Preparation method of flatulence slow-rebound sponge material
By combining the polyether polyol with a specific ratio with polymer polyol and inert gas, the problems of the bearing capacity and the reduction of aldehyde substances of slow rebound sponge materials are solved, and higher support performance and safety are achieved.
Patent Information
- Application Number
- CN202411381072.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-12-06
AI Technical Summary
The existing slow rebound sponge materials have poor bearing capacity, are fragile, and have low folding times. The aldehydes produced during foaming are difficult to effectively reduce, affecting consumer health and product safety.
A mixture of polyether polyols and polymer polyols of a specific ratio is used to combine inert gas and modified isocyanates to prepare a gas slow rebound sponge material through continuous production line foaming technology to neutralize aldehyde substances and improve the cell structure.
It significantly improves the support performance and cell structure of the sponge, reduces the content of aldehyde substances, meets the national formaldehyde and acetaldehyde emission standards, and provides safer and healthier products.
Smart Images

Figure BDA0005069919480000031 
Figure BDA0005069919480000041 
Figure BDA0005069919480000051
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing an inflation slow-rebound sponge material. Background Art
[0002] Sponge refers to foamed materials in general. Foamed products of resin, rubber and plastic are all called sponges. Polyurethane sponge is a foamed polyurethane material that has both the elasticity of rubber and the strength and excellent processing properties of plastic. It can be used to prepare polyurethane slow-rebound materials. Because of its porous honeycomb structure, it has excellent softness, elasticity, water absorption and water resistance, and is widely used in sofas, mattresses, soft packaging and other industries.
[0003] As one of the sponges, the slow-rebound sponge is mainly composed of polyurethane foam plastic, which has viscoelasticity and can be shaped by body temperature and pressure, effectively dissolving the pressure of the human body into zero pressure, offsetting the reaction force, and providing the most uniform support for the body, thereby having a tight wrapping feeling; however, most of the existing slow-rebound sponges have poor bearing capacity and are relatively fragile, with too few folding times. At the same time, they also have defects such as low tension, hardness and strength.
[0004] At present, during the foaming process of sponges, polyether polyols and various small materials will react and foam to produce aldehydes. The main formaldehyde produced is a colorless, soluble, irritating gas. Long-term inhalation of formaldehyde gas can damage the liver, kidneys, blood system, digestive system, respiratory system, central nervous system and immune system. The general mattress formaldehyde standard is mainly based on GB / T 33243-2016 "Limits of Formaldehyde Emission from Furniture", which stipulates that the formaldehyde emission in mattresses should be controlled at 0.5mg / m 3 Below, acetaldehyde release should be controlled at 1mg / m 3 In order to protect the health of consumers, the formaldehyde content of mattresses should meet the national standard limit to ensure the safety of the product. At present, the technology controls the formaldehyde and acetaldehyde content to 0.2-0.5mg / m 3 How to reduce aldehyde substances again is also a challenge for the polyurethane industry.
[0005] Chinese patent application CN 102643404A discloses a slow-rebound polyether polyurethane sponge, comprising 20-85 parts by weight of a first polyol, 10-90 parts by weight of a second polyol, and 8-30 parts by weight of MDI isocyanate, as well as a foaming agent, a catalyst, a surfactant, a flame retardant, and 0.2-0.8 parts by weight of a silicone rubber toughening agent; the first polyol is a polymer of ethylene glycol and propylene glycol, with a functionality of 3 and a hydroxyl value of 45-99 mgKOH / g; the second polyol is a copolymer of trimethylolpropane and butylene oxide, with an EO content of more than 60% and a hydroxyl value of 3-22 mgKOH / g. It has good performance in slow resilience and strength, but poor support performance. Summary of the invention
[0006] The technical problem to be solved by the present invention is to reduce aldehyde substances and improve the pore structure of polyurethane sponge in the prior art, and to enhance the sponge support performance. A new method for preparing an inflatable slow-rebound sponge material is provided, and the inflatable slow-rebound sponge material has the advantages of reducing aldehyde substances and improving the pore structure of polyurethane sponge, and enhancing the sponge support performance.
[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows: a method for preparing an inflation slow-rebound sponge material, comprising the following steps:
[0008] (1) Preparation of components: by weight, component A: 30-50 parts of polyether polyol I, 20-40 parts of polyether polyol II, 30-50 parts of polymer polyol, 5-8 parts of cell opener, 1.2-1.8 parts of foam stabilizer, 0.5-1 parts of catalyst, 1-1.5 parts of foaming agent, 1-2 parts of crosslinking agent; component B: 30-50 parts of isocyanate; the weight ratio of polyol in component A to component B is 100 : 30~50; wherein, the molecular weight of polyether polyol I is 3000~5000, the viscosity is 1000~3000mPa·s, and the functionality is 2~4; the molecular weