Anti-ultraviolet compatilizer, modified nylon and preparation method and application of modified nylon
By introducing norbornene dianhydride grafted ultraviolet absorber into polyamide materials, the performance deterioration of polyamide materials under environmental factors such as ultraviolet rays is solved, and the compatibility and dispersion of glass fiber and nylon are improved, thereby enhancing the enhancement of the compatibility and dispersion of glass fiber and nylon. The toughening and UV resistance of the material are extended.
Patent Information
- Application Number
- CN202411404284.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-09
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-10-09
AI Technical Summary
The existing polyamide materials have deteriorated performance under environmental factors such as ultraviolet rays, moisture, and temperature. The compatibility and dispersion of glass fibers, polyolefin elastomers and anti-ultraviolet additives in the system are insufficient, which affects the service life of the material.
By introducing norbornene dianhydride grafted UV absorber into the polyamide material, it uses its esterification reaction with glass fiber and polyolefin elastomer to form an anti-UV compatibility agent, and granulates through a twin screw extrusion device. Improve the compatibility and dispersion of glass fiber with nylon.
It significantly improves the compatibility and dispersion of glass fiber with nylon, enhances the toughening and UV resistance of the material, and extends the service life of the material.
Smart Images

Figure CN119080988A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials, and specifically relates to an anti-ultraviolet compatibilizer, modified nylon and a preparation method and application thereof. Background Art
[0002] Polyamide (commonly known as nylon, PA for short) is the polymer material with the largest output, the most types and the widest application among the five major engineering plastics. With its excellent mechanical properties, wear and corrosion resistance, easy processing and molding, easy dyeing, self-lubrication and other characteristics, it has become an indispensable structural material for domestic and foreign automobile, machinery, electronics, national defense, aerospace, clothing, packaging and other industries. However, due to the presence of a large number of amide groups (-CONH-) in the main chain structure of polyamide, the chromophore has a strong polarity and is easily affected by environmental factors such as ultraviolet rays, moisture, and temperature, which causes the material performance to deteriorate, thereby affecting the service life of the material. Considering the service life of actual applications and the application of long-term outdoor exposure environment, introducing anti-ultraviolet additives in the modification stage of polyamide resin is one of the most convenient means. Combined with the current industrialization status of conventional glass fiber reinforcement modification and polyolefin elastomer (POE) toughening modification of polyamide materials, it is crucial to improve the compatibility between glass fiber, POE and anti-ultraviolet additives and their dispersibility in the system. Summary of the invention
[0003] The main purpose of the present invention is to provide an anti-ultraviolet compatibilizer, modified nylon and preparation method and application thereof, so as to overcome the deficiencies of the prior art.
[0004] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:
[0005] The embodiment of the present invention provides a method for preparing an anti-ultraviolet compatibilizer, which comprises:
[0006] The mixed reaction system including at least nadic anhydride, a hydroxyl-containing ultraviolet absorber, and a catalyst is subjected to an esterification reaction to obtain a nadic anhydride-grafted ultraviolet absorber;
[0007] Furthermore, the polyolefin elastomer, the grafted ultraviolet absorber of nadic anhydride, the nadic anhydride and the initiator are mixed and input into a twin-screw extruder for granulation to obtain an anti-ultraviolet compatibilizer.
[0008] The embodiment of the present invention also provides an anti-ultraviolet compatibilizer prepared by the aforementioned preparation method.
[0009] The embodiment of the present invention also provides the use of the aforementioned anti-ultraviolet compatibilizer in the preparation of modified nylon.
[0010] The embodiment of the present invention further provides a modified nylon, wherein the raw materials for preparing the modified nylon include the following components calculated by mass: 55-65 parts of nylon, 25-40 parts of glass fiber, 3-6 parts of anti-ultraviolet compatibilizer and 0.2-0.5 parts of antioxidant;
[0011] Wherein, the anti-ultraviolet compatibilizer includes the aforementioned anti-ultraviolet compatibilizer.
[0012] The present invention also provides a method for preparing the modified nylon, which comprises:
[0013] Nylon, glass fiber, anti-ultraviolet compatibilizer and antioxidant are placed in a high-speed mixing device and mixed evenly, and then the obtained materials are input into a twin-screw extruder for granulation to obtain modified nylon.
[0014] Compared with the prior art, the present invention has the following beneficial effects:
[0015] (1) The anti-ultraviolet compatibilizer provided by the present invention is grafted with a rigid anhydride structure, which can react with the hydroxyl group on the surface of the glass fiber and the terminal amine group of PA66; secondly, the ultraviolet absorber structure in the NA-g-UV structure grafted with POE has a large number of intramolecular hydrogen bond structures (such as one or more of carbonyl, ester, hydroxyl, NN bond, C==N bond, etc.), and these groups can form intermolecular hydrogen bonds with the amide group in the PA66 molecular chain, thereby improving the compatibility of the two;
[0016] (2) The anti-ultraviolet compatibilizer in the present invention can act as a link between glass fiber and nylon, thereby enabling the glass fiber and the anti-ultraviolet compatibilizer to obtain excellent dispersion in the entire system, so as to maximize their strengthening, toughening and anti-ultraviolet effects. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0018] Figure 1 is a schematic diagram of the reaction for preparing NA-g-UV 531 in Example 1 of the present invention;
[0019] Figure 2 It is a reaction schematic diagram of preparing the anti-ultraviolet compatibilizer in Example 1 of the present invention. DETAILED DESCRIPTION
[0020] In view of the defects of the prior art, the inventor of this case has proposed the technical solution of the present invention after long-term research and extensive practice. The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0021] Specifically, as one aspect of the technical solution of the present invention, a method for preparing an anti-ultraviolet compatibilizer involves:
[0022] The mixed reaction system including at least nadic anhydride, a hydroxyl-containing ultraviolet absorber, and a catalyst is subjected to an esterification reaction to obtain a nadic anhydride-grafted ultraviolet absorber;
[0023] Furthermore, the polyolefin elastomer, the grafted ultraviolet absorber of nadic anhydride, the nadic anhydride and the initiator are mixed and input into a twin-screw extruder for granulation to obtain an anti-ultraviolet compatibilizer.
[0024] In some preferred embodiments, the preparation method specifically includes: subjecting a mixed reaction system comprising nadic anhydride, a hydroxyl-containing ultraviolet absorber, a catalyst, and a solvent to an esterification reaction at 60-65° C. for 3 to 4 hours, and then filtering, washing, and drying to obtain a nadic anhydride-grafted ultraviolet absorber.
[0025] Further, the hydroxyl-containing ultraviolet absorber includes any one or more combinations of triazine ultraviolet absorbers, salicylate ultraviolet absorbers, benzotriazole ultraviolet absorbers, and benzophenone ultraviolet absorbers, but is not limited thereto.
[0026] Furthermore, the hydroxyl-containing ultraviolet absorber includes any one or more combinations of triazine ultraviolet absorbers, salicylate ultraviolet absorbers, and benzotriazole ultraviolet absorbers, but is not limited thereto.
[0027] Furthermore, the benzophenone ultraviolet absorber includes any one or more combinations of UV-531, UV-1009, UV-981, and UV-2126, but is not limited thereto.
[0028] Furthermore, the triazine ultraviolet absorber includes any one or more combinations of UV-1577, UV-1164, UV-400, and triazine-5, but is not limited thereto.
[0029] Furthermore, the salicylate UV absorber includes any one or more combinations of ethylhexyl salicylate, octyl salicylate, phenyl salicylate, isohexadecanyl salicylate, hexyl salicylate, and benzyl salicylate, but is not limited thereto.
[0030] Furthermore, the benzotriazole ultraviolet absorber includes any one or more combinations of UV-P, UV-326, UV-327, and UV-329, but is not limited thereto.
[0031] Further, the catalyst includes triethylamine, but is not limited thereto.
[0032] Further, the solvent includes dichloromethane, but is not limited thereto.
[0033] Furthermore, the molar ratio of the nadic anhydride to the hydroxyl-containing ultraviolet absorber is 1:1.5-2.5.
[0034] In some preferred embodiments, the mass ratio of the polyolefin elastomer, the nadic anhydride grafted UV absorber, the nadic anhydride and the initiator is 100:3N6:3-6:0.6-1.
[0035] In some preferred embodiments, the initiator includes a 2,2,6,6-tetramethyl-1-oxypiperidine (TEMPO)-di-tert-butyl peroxide (DTBP) complex system, but is not limited thereto.
[0036] In some preferred embodiments, the process parameters adopted by the twin-screw extruder include: processing temperature of 200-225°C, screw speed of 260-300rpm, and feed speed of 10-15rpm.
[0037] In some more specific embodiments, the method for preparing the anti-ultraviolet compatibilizer comprises the following steps:
[0038] Step (1): using triethylamine as a catalyst and dichloromethane as a solvent, esterification reaction is carried out at 60°C with nadic anhydride (NA) and a hydroxyl-containing ultraviolet absorber (UV) in a molar ratio of 1:2, and the reaction time is controlled to be 3 to 4 hours. After suction filtration, washing and drying, a nadic anhydride grafted ultraviolet absorber product (NA-g-UV) is obtained.
[0039] Step (2): 100 parts of polyolefin elastomer (POE), 3-6 parts of NA-g-UV, 3-6 parts of nadic anhydride, and 0.6-1 part of initiator are weighed by weight, and mixed evenly in a high-speed mixer. The materials are added to the feed port, and enter the twin-screw extruder from the feed port at a set speed, and the reaction extrusion is carried out according to the set conditions. The extrudate is cooled in a cooling water tank and pelletized to obtain POE grafted NA and NA-g-UV products.
[0040] Preferably, the hydroxyl-containing UV absorber is selected from one or more of benzophenone, triazine, salicylate, and benzotriazole UV absorbers.
[0041] Preferably, the initiator is selected from a 2,2,6,6-tetramethyl-1-oxypiperidine (TEMPO)-di-tert-butyl peroxide (DTBP) complex system.
[0042] Preferably, the setting conditions are as follows: the processing temperature is set at 200-225°C, the screw speed is 260-300rpm, and the feeding speed is 10rpm.
[0043] Another aspect of the embodiments of the present invention further provides an anti-ultraviolet compatibilizer obtained by the aforementioned preparation method.
[0044] Another aspect of the embodiments of the present invention further provides the use of the aforementioned anti-ultraviolet compatibilizer in the preparation of modified nylon.
[0045] Another aspect of the embodiment of the present invention further provides a modified nylon, wherein the raw materials for preparing the modified nylon include the following components calculated by mass: 55-65 parts of nylon, 25-40 parts of glass fiber, 3-6 parts of anti-ultraviolet compatibilizer and 0.2-0.5 parts of antioxidant;
[0046] Wherein, the anti-ultraviolet compatibilizer includes the aforementioned anti-ultraviolet compatibilizer.
[0047] In some preferred embodiments, the nylon includes nylon 66 and / or nylon 6, but is not limited thereto.
[0048] In some preferred embodiments, the antioxidant includes antioxidant 1098, but is not limited thereto.
[0049] Another aspect of the embodiments of the present invention further provides a method for preparing the aforementioned modified nylon, which comprises:
[0050] Nylon, glass fiber, anti-ultraviolet compatibilizer and antioxidant are placed in a high-speed mixing device and mixed evenly, and then the obtained materials are input into a twin-screw extruder for granulation to obtain modified nylon.
[0051] In some preferred embodiments, the process parameters adopted by the twin-screw extruder include: temperature of 240-280° C., screw speed of 260-300 rpm, and feed speed of 10 rpm.
[0052] In some more specific embodiments, the preparation method of the modified nylon includes: weighing 55-65 parts of nylon, 25-40 parts of glass fiber, 3-6 parts of anti-ultraviolet compatibilizer, and 0.2-0.5 parts of antioxidant 1098 into a high-speed mixer for mixing, and then placing in a twin-screw extruder after mixing, setting the extrusion temperature to 240-280°C, the screw speed to 260-300rpm, and the feed speed to 10rpm. The extrudate is cooled in a cooling water tank and then pelletized to obtain modified nylon pellets.
[0053] The technical solution of the present invention is further described in detail below in conjunction with several preferred embodiments and drawings. This embodiment is implemented on the premise of the technical solution of the invention, and a detailed implementation method and specific operation process are given, but the protection scope of the present invention is not limited to the following embodiments.
[0054] Unless otherwise specified, the experimental materials used in the following examples can be purchased from conventional biochemical reagent companies.
[0055] Example 1: An anti-ultraviolet compatibilizer of the present invention, the specific preparation method is as follows:
[0056] Step (1): With triethylamine as catalyst and dichloromethane as solvent, nadic anhydride (NA) and 2-hydroxy-4-n-octyloxybenzophenone (UV-531) are subjected to esterification reaction at 60°C in a molar ratio of 1:2, and the reaction time is controlled to be 3 to 4 hours. After suction filtration, washing and drying, the nadic anhydride grafted 2-hydroxy-4-n-octyloxybenzophenone product (NA-g-UV 531) is obtained.
[0057] Step (2): Weigh 100 parts of polyolefin elastomer, 8 parts of grafting monomer (4 parts of nadic anhydride + 4 parts of NA-g-UV 531), and 0.8 parts of TEMPO-DTBP initiator by mass, and mix them in a high-speed mixer. After mixing, add the materials to the feed port and add them to the twin-screw extruder from the feed port at a set speed of 10 rpm. The processing temperature is 205°C, and the temperature settings of each section of the twin-screw extruder are: 165°C, 175°C, 185°C, 195°C, 200°C, 200°C, 205°C, 205°C, 195°C, and the screw speed is 260 rpm. The extrudate is cooled in a cooling water tank and pelletized to obtain a grafted product. The raw material composition and processing conditions of this embodiment are listed in Table 1. The grafting rate and melt index of the compatibilizer are tested, and the test results are listed in Table 1. The reaction schematic diagram for preparing NA-g-UV 531 in this embodiment is shown in Figure 1. Figure 1 As shown, the reaction diagram for preparing the anti-ultraviolet compatibilizer is as follows Figure 2 shown.
[0058] Embodiment 2:
[0059] The component ratio and preparation method of the anti-ultraviolet compatibilizer of this embodiment are basically the same as those of Example 1, except that the ultraviolet absorber in this embodiment is UV-1577 (triazine, 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-hexyloxy-phenol). The raw material composition and processing conditions of this embodiment are listed in Table 1, and the grafting rate and melt index of the compatibilizer are tested, and the test results are listed in Table 1.
[0060] Embodiment 3:
[0061] The component ratio and preparation method of the anti-ultraviolet compatibilizer of this embodiment are basically the same as those of Example 1, except that the amount of initiator used in this embodiment is 0.6 parts. The raw material composition and processing conditions of this embodiment are listed in Table 1, and the grafting rate and melt index of the compatibilizer are tested, and the test results are listed in Table 1.
[0062] Embodiment 4:
[0063] The component ratio and preparation method of the anti-ultraviolet compatibilizer of this embodiment are basically the same as those of Example 1, except that the amount of grafting monomer used in this embodiment is 6 parts (3 parts of nadic anhydride + 3 parts of NA-g-UV 531). The raw material composition and processing conditions of this embodiment are listed in Table 1, and the grafting rate and melt index of the compatibilizer are tested, and the test results are listed in Table 1.
[0064] Embodiment 5:
[0065] The component ratio and preparation method of the anti-ultraviolet compatibilizer of this embodiment are basically the same as those of Example 1, except that the amount of grafting monomer used in this embodiment is 10 parts (5 parts of nadic anhydride + 5 parts of NA-g-UV 531). The raw material composition and processing conditions of this embodiment are listed in Table 1, and the grafting rate and melt index of the compatibilizer are tested, and the test results are listed in Table 1.
[0066] Embodiment 6:
[0067] The component ratio and preparation method of the anti-ultraviolet compatibilizer of this embodiment are basically the same as those of Example 1, except that the processing temperature in this embodiment is 215°C, and the temperature settings of each section of the twin-screw extruder are: 165°C, 175°C, 185°C, 195°C, 200°C, 205°C, 215°C, 215°C, 215°C, 200°C. The raw material composition and processing conditions of this embodiment are listed in Table 1, and the grafting rate and melt index of the compatibilizer are tested, and the test results are listed in Table 1.
[0068] Embodiment 7:
[0069] The component ratio and preparation method of the anti-ultraviolet compatibilizer of this embodiment are basically the same as those of Example 1, except that the screw speed in this embodiment is 300 rpm. The raw material composition and processing conditions of this embodiment are listed in Table 1, and the grafting rate and melt index of the compatibilizer are tested, and the test results are listed in Table 1.
[0070] Comparative Example 1:
[0071] The component ratio and preparation method of the anti-ultraviolet compatibilizer of this comparative example are basically the same as those of Example 1, except that the amount of initiator used in this comparative example is 1.2 parts. The raw material composition and processing conditions of this comparative example are listed in Table 1, and the grafting rate and melt index of the compatibilizer are tested, and the test results are listed in Table 1.
