diol in this comparative example is replaced by butanediol from propylene glycol. Since butanediol itself has a high boiling point, it cannot be removed as quickly as propylene glycol during the polycondensation process to assist the growth of the molecular chain. Therefore, under the same reaction conditions, a large amount of butanediol will still remain, resulting in difficulty in increasing the molecular weight of the product, resulting in reduced mechanical properties of the material.

[0182] Comparative Example 6 The preparation method of a copolyester provided in this comparative example is basically the same as that in Example 1, except that: the feed ratio in step (2) is adjusted to 0.5 mol of pyrrolidone ring-containing monomer SPA, 0.5 mol of tetradecyl diacid, 1.05 mol of tetradecyl glycol and 0.55 mol of propylene glycol, and finally a copolyester is obtained. The structure is determined by infrared, nuclear magnetic resonance and other characterizations as follows:

[0183] As shown in formula 5-4.

[0184]

[0185] After testing, the intrinsic viscosity of the obtained copolyester is 1.25dL / g, the weight average molecular weight is 176342g / moL, the dispersion is 2.0, the melting peak temperature is 55℃, the melting enthalpy is 43.2J / g, the crystallization peak temperature is 43℃, and the crystallization enthalpy is 46.2J / g. At the same time, the modulus of the copolyester reaches 120MPa, the strength exceeds 15MPa, and the elongation at break exceeds 500%.

[0186] Compared with Example 1, this comparative example introduces too much diacid monomer containing a pyrrolidone ring, which destroys the crystallization ability of the material and leads to a decrease in thermal, mechanical and barrier properties.

[0187] Comparative Example 7 The preparation method of a copolyester provided in this comparative example is basically the same as that in Example 1, except that the feed ratio in step (2) is adjusted to 0.05 mol of pyrrolidone ring-containing monomer SPA, 0.95 mol of tetradecyl diacid, 1.05 mol of tetradecyl glycol, and 0.55 mol of propylene glycol, and finally a copolyester is obtained. Characterization by infrared, nuclear magnetic resonance, etc. determines that its structure is shown in Formula 5-4.

[0188] The test results show that the surface contact angle of the obtained copolyester is 93° and the water vapor barrier coefficient is 5.127×10 -14 g cm / cm 2 ·s·Pa. Meanwhile, in deionized water, the copolyester had almost no mass loss after being degraded in deionized water for 180 days, and in PBS buffer containing CALB enzyme, the copolyester had almost no mass loss after being degraded for 30 days.

[0189] Compared with Example 1, the amount of the diacid monomer containing a pyrrolidone ring introduced in this comparative example is too low, resulting in excessively high hydrophilicity of the material, and failing to effectively improve the degradation performance of the copolyester.

[0190] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.

[0191] The various aspects, embodiments, features and examples of the present application should be considered as illustrative in all aspects and are not intended to limit the present application, the scope of which is defined solely by the claims. Other embodiments, modifications and uses will be apparent to those skilled in the art without departing from the spirit and scope of the present application as claimed.

[0192] Although the present application has been described with reference to illustrative embodiments, it will be appreciated by those skilled in the art that various other changes, omissions, and / or additions may be made and that elements of the described embodiments may be substituted with substantial equivalents without departing from the spirit and scope of the present application. In addition, many modifications may be made to adapt a particular situation or material to the teachings of the present application without departing from the scope of the present application. Therefore, it is not intended herein to limit the present application to the disclosed specific embodiments for carrying out the present application, but rather it is intended that the present application will include all embodiments within the scope of the appended claims.

Claims

1. A monomer containing a pyrrolidone ring, characterized in that: The monomer has a structure shown in Formula 1, Here, R contains an ether bond or a thioether bond.

2. The pyrrolidone ring-containing monomer according to claim 1, characterized in that R includes at least one of the following structural units:

3. A method for preparing a monomer containing a pyrrolidone ring, characterized in that: include: Allowing itaconic acid and diamine to undergo Michael addition reaction to obtain the monomer; Wherein, the monomer has a structure shown in Formula 1, and the diamine has a structure shown in Formula 2, R contains an ether bond or a thioether bond.

