Preparation method of phenolic resin

By using the combination of two-stage heating method and functional additives in the preparation of phenolic resin, the problem of high free phenolic content in the constant temperature reaction is solved, and the preparation of low content in phenolic resin is achieved, environmental pollution is reduced and product quality is improved.

CN119081032APending Publication Date: 2024-12-06SHANGHAI CHUNBAO CHEM CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411269820.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

During the preparation of phenolic resin, the constant temperature heating reaction cannot fully exert the role of raw materials, resulting in high content of free phenol and free aldehyde in the product, causing environmental pollution.

Method used

Using a two-stage heating method, phenol, formaldehyde and catalyst were mixed with water, pressurized by 0.025-0.03MPa, first heated to 40-45℃ and then to 87-89℃, heated to stop heating and reacted under normal pressure, then cooled down and vacuumed Dehydration, combining functional additives of urea and polyether modified silicone oil to regulate the reaction process and reduce the content of free phenol and free aldehydes.

Benefits of technology

It effectively reduces the free phenol and free aldehyde content in phenolic resin, improves the application quality of the product, reduces environmental pollution, and is simple and efficient in operation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention relates to the technical field of phenolic resin, and particularly discloses a phenolic resin preparation method which comprises the following steps: (1) preparing raw materials containing phenol, formaldehyde, a catalyst and water; (2) mixing the phenol, the formaldehyde, the catalyst and the water in the step (1), pressurizing to 0.025-0.03 MPa, stirring at the speed of 70-80 r / min, and continuously stirring; then the temperature is raised to 40-45 DEG C within 7-8 min, then the temperature is raised to 87-89 DEG C within 30-35 min, and heating is stopped; the heat release temperature of the subsequent self-reaction is 100-105 DEG C, the reaction time is 25-30 minutes, and the normal pressure is kept in the process to obtain a product; and (3) cooling the product obtained in the step (2) to 50-60 DEG C, and carrying out vacuum dehydration to obtain the phenolic resin. The whole operation is simple and efficient, and the effects of all the raw materials can be fully exerted, so that the content of free phenol and free aldehyde in the phenolic resin is obviously low.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of phenolic resins, and more specifically, to a method for preparing phenolic resins. Background Art

[0002] Phenolic resin is a synthetic polymer obtained by the reaction of phenol or substituted phenol with formaldehyde. It is a closed-cell rigid foam plastic prepared by adding additives such as foaming agent and curing agent, expanding, cross-linking and curing at a certain temperature. Due to its low price, light weight and the recognition of its fire retardant properties by the industrial sector, it has been gradually used in construction, aerospace, transportation, military defense and other fields.

[0003] Currently, the preparation of phenolic resin is mainly divided into two main steps. First, under appropriate conditions, phenol and formaldehyde are reacted to form hydroxymethylphenol, and then condensation and polycondensation reactions are caused between hydroxymethylphenol and between hydroxymethylphenol and phenol molecules to form phenolic resin with a certain molecular weight. For example, the invention patent application document with patent publication number CN114644742A discloses a process for preparing a highly uniform phenolic resin, which comprises the following steps: (1) preparation of raw materials: preparing 300 g of phenol, 400 ml of formaldehyde solution, 100 ml of concentrated hydrochloric acid, 100 ml of sodium hydroxide solution, 500 ml of ethanol and 100 ml of molybdic acid solution; (2) preparation of the reaction solution; (3) adding a catalyst; (4) preparation of the phenolic resin: using a reactor to heat the mixed solution of step (3) at a constant temperature and stirring it regularly until the reaction is complete and a white or yellow precipitate is generated; (5) cleaning of the phenolic resin; (6) post-treatment of the phenolic resin; (7) preparation of the finished product; and (8) secondary cleaning.

[0004] With respect to the above-mentioned related technologies, the inventors believe that in the preparation of phenolic resin, by first mixing the raw materials and then adopting constant temperature heating for cross-stirring reaction during the process, although the phenolic resin can be quickly obtained and the operation is relatively simple and efficient, the constant temperature reaction process cannot fully exert the effects of the raw materials, and often a high content of free phenol and free aldehyde will exist in the phenolic resin product, and the free phenol and free aldehyde are easily volatilized during use, which will cause serious pollution to the water and atmosphere in the environment.