[0072] Comparative Example 2:
[0073] The component ratio and preparation method of the anti-ultraviolet compatibilizer of this comparative example are basically the same as those of Example 1, except that the processing temperature in this comparative example is 230°C, and the temperature settings of each section of the twin-screw extruder are: 165°C, 175°C, 185°C, 195°C, 220°C, 220°C, 230°C, 230°C, 230°C, 220°C. The raw material composition and processing conditions of this comparative example are listed in Table 1, and the grafting rate and melt index of the compatibilizer are tested, and the test results are listed in Table 1.
[0074] Comparative Example 3:
[0075] The component ratio and preparation method of the anti-ultraviolet compatibilizer of this comparative example are basically the same as those of Example 1, except that the screw speed in this comparative example is 350 rpm. The raw material composition and processing conditions of this comparative example are listed in Table 1, and the grafting rate and melt index of the compatibilizer are tested, and the test results are listed in Table 1.
[0076] Comparative Example 4:
[0077] The component ratio and preparation method of the anti-ultraviolet compatibilizer of this comparative example are basically the same as those of Example 1, except that the grafting monomer in this comparative example is 8 parts of nadic anhydride. The raw material composition and processing conditions of this comparative example are listed in Table 1, and the grafting rate and melt index of the compatibilizer are tested, and the test results are listed in Table 1.
[0078] Comparative Example 5:
[0079] The component ratio and preparation method of the anti-ultraviolet compatibilizer of this comparative example are basically the same as those of Example 1, except that the grafting monomer in this comparative example is 8 parts of NA-g-UV 531. The raw material composition and processing conditions of this comparative example are listed in Table 1, and the grafting rate and melt index of the compatibilizer are tested, and the test results are listed in Table 1.
[0080] Table 1 Raw material composition, processing conditions, grafting rate and melt index of each embodiment and comparative example
[0081]
[0082]
[0083] It can be seen from Examples 1, 3 and Comparative Example 1 that when the initiator dosage is in the range of 0.6-1 part, as the initiator dosage increases, the grafting rate shows a trend of first increasing and then decreasing. This is attributed to the fact that the increase of the initiator within a certain range can induce the polymer macromolecule to produce more free radicals, increase the grafting sites on the macromolecular chain, increase the chance of contact with the monomer, and thus increase the grafting rate. However, when the initiator dosage increases beyond a certain limit, the excessive concentration of free radicals generated will lead to an intensification of the coupling reaction, which is not conducive to the grafting reaction, and is easy to aggravate side reactions such as cross-linking, resulting in a weakening of the system fluidity and a significant reduction in the melt index.
[0084] It can be seen from Examples 1 and 4 and 5 that as the amount of grafted monomer increases, the grafting rate increases. This is attributed to the increase in the content of the grafted monomer, which increases the number of effective collisions between the grafted monomer and the free radicals of the matrix resin, and increases the probability of collision with the POE free radical per unit time, thereby increasing the grafting rate.
[0085] It can be seen from Example 1, Example 6 and Comparative Example 2 that as the processing temperature increases, the grafting rate of the system first increases and then decreases. The processing temperature can affect the efficiency and activity of the grafting reaction by affecting the decomposition rate of the initiator. When the temperature is low, TEMPO in TEMPO-DTBP tends to covalently bind to the growing free radicals to form dormant species. At this time, the decomposition rate of DTBP is also slow, which makes the grafting reaction rate of the system low; as the temperature increases, the TEMPO dormant species can be reversely split into growing free radicals, while accelerating the decomposition of DTBP, so that the composite initiator system can induce the production of more macromolecular free radicals, which is conducive to the grafting reaction. When the temperature rises to 230°C, the grafting rate no longer increases, mainly because the free radical concentration generated by NA at this time is too high to easily induce side reactions, inhibiting the grafting reaction, and the cross-linking side reaction causes the fluidity of the system to weaken and the melt index to be greatly reduced.
[0086] It can be seen from Example 1, Example 7 and Comparative Example 3 that when the screw speed is in the range of 260-350rpm, the grafting rate decreases with the increase of the screw speed. Since the shear force increases to a certain extent with the increase of the screw speed, some initiators will be squeezed out before they have time to decompose and take effect, which is equivalent to a reduction in the effective content of the initiator participating in the reaction, resulting in a decrease in the grafting rate.
[0087] It can be seen from Example 1 and Comparative Examples 3-4 that when all the grafting monomers are replaced with nadic anhydride, the grafting rate is improved to a certain extent, but the melt index decreases significantly; when all the grafting monomers are replaced with NA-g-UV 531, the melt index decreases slightly, but the grafting rate decreases significantly.