4. The preparation method according to claim 3, characterized in that: R includes at least one of the following structural units: And / or, the preparation method specifically comprises: subjecting a mixed reaction system comprising itaconic acid, a diamine and water to the Michael addition reaction at 130-180° C. to obtain the monomer; And / or, the reaction time is 24-48h; And / or, the molar ratio of itaconic acid to diamine is 1.8-2.2:

1.

5. A degradable long-chain random copolyester, characterized in that: The copolyester has a structure shown in Formula 3, Among them, R1 contains an ether bond or a thioether bond, R2 and R3 include straight-chain alkyl groups containing 10-30 carbon atoms, x and y are both integers of 1-10, m is an integer of 20-100, and the molar ratio of R1 to R3 is 1:9-3:

7.

6. The degradable long-chain random copolyester according to claim 5, characterized in that: R1 includes at least one of the following structural units:

7. The degradable long-chain random copolyester according to claim 5, characterized in that: The degradable long-chain random copolyester has a weight average molecular weight higher than 120,000 g / mol, a dispersity of 2.0-3.0, and an intrinsic viscosity of 1.15-1.35 dL / g; And / or, the melt crystallization enthalpy or melting enthalpy of the degradable long-chain random copolyester is above 50 J / g, the melting point is above 60° C., the Young's modulus is 200-800 MPa; the water vapor barrier coefficient is 1.10×10 -13 -4.65×10 -14 g cm / cm 2 ·s·Pa; And / or, the water contact angle of the degradable long-chain random copolyester is 85°-70°, the mass loss rate after degradation in water for 6 months is 20%-60%, and the mass loss rate after degradation by Antarctic Candida lipase b for 30 days is 30%-90%.

8. The degradable long-chain random copolyester according to claim 7, characterized in that: The weight average molecular weight of the degradable long-chain random copolyester is 140,000-200,000 g / mol.

9. A method for preparing a degradable long-chain random copolyester, characterized in that: include: subjecting a first mixed system comprising monomer A, monomer B, monomer C, monomer D and an esterification catalyst to an esterification reaction or an ester exchange reaction to obtain an intermediate product; subjecting the second mixed system comprising the intermediate product, a polycondensation catalyst and a stabilizer to a polycondensation reaction to obtain the degradable long-chain random copolyester; Wherein, the monomer A includes an aliphatic dibasic acid or an ester thereof containing R3, the monomer B includes a long-chain diol containing R2, the monomer C includes a pyrrolidone ring-containing monomer described in any one of claims 1-2, the monomer D includes propylene glycol, and R2 and R3 include alkyl groups containing 10-30 carbon atoms.

10. The preparation method according to claim 9, characterized in that: In the first mixed system, the ratio of the sum of the molar amounts of the monomer A and the monomer C to the sum of the molar amounts of the monomer B and the monomer D is 1:m, the molar ratio of the monomer A to the monomer C is 1:9-3:7, and the molar ratio of the monomer B to the monomer D is n:(mn), wherein m=1.4-1.6, n=0.9-1.1; And / or, the esterification reaction or transesterification reaction is carried out under a protective atmosphere and the reaction temperature is 175-200°C; And / or, the reaction time of the esterification reaction or transesterification reaction is 4h-6h; and / or, when the esterification reaction or transesterification reaction is carried out until the yield of by-product water or methanol is greater than or equal to 90% of the theoretical yield, the intermediate product is obtained; and / or, in the first mixed system, the ratio of the esterification catalyst to the sum of the molar amounts of the monomer A and the monomer C is 0.5:1000-2.0:1000; And / or, the esterification catalyst includes any one or more combinations of titanium catalysts, antimony catalysts, tin catalysts, and acetic acid catalysts, wherein the titanium catalyst includes any one or more combinations of tetrabutyl titanate, isopropyl titanate, isobutyl titanate, propylene glycol titanium, and titanium dioxide; the antimony catalyst includes any one or more combinations of antimony trioxide, antimony acetate, and propylene glycol antimony; the tin catalyst includes any one or more combinations of butyl stannoic acid, dibutyl tin oxide, stannous isooctanoate, stannous oxalate, dibutyl tin diacetate, dibutyl tin dilaurate, and dioctyl tin oxide; the acetic acid catalyst includes any one or more combinations of lithium acetate, potassium acetate, calcium acetate, magnesium acetate, barium acetate, zinc acetate, cobalt acetate, antimony acetate, lead acetate, and manganese acetate.