[0005] Therefore, it is urgent to propose a solution to solve the above technical problems. Summary of the invention

[0006] In order to enable each raw material to fully exert its own role in the preparation of phenolic resin, and thus obtain a phenolic resin product with low free phenol and free formaldehyde content, the present application provides a method for preparing phenolic resin.

[0007] The present application provides a method for preparing a phenolic resin, which adopts the following technical scheme: A method for preparing a phenolic resin comprises the following steps: (1) preparing a raw material comprising phenol, formaldehyde, a catalyst and water; (2) After mixing the phenol, formaldehyde, catalyst and water in step (1), pressurizing to 0.025-0.03 MPa, stirring at a speed of 70-80 r / min, and continuously stirring; then heating to 40-45° C. within 7-8 min, then heating to 87-89° C. within 30-35 min, and stopping heating; the subsequent self-reaction exothermic temperature is 100-105° C., the reaction time is 25-30 min, and normal pressure is maintained during the process to obtain a product; (3) The product obtained in step (2) is cooled to 50-60° C. and subjected to vacuum dehydration to obtain a phenolic resin.

[0008] By adopting the above technical scheme, after the raw materials of phenol, formaldehyde, catalyst and water are mixed, the mixture is pressurized to 0.025-0.03MPa, and the temperature is increased to 40-45°C within 7-8min and to 87-89°C within 30-35min in two stages, so that phenol and formaldehyde are more conducive to addition reaction and generate hydroxymethylphenol; when the temperature is increased to 87-89°C, condensation reaction begins to occur between hydroxymethylphenols and between hydroxymethylphenol and phenol molecules to generate diphenol core and polyphenol core oligomers, and a large amount of reaction heat is released at this time. Subsequently, when the heating is stopped, the pressure is adjusted to normal pressure, and as the temperature continues to rise and is controlled at 100-105°C, the reaction can be fully reacted and a highly cross-linked body structure can be generated; finally, the phenolic resin is obtained after cooling and vacuum dehydration. During the whole process, all raw materials are mixed at one time, so that the function of each raw material can be fully exerted, the content of free phenol and free formaldehyde in the phenolic resin is significantly lower, the operation is simple and efficient, and the overall performance is outstanding.

[0009] Preferably, step (2) is specifically configured as follows: after mixing the phenol, formaldehyde, catalyst and water in step (1), pressurizing to 0.025 MPa, stirring at a speed of 75 r / min, and continuously stirring; then heating to 42° C. within 8 min, then heating to 88° C. within 35 min, and stopping heating; the subsequent self-reaction exothermic temperature is 103° C., the reaction time is 28 min, and normal pressure is maintained during the process to obtain the product.

[0010] By adopting the above technical solution, in the operation of step (2), the selection and coordination of the above parameters can make the role of each raw material fully exerted more thoroughly, and the free phenol and free formaldehyde contents of the prepared phenolic resin are also lower, and the overall application quality is better.

[0011] Preferably, in step (1), the composition weight parts of phenol, formaldehyde, catalyst and water are as follows: Phenol 0.9-1.1 parts; Formaldehyde 1.2-2.0 parts; Catalyst 0.01-0.03 parts; 1-1.3 parts water.

[0012] By adopting the above technical scheme, the above-mentioned raw materials in parts by weight can not only fully play their own roles in the preparation when mixed and used, but also form a mixed system that is more compatible with the operation control system. Under the control of various operating parameters, the raw materials can be fully reacted and utilized, thereby ensuring that the obtained phenolic resin has a lower content of free phenol and free aldehyde, and is not easy to cause significant pollution to the water and atmosphere in the environment during subsequent applications, and the overall application quality is better.

[0013] Preferably, in step (1), the composition weight parts of phenol, formaldehyde, catalyst and water are as follows: 1 part of phenol; 1.5 parts of formaldehyde; 0.02 parts of catalyst; 1.2 parts water.

[0014] By adopting the above technical solution, the above-mentioned raw materials in parts by weight are mixed and applied, the raw material mixing system and the preparation operation control system have better compatibility, and the free phenol and free formaldehyde contents of the prepared phenolic resin are also low.

[0015] Preferably, the raw materials in step (1) further include 0.2-0.4 parts by weight of a functional additive, the functional additive is composed of urea and polyether-modified silicone oil, and the weight ratio of urea to polyether-modified silicone oil is 1:(0.3-0.4); The polyether-modified silicone oil is prepared by the following steps: S1. Mixing a hydrogen-containing silicone oil having a hydrogen group mass fraction of 1-2% and a polyether having a relative molecular mass of 1500-3000 in a weight ratio of (13-16):1 to obtain a reaction mixture; S2. Add 0.1-0.3% of the weight of the catalyst to the reaction mixture, and react at 90-110° C. for 8-12 hours to obtain polyether-modified silicone oil.