[0088] The compatibilizers prepared in Example 1, Example 2, Example 6, Example 7, and Comparative Examples 1-5 were applied to a nylon 66 and glass fiber composite material system, as follows:
[0089] Embodiment 8:
[0090] Weigh 6665 parts of nylon and 30 parts of glass fiber, 4.6 parts of the anti-ultraviolet compatibilizer obtained in Example 1, and 10980.4 parts of antioxidant and put them into a high-speed mixer for mixing. After mixing, put them into a twin-screw extruder, set the extrusion temperature to 270°C, the screw speed to 260rpm, and the feed speed to 10rpm. After the extrudate is cooled in a cooling water tank, it is pelletized to obtain reinforced and toughened anti-ultraviolet nylon pellets, and injection molding is used to obtain test specimens. The test results of various properties are listed in Table 2.
[0091] Embodiment 9:
[0092] The preparation method of the anti-ultraviolet modified nylon in this embodiment is substantially the same as that in embodiment 8, except that the compatibilizer in this embodiment is selected from that obtained in embodiment 2. The test results of various properties are listed in Table 2.
[0093] Embodiment 10:
[0094] The preparation method of the anti-ultraviolet modified nylon in this embodiment is substantially the same as that in embodiment 8, except that the compatibilizer in this embodiment is selected from that obtained in embodiment 6. The test results of various properties are listed in Table 2.
[0095] Embodiment 11:
[0096] The preparation method of the anti-ultraviolet modified nylon in this embodiment is substantially the same as that in embodiment 8, except that the compatibilizer in this embodiment is selected from that obtained in embodiment 7. The test results of various properties are listed in Table 2.
[0097] Embodiment 12:
[0098] The preparation method of the anti-ultraviolet modified nylon in this embodiment is basically the same as that in embodiment 8, except that the amount of anti-ultraviolet compatibilizer added in this embodiment is 6 parts. The test results of various properties are listed in Table 2.
[0099] Comparative Example 6:
[0100] The preparation method of the anti-ultraviolet modified nylon in this comparative example is basically the same as that in Example 8, except that the compatibilizer in this comparative example is selected from the one obtained in Comparative Example 1. The test results of various properties are listed in Table 2.
[0101] Comparative Example 7:
[0102] The preparation method of the anti-ultraviolet modified nylon in this comparative example is basically the same as that in Example 8, except that the compatibilizer in this comparative example is selected from the one obtained in Comparative Example 2. The test results of various properties are listed in Table 2.
[0103] Comparative Example 8:
[0104] The preparation method of the anti-ultraviolet modified nylon in this comparative example is basically the same as that in Example 8, except that the compatibilizer in this comparative example is selected from the one obtained in Comparative Example 3. The test results of various properties are listed in Table 2.
[0105] Comparative Example 9:
[0106] The preparation method of the modified nylon in this comparative example is basically the same as that in Example 8, except that the compatibilizer in this comparative example is selected from the one obtained in Comparative Example 4. The test results of various properties are listed in Table 2.
[0107] Comparative Example 10:
[0108] The preparation method of the modified nylon in this comparative example is basically the same as that in Example 8, except that the compatibilizer in this comparative example is selected from the one obtained in Comparative Example 5. The test results of various properties are listed in Table 2.
[0109] Comparative Example 11:
[0110] The preparation method of the modified nylon in this comparative example is basically the same as that in Example 8, except that the anti-ultraviolet compatibilizer in this comparative example is replaced by 4.6 parts of NA-g-UV 531 anti-ultraviolet agent. The test results of various properties are listed in Table 2.
[0111] Comparative Example 12:
[0112] The preparation method of the modified nylon in this comparative example is basically the same as that in Example 8, except that no anti-ultraviolet compatibilizer is added in this comparative example. The test results of various properties are listed in Table 2.
[0113] Comparative Example 13:
[0114] The preparation method of the modified nylon in this comparative example is basically the same as that in Example 8, except that the anti-ultraviolet compatibilizer is replaced by UV 531 anti-ultraviolet agent in this comparative example. The test results of various properties are listed in Table 2.