11. The preparation method according to claim 9, characterized in that: The ratio of the polycondensation catalyst to the sum of the molar amounts of the monomer A and the monomer C is 0.1:1000-0.5:1000; and / or, the ratio of the stabilizer to the sum of the molar amounts of the monomer A and the monomer C is 0.5:1000-2.0:1000; And / or, the reaction temperature of the polycondensation reaction is 200-230°C; And / or, the reaction time of the polycondensation reaction is 8h-24h; And / or, the polycondensation reaction is carried out under a vacuum degree of less than 5 Pa; And / or, the polycondensation catalyst includes any one or more combinations of titanium catalysts, antimony catalysts, tin catalysts, and acetic acid catalysts, wherein the titanium catalyst includes any one or more combinations of tetrabutyl titanate, isopropyl titanate, isobutyl titanate, titanium propylene glycol, and titanium dioxide; the antimony catalyst includes any one or more combinations of antimony trioxide, antimony acetate, and antimony propylene glycol; the tin catalyst includes any one or more combinations of butyl stannic acid, dibutyl tin oxide, stannous isooctanoate, stannous oxalate, dibutyl tin diacetate, dibutyl tin dilaurate, and dioctyl tin oxide; the acetic acid catalyst includes any one or more combinations of lithium acetate, potassium acetate, calcium acetate, magnesium acetate, barium acetate, zinc acetate, cobalt acetate, antimony acetate, lead acetate, and manganese acetate; And / or, the stabilizer includes antioxidant 1010, antioxidant 1076, antioxidant 1500, antioxidant 425, heat stabilizer 330, heat stabilizer 1178, heat stabilizer 618, heat stabilizer 626, heat stabilizer 168, trimethyl phosphite, triethyl phosphite, triisooctyl phosphite, triisodecyl phosphite, trilauryl phosphite, tritridecyl phosphite, trioctadecyl phosphite, triphenyl phosphite, tri-p-tolyl phosphite, diphenyl tridecyl phosphite, tri(2,4-di-tert-butyl phosphite) any one or more combinations of: dibutylbenzene) ester, di(2,4-di-p-isopropylphenyl) pentaerythritol bisphosphite phosphoric acid, pentaerythritol tetraphosphite phenyl tridecyl, pentaerythritol diphosphite tridecyl, pentaerythritol diisodecyl phosphite, tetraphenyl dipropylene glycol diphosphite, phosphoric acid, phosphorous acid, polyphosphoric acid and triethyl phosphonoacetate, light stabilizer 791, light stabilizer 700, light stabilizer 783, light stabilizer 119, light stabilizer 770, light stabilizer 622, light stabilizer 944, and light stabilizer 1164.

Citation Information

Patent Citations

  • Macromolecule with main chain containing thioether group and synthesis method thereof

    CN114854017A

  • Bio-based branching agent, preparation method and preparation method of low-melt-index long-chain branched poly (butylene terephthalate)-butylene adipate

    CN118344275A

  • Use of 2-pyrrolidone compounds as a cosmetic active solubilization agent including assets of care for the keratin fibers

    FR2961100A1

  • Plastic composition comprising a vinyl resin and a bis-nu-substituted pyrrolidinone

    US2993021A

  • Process of making an isocyanurate foam

    US4315079A