[0016] By adopting the above technical scheme, urea can react with free formaldehyde in the preparation of phenolic resin, and increase the degree of condensation, increase the consumption of phenol, and finally reduce the content of free phenol and free aldehyde; in the preparation of phenolic resin, polyether-modified silicone oil can reduce free phenol and free aldehyde by chemical copolymerization, and polyether-modified silicone oil is prepared from hydrogen-containing silicone oil and polyether of the above specifications, wherein Si-OC hydrolyzable copolymer linked by Si-OC bond is more prone to hydrolysis and has a better copolymerization effect; at the same time, when urea and polyether-modified silicone oil are used as functional additives, the two can bring about excellent compounding and synergistic effects to each other, and through the dual effects of regulating the reaction process and accelerating the consumption of phenol and formaldehyde, the content of free phenol and free aldehyde in the phenolic resin finally obtained is further reduced, thereby significantly reducing the pollution of the phenolic resin after application, and improving the overall application quality of the phenolic resin.

[0017] Preferably, the weight ratio of the urea to the polyether-modified silicone oil is 1:0.35.

[0018] By adopting the above technical scheme, when the urea and polyether-modified silicone oil in the above weight ratio are used in combination, the coordination system formed by them can exert a better application effect, and the free phenol and free formaldehyde content in the phenolic resin finally obtained is also relatively low.

[0019] Preferably, the polyether-modified silicone oil is prepared by the following steps: S1, mixing hydrogen-containing silicone oil with a hydrogen group mass fraction of 1.5% and polyether with a relative molecular mass of 2500 in a weight ratio of 14.5:1 to obtain a reaction mixture; S2. Add 0.2% of the weight of the catalyst to the reaction mixture and react at 105° C. for 11 hours to obtain polyether-modified silicone oil.

[0020] By adopting the above technical scheme, when the polyether-modified silicone oil prepared as above is used, it can not only fully play its own role in the preparation of phenolic resin and in the reaction system formed by various raw materials, but also form a more excellent compounding effect with urea, so that the functional additives in the preparation of phenolic resin are more adaptable, and further, the low content of free phenol and free aldehyde in the phenolic resin is also significantly better, so as to obtain a phenolic resin with better application quality.

[0021] Preferably, in step (1), the catalyst is composed of sodium hydroxide, calcium oxide and zinc oxide, and the weight ratio of sodium hydroxide, calcium oxide and zinc oxide is 1:(1.3-1.5):(1.6-2.0).

[0022] By adopting the above technical scheme, the role of sodium hydroxide in the synthesis of phenolic resin is to accelerate the polymerization process of the resin through its alkaline catalytic effect, and at the same time adjust the acidity and alkalinity of the reaction medium, thereby affecting the structure and characteristics of the final resin; calcium oxide plays a catalytic role in the synthesis of phenolic resin, promotes the formation of ortho-addition products in the synthesis reaction, and is beneficial to the rapid curing of phenolic resin; zinc oxide can optimize the synthesis process of phenolic resin and promote the addition reaction of phenol and formaldehyde; and when sodium hydroxide, calcium oxide and zinc oxide are used as a catalyst, the catalytic system formed can show strong adaptability with the operation control system in the preparation process, thereby ensuring that the final phenolic resin has a lower free phenol and free aldehyde content.

[0023] Preferably, the weight ratio of the sodium hydroxide, calcium oxide and zinc oxide is 1:1.4:1.8.

[0024] By adopting the above technical scheme, the sodium hydroxide, calcium oxide and zinc oxide in the above weight ratio can cooperate with each other better when used, so that the catalyst can play a better corresponding effect in the preparation of phenolic resin, thereby reducing the content of free phenol and free aldehyde in the phenolic resin.

[0025] In summary, this application has the following beneficial effects: 1. The present application comprises mixing raw materials containing phenol, formaldehyde, a catalyst and water at one time, pressurizing the mixture to 0.025-0.03 MPa, heating the mixture to 40-45° C. within 7-8 min and to 87-89° C. within 30-35 min, stopping heating, reacting the mixture at normal pressure and 100-105° C. for 25-30 min, and finally cooling the mixture and performing vacuum dehydration to obtain a phenolic resin; the whole operation is not only simple and efficient, but also enables the functions of the raw materials to be fully exerted, thereby significantly reducing the content of free phenol and free aldehyde in the phenolic resin; 2. When urea and polyether-modified silicone oil are used as functional additives in the present application, the combination of the two can not only regulate the reaction process, but also accelerate the consumption of phenol and formaldehyde in the preparation process, so that the content of free phenol and free aldehyde in the final phenolic resin is further reduced; 3. The present application adopts a catalyst composed of sodium hydroxide, calcium oxide and zinc oxide. The catalytic system formed by the three can show strong adaptability with the operation control system in the preparation process, thereby reducing the content of free phenol and free aldehyde in the phenolic resin. DETAILED DESCRIPTION

[0026] The present application is further described in detail below in combination with preparation examples, embodiments and comparative examples.

[0027] Preparation examples of raw materials and / or intermediates Preparation Example 1 A polyether modified silicone oil is prepared by the following steps: S1. Mix hydrogen-containing silicone oil with a hydrogen group mass fraction of 1.5% and polyether with a relative molecular mass of 2250 in a weight ratio of 14.5:1 to obtain a reaction mixture; S2. Add 0.2% of the weight of the catalyst to the reaction mixture and react at 100° C. for 10 h to obtain polyether-modified silicone oil.

[0028] Note: The catalyst used above is triethanolamine.

[0029] Preparation Example 2 A polyether-modified silicone oil, which is different from Preparation Example 1 in that it is prepared by the following steps: S1. Mixing hydrogen-containing silicone oil having a hydrogen group mass fraction of 1% and polyether having a relative molecular mass of 1500 in a weight ratio of 13:1 to obtain a reaction mixture; S2. Add 0.1% of the weight of the catalyst to the reaction mixture and react at 90° C. for 12 h to obtain polyether-modified silicone oil.

[0030] Preparation Example 3 A polyether-modified silicone oil, which is different from Preparation Example 1 in that it is prepared by the following steps: S1. Mixing hydrogen-containing silicone oil having a hydrogen group mass fraction of 2% and polyether having a relative molecular mass of 3000 in a weight ratio of 16:1 to obtain a reaction mixture; S2. Add 0.3% of the weight of the catalyst to the reaction mixture and react at 110° C. for 8 h to obtain polyether-modified silicone oil.

[0031] Preparation Example 4 A polyether-modified silicone oil, which is different from Preparation Example 1 in that it is prepared by the following steps: S1, mixing hydrogen-containing silicone oil with a hydrogen group mass fraction of 1.5% and polyether with a relative molecular mass of 2500 in a weight ratio of 14.5:1 to obtain a reaction mixture; S2. Add 0.2% of the weight of the catalyst to the reaction mixture and react at 105° C. for 11 hours to obtain polyether-modified silicone oil. Example

[0032] Example 1 A method for preparing a phenolic resin, wherein the weights of phenol, formaldehyde, catalyst and water used are shown in Table 1, and the method comprises the following steps: (1) preparing a raw material comprising phenol, formaldehyde, a catalyst and water; (2) After mixing the phenol, formaldehyde, catalyst and water in step (1), pressurizing to 0.025 MPa, stirring at a speed of 75 r / min, and continuously stirring; then heating to 42° C. within 8 min, and then heating to 88° C. within 35 min, and stopping heating; the subsequent self-reaction exothermic temperature is 103° C., the reaction time is 28 min, and normal pressure is maintained during the process to obtain a product; (3) The product obtained in step (2) is cooled to 50-60° C. and subjected to vacuum dehydration to obtain a phenolic resin.

[0033] Note: In the above operation, the catalyst is composed of sodium hydroxide, calcium oxide and zinc oxide in a weight ratio of 1:1.4:1.8; in step (3), the temperature is lowered to 55°C.

[0034] Embodiment 2-4 A method for preparing a phenolic resin, which is different from Example 1 in that the weights of the phenol, formaldehyde, catalyst and water used are shown in Table 1. Table 1 Weights of the phenol, formaldehyde, catalyst and water used in Examples 1-4 (kg / portion) raw material Example 1 Example 2 Example 3 Example 4 phenol 1 1 0.9 1.1 formaldehyde 1.5 1.6 1.2 2.0 catalyst 0.02 0.02 0.01 0.03 water 1.2 1.15 1 1.3 Example 5 A method for preparing a phenolic resin, which is different from Example 1 in that the catalyst is composed of sodium hydroxide, calcium oxide and zinc oxide in a weight ratio of 1:1.3:1.6.