[0115] Table 2 Test results of various properties of modified nylon resins in various embodiments and comparative examples
[0116]
[0117]
[0118] From the data of Examples 8-12 and Comparative Examples 6-8 in Table 2, it can be seen that the anti-ultraviolet compatibilizer (POE-g-[NA&NA-g-UV]) prepared by appropriate processing temperature, screw speed, initiator and monomer addition amount can play a good toughening and anti-ultraviolet effect in the glass fiber reinforced PA66 system, which is attributed to: first, POE itself has good toughness, which is the basis of toughening; secondly, the anhydride group carried by the grafted NA can react with a large number of hydroxyl groups on the surface of the glass fiber and the terminal amine group of PA66; in addition, the ultraviolet absorber carried by the grafted NA-g-UV contains rich intramolecular hydrogen bonds (there are one or more of carbonyl groups, ester groups, hydroxyl groups, NN bonds, C=N bonds, etc.), which can form stable intermolecular hydrogen bonds with the PA66 molecular chain, thereby greatly improving the compatibility and dispersibility of the glass fiber, POE grafted anti-ultraviolet compatibilizer and the entire system, thereby obtaining a better toughening and anti-ultraviolet effect. On the contrary, the effect is not good. The POE grafted product with a low grafting rate reduces the content of its grafted anhydride groups and ultraviolet absorbers, affecting the compatibility and dispersibility of the compatibilizer with the glass fiber system. From the test data of Comparative Example 9, it can be seen that the POE system without ultraviolet absorber grafting, that is, the single POE-g-NA toughened PA66 / GF system, can obtain excellent toughening effect, but basically has no anti-ultraviolet effect. From the test data of Comparative Example 10, it can be seen that the strengthening, toughening and anti-ultraviolet effects of the anti-ultraviolet compatibilizer system without anhydride groups are not as good as those of the embodiment, mainly because the glass fiber cannot obtain the best compatibility effect with the system through the anhydride group, which reduces the dispersion effect of the system and reduces the performance. From the test data of Comparative Example 11, it can be seen that although the effective content of the ultraviolet absorber in Comparative Example 11 increases, the dispersion is not as good as that of the POE graft, resulting in its poor anti-ultraviolet effect, and the absence of the POE matrix loses the meaning of toughening.
[0119] In the above embodiments and comparative examples, the test methods and standards of various performance parameters are as follows:
[0120] (1) Grafting rate: The total grafting rate of NA and NA-g-UV in the grafted product was calculated by acid-base titration. Weigh 1.0 g of the purified grafted product and heat it under reflux in 50 ml of xylene solution for 30 min to fully dissolve the grafted product. Then titrate it with a 0.1 mol / L KOH-ethanol standard solution, using colorless phenolphthalein test solution as an indicator. Add it dropwise under continuous stirring. When the solution turns red, record the volume V1 of the KOH-ethanol standard solution used. Then use CH 3 Back titrate the COOH-ethanol standard solution. When the solution changes from red to colorless, stop titrating and record the CH 3 The volume of COOH standard solution V2. Measure three times according to the above experimental steps and take the average value, and calculate the grafting rate GR according to the following formula:
[0121]
[0122] In the formula, C is KOH and CH 3 COOH-ethanol standard solution concentration (mol / L); M is the average molecular weight of NA and NA-g-UV (g / mol); m is the mass of the grafted sample titrated (g).
[0123] (2) Melt index: According to GB / T 3682-2000, the mass of the sample flowing out of the die of the special equipment within ten minutes is measured by using a melt flow rate meter. The test conditions are as follows: temperature 230°C, weight 2.16 kg (230°C*2.16 kg). Each sample is tested five times and the average value is taken.
[0124] (3) Mechanical properties: The tensile strength and elongation at break were tested according to ISO 527-1 / -2, the flexural strength was tested according to ISO 178, and the notched impact strength of a simply supported beam was tested according to ISO 179 / 1eA.
[0125] (4) Color difference ΔE: Refer to GB / T 16422.3-2014 standard, use UVA-340 fluorescent ultraviolet lamp to carry out ultraviolet aging test, use colorimeter to test the color difference ΔE of samples before and after aging, test five samples in each group and take the average value.
[0126] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.
[0127] It should be understood that the technical solution of the present invention is not limited to the above-mentioned specific implementation cases. Any technical deformation made according to the technical solution of the present invention without departing from the scope of protection of the purpose of the present invention and the claims shall fall within the protection scope of the present invention.