[0035] Example 6 A method for preparing a phenolic resin, which is different from Example 1 in that the catalyst is composed of sodium hydroxide, calcium oxide and zinc oxide in a weight ratio of 1:1.5:2.0.

[0036] Example 7 A method for preparing a phenolic resin, which is different from Example 1 in that no sodium hydroxide is used in the catalyst.

[0037] Example 8 A method for preparing a phenolic resin, which is different from Example 1 in that calcium oxide is not used in the catalyst.

[0038] Example 9 A method for preparing a phenolic resin, which is different from Example 1 in that zinc oxide is not used in the catalyst.

[0039] Example 10 A method for preparing a phenolic resin, which is different from Example 1 in that sodium hydroxide and zinc oxide are not used in the catalyst.

[0040] Embodiment 11 A method for preparing a phenolic resin, which is different from Example 1 in that sodium hydroxide and calcium oxide are not used in the catalyst.

[0041] Example 12 A method for preparing a phenolic resin, which is different from Example 1 in that calcium oxide and zinc oxide are not used in the catalyst.

[0042] Embodiment 13 A method for preparing a phenolic resin, which is different from that in Example 1 in that step (2) is specifically configured as follows: after mixing the phenol, formaldehyde, catalyst and water in step (1), pressurizing to 0.0275 MPa, stirring at a speed of 75 r / min, and continuously stirring; then heating to 42.5° C. within 7.5 min, then heating to 88° C. within 32.5 min, and stopping heating; the subsequent self-reaction exothermic temperature is 102.5° C., the reaction time is 27.5 min, and normal pressure is maintained during the process to obtain a product.

[0043] Embodiment 14 A method for preparing a phenolic resin, which is different from that in Example 1 in that step (2) is specifically configured as follows: after mixing the phenol, formaldehyde, catalyst and water in step (1), pressurizing to 0.025 MPa, stirring at a speed of 70 r / min, and continuously stirring; then heating to 40° C. within 7 min, then heating to 87° C. within 30 min, and stopping heating; the subsequent self-reaction exothermic temperature is 100° C., the reaction time is 25 min, and normal pressure is maintained during the process to obtain a product.

[0044] Embodiment 15 A method for preparing a phenolic resin, which is different from that in Example 1 in that step (2) is specifically configured as follows: after mixing the phenol, formaldehyde, catalyst and water in step (1), pressurizing to 0.03 MPa, stirring at a speed of 80 r / min, and continuously stirring; then heating to 45° C. within 8 min, then heating to 89° C. within 35 min, and stopping heating; the subsequent self-reaction exothermic temperature is 105° C., the reaction time is 30 min, and normal pressure is maintained during the process to obtain a product.

[0045] Example 16 A method for preparing a phenolic resin, which is different from that in Example 1 in that the raw materials in step (1) further include 0.3 parts by weight of a functional additive, the functional additive is composed of urea and polyether-modified silicone oil in a weight ratio of 1:0.35, and the polyether-modified silicone oil is obtained from Preparation Example 1, and the polyether-modified silicone oil is mixed with the raw materials when used.

[0046] Embodiment 17 A method for preparing a phenolic resin, which is different from Example 16 in that the weight portion of the functional additive used is 0.2 parts.

[0047] Embodiment 18 A method for preparing a phenolic resin, which is different from Example 16 in that the weight portion of the functional additive used is 0.4 parts.

[0048] Embodiment 19 A method for preparing a phenolic resin, which is different from Example 16 in that the functional additive consists of urea and polyether-modified silicone oil in a weight ratio of 1:0.3.

[0049] Embodiment 20 A method for preparing a phenolic resin, which is different from Example 16 in that the functional additive consists of urea and polyether-modified silicone oil in a weight ratio of 1:0.4.

[0050] Embodiment 21 A method for preparing a phenolic resin, which is different from Example 16 in that the polyether-modified silicone oil is obtained from Preparation Example 2.

[0051] Embodiment 22 A method for preparing a phenolic resin, which is different from Example 16 in that the polyether-modified silicone oil is obtained from Preparation Example 3.

[0052] Embodiment 23 A method for preparing a phenolic resin, which is different from Example 16 in that urea is not used in the functional additive.

[0053] Embodiment 24 A method for preparing a phenolic resin, which is different from Example 16 in that no polyether-modified silicone oil is used in the functional additive.

[0054] Embodiment 25 A method for preparing a phenolic resin, which is different from Example 16 in that the polyether-modified silicone oil is obtained from Preparation Example 4.

[0055] Comparative Example Comparative Example 1 A method for preparing a phenolic resin, which is different from that in Example 1 in that step (2) is specifically configured as follows: after mixing the phenol, formaldehyde, catalyst and water in step (1), heating to 103° C., reacting for 40 min, stirring at a speed of 75 r / min, and continuously stirring to obtain a product.

[0056] Performance test samples: The phenolic resins obtained in Examples 1-25 were used as test samples 1-25, and the phenolic resin obtained in Comparative Example 1 was used as control sample 1.

[0057] Test method: According to the requirements of standard GB / T 30773-2014 "Determination of free phenol content in phenolic resin by gas chromatography", test samples 1-25 and control sample 1 were tested, and the free phenol content obtained by the test was recorded in Table 2; according to the requirements of standard GB / T 32684-2016 "Determination of free formaldehyde content in plastic phenolic resin", test samples 1-25 and control sample 1 were tested, and the free formaldehyde content obtained by the test was recorded in Table 2.

[0058] Table 2 Test results of test samples 1-25 and control sample 1 In combination with Example 1, Example 13-15 and Comparative Example 1 and Table 2, it can be seen that in the preparation of phenolic resin, the raw materials containing phenol, formaldehyde, catalyst and water are mixed once and then pressurized at 0.025-0.03MPa, and the temperature is raised to 40-45°C within 7-8min and to 87-89°C within 30-35min in two stages, and then the heating is stopped, and the reaction is carried out for 25-30min at normal pressure and a temperature of 100-105°C, and finally the phenolic resin is obtained after cooling and vacuum dehydration; and the obtained phenolic resin has significantly lower free phenol and free aldehyde content after testing. At the same time, if the raw materials are mixed, the reaction is carried out at a constant temperature by heating once and the free phenol and free aldehyde content in the obtained phenolic resin is found to be significantly higher. It can be seen that the application of the preparation method of phenolic resin can give full play to the role of each raw material in the application process, and then obtain a phenolic resin with a low content of free phenol and free aldehyde, which has an outstanding progressive effect.

[0059] It can be seen from Examples 1-4 and Table 2 that, when 0.9-1.1 parts by weight of phenol, 1.2-2.0 parts by weight of formaldehyde, 0.01-0.03 parts by weight of catalyst and 1-1.3 parts by weight of water are mixed, the obtained phenolic resin can be guaranteed to have a low content of free phenol and free aldehyde.

[0060] In combination with Example 1 and Example 5-12 and in combination with Table 2, it can be seen that when a catalyst composed of sodium hydroxide, calcium oxide and zinc oxide in a weight ratio of 1:(1.3-1.5):(1.6-2.0) is used, the free phenol and free aldehyde contents of the obtained phenolic resin are relatively low after testing; and when any one or two of sodium hydroxide, calcium oxide and zinc oxide are used as catalysts, it is found that the free phenol and free aldehyde contents in the phenolic resin are significantly relatively high; it can be seen that only when sodium hydroxide, calcium oxide and zinc oxide form a catalyst application, the three form a catalytic system that is more compatible with the operation control system in the phenolic resin preparation process, thereby ensuring that the phenolic resin finally obtained has a lower free phenol and free aldehyde content. Among them, when the weight ratio of sodium hydroxide, calcium oxide and zinc oxide is 1:1.4:1.8, the application effect brought by the catalyst is better.

[0061] In combination with Example 1 and Example 16-20 and in combination with Table 2, it can be seen that when the present application uses a functional additive composed of urea and polyether-modified silicone oil, the free phenol and free aldehyde content in the phenolic resin can be further reduced. In combination with Example 23-24 and in combination with Table 2, it can be seen that if any one of urea and polyether-modified silicone oil is used alone as a functional additive, the effect of reducing the free phenol and free aldehyde content in the phenolic resin is effective, and the sum of the effects of the two being used separately is also far less than the excellent effect brought by the compounding of the two. It can be seen that urea and polyether-modified silicone oil can play an excellent compounding synergistic effect with each other, and then have a significant effect on the further reduction of the free phenol and free aldehyde content in the phenolic resin. In combination with Example 21-22, Example 25 and in combination with Table 2, it can be seen that the polyether-modified silicone oil prepared by the present application can be compounded with urea and play an excellent effect.