Claims
1. A method for preparing an anti-ultraviolet compatibilizer, characterized in that: include: The mixed reaction system including at least nadic anhydride, a hydroxyl-containing ultraviolet absorber, and a catalyst is subjected to an esterification reaction to obtain a nadic anhydride-grafted ultraviolet absorber; Furthermore, the polyolefin elastomer, the grafted ultraviolet absorber of nadic anhydride, the nadic anhydride and the initiator are mixed and input into a twin-screw extruder for granulation to obtain an anti-ultraviolet compatibilizer.
2. The preparation method according to claim 1, characterized in that: Specifically include: The mixed reaction system including nadic anhydride, a hydroxyl-containing ultraviolet absorber, a catalyst and a solvent is subjected to an esterification reaction at 60-65° C. for 3N4h, and then filtered, washed and dried to obtain a nadic anhydride grafted ultraviolet absorber.
3. The preparation method according to claim 2, characterized in that: The hydroxyl-containing ultraviolet absorber includes any one or more combinations of triazine ultraviolet absorbers, salicylate ultraviolet absorbers, benzotriazole ultraviolet absorbers, and benzophenone ultraviolet absorbers; preferably, the hydroxyl-containing ultraviolet absorber includes any one or more combinations of triazine ultraviolet absorbers, salicylate ultraviolet absorbers, and benzotriazole ultraviolet absorbers; preferably, the benzophenone ultraviolet absorber includes any one or more combinations of UV-531, UV-1009, UV-981, and UV-2126. combination; preferably, the triazine ultraviolet absorber includes any one or more combinations of UV-1577, UV-1164, UV-400, and triazine-5; preferably, the salicylate ultraviolet absorber includes any one or more combinations of ethylhexyl salicylate, octyl salicylate, phenyl salicylate, isohexadecanyl salicylate, hexyl salicylate, and benzyl salicylate; preferably, the benzotriazole ultraviolet absorber includes any one or more combinations of UV-P, UV-326, UV-327, and UV-329; and / or, the catalyst comprises triethylamine; and / or, the solvent comprises dichloromethane; And / or, the molar ratio of the nadic anhydride to the hydroxyl-containing ultraviolet absorber is 1:1.5-2.
5.
4. The preparation method according to claim 1, characterized in that: The mass ratio of the polyolefin elastomer, the nadic anhydride grafted ultraviolet absorber, the nadic anhydride and the initiator is 100:3-6:3-6:0.6-1; And / or, the initiator comprises a 2,2,6,6-tetramethyl-1-oxypiperidine-di-tert-butyl peroxide composite system; And / or, the process parameters adopted by the twin-screw extruder include: processing temperature of 200-225°C, screw speed of 260-300rpm, and feeding speed of 10-15rpm.
5. An anti-ultraviolet compatilizer obtained by the preparation method described in any one of claims 1 to 4.
6. Use of the anti-ultraviolet compatibilizer according to claim 5 in the preparation of modified nylon.
7. A modified nylon, characterized in that: The raw materials for preparing the modified nylon include the following components calculated by mass: 55-65 parts of nylon, 25-40 parts of glass fiber, 6 parts of anti-ultraviolet compatibilizer 3N and 0.2-0.5 parts of antioxidant; Wherein, the anti-UV compatibilizer includes the anti-UV compatibilizer described in claim 5.
8. The modified nylon according to claim 7, characterized in that: The nylon includes nylon 66 and / or nylon 6; And / or, the antioxidant includes antioxidant 1098.
9. The method for preparing modified nylon according to claim 6 or 7, characterized in that: include: Nylon, glass fiber, anti-ultraviolet compatibilizer and antioxidant are placed in a high-speed mixing device and mixed evenly, and then the obtained materials are input into a twin-screw extruder for granulation to obtain modified nylon.
10. The preparation method according to claim 9, characterized in that: The process parameters adopted by the twin-screw extruder include: temperature of 240-280° C., screw speed of 260-300 rpm, and feed speed of 10-15 rpm.
Citation Information
Patent Citations
Bonding resin of polyethylene composite pipeline and preparation method thereof
CN107189729A
Rigid polyester polyol and preparation method thereof
CN115894880A
Compatibilizer and synthesis method thereof, compatibilization method of polyamide and polyolefin blend system, and polyamide and polyolefin blend
CN118085146A
Method for modifying cyclic olefin copolymer using reactive extrusion method
JP2007182467A
Glass-reinforced polymer composition comprising 4-methyl-1-pentene polymer in combination with a graft modified acid polymer of 4-methyl-1-pentene polymer
US4501827A