[0062] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed. However, as long as it is within the scope of the claims of the present application, it shall be protected by the patent law.

Claims

1. A method for preparing a phenolic resin, It is characterized in that The following steps are involved: (1) preparing a raw material comprising phenol, formaldehyde, a catalyst and water; (2) After mixing the phenol, formaldehyde, catalyst and water in step (1), pressurizing to 0.025-0.03 MPa, stirring at a speed of 70-80 r / min, and continuously stirring; then heating to 40-45° C. within 7-8 minutes, and then heating to 87-89° C. within 30-35 minutes, and stopping heating; the subsequent self-reaction exothermic temperature is 100-105° C., the reaction time is 25-30 minutes, and normal pressure is maintained during the process to obtain the product; (3) The product obtained in step (2) is cooled to 50-60° C. and subjected to vacuum dehydration to obtain a phenolic resin.

2. The method for preparing a phenolic resin according to claim 1, Features: The specific setting of step (2) is as follows: after mixing the phenol, formaldehyde, catalyst and water in step (1), pressurizing to 0.025 MPa, stirring at a speed of 75 r / min, and stirring continuously; then heating to 42° C. within 8 minutes, and then heating to 88° C. within 35 minutes, and stopping heating; the subsequent self-reaction exothermic temperature is 103° C., the reaction time is 28 minutes, and normal pressure is maintained during the process to obtain the product.

3. The method for preparing a phenolic resin according to claim 1, Features: In step (1), the composition weight parts of phenol, formaldehyde, catalyst and water are as follows: Phenol 0.9-1.1 parts; Formaldehyde 1.2-2.0 parts; Catalyst 0.01-0.03 parts; 1-1.3 parts water.

4. The method for preparing a phenolic resin according to claim 3, Features: In step (1), the composition weight parts of phenol, formaldehyde, catalyst and water are as follows: 1 part of phenol; 1.5 parts of formaldehyde; 0.02 parts of catalyst; 1.2 parts water.

5. The method for preparing a phenolic resin according to claim 3, Features: The raw materials in step (1) further include 0.2-0.4 parts by weight of a functional additive, the functional additive is composed of urea and polyether-modified silicone oil, and the weight ratio of urea to polyether-modified silicone oil is 1:(0.3-0.4); The polyether-modified silicone oil is prepared by the following steps: S1, mixing a hydrogen-containing silicone oil having a hydrogen group mass fraction of 1-2% and a polyether having a relative molecular mass of 1500-3000 in a weight ratio of (13-16):1 to obtain a reaction mixture; S2. Add 0.1-0.3% of the weight of the catalyst to the reaction mixture, and react at 90-110° C. for 8-12 hours to obtain polyether-modified silicone oil.

6. The method for preparing a phenolic resin according to claim 5, Features: The weight ratio of the urea to the polyether-modified silicone oil is 1:0.

35.

7. The method for preparing a phenolic resin according to claim 5, Features: The polyether-modified silicone oil is prepared by the following steps: S1, mixing hydrogen-containing silicone oil having a hydrogen group mass fraction of 1.5% and polyether having a relative molecular mass of 2500 in a weight ratio of 14.5:1 to obtain a reaction mixture; S2. Add 0.2% catalyst by weight of the reaction mixture and react at 105°C for 11 hours to obtain polyether-modified silicone oil.

8. The method for preparing a phenolic resin according to claim 1, Features: In step (1), the catalyst is composed of sodium hydroxide, calcium oxide and zinc oxide, and the weight ratio of sodium hydroxide, calcium oxide and zinc oxide is 1: (1.3-1.5): (1.6-2.0).

9. The method for preparing a phenolic resin according to claim 8, Features: The weight ratio of the sodium hydroxide, calcium oxide and zinc oxide is 1:1.4:1.8.

Citation Information

Cited By

  • Preparation method of phenolic resin for new energy automobile battery and application of phenolic resin in epoxy resin curing

    CN120005130A

  • Preparation Method of Phenolic Resin for New Energy Vehicle Batteries and Its Application in Curing of Epoxy Resins

    CN120005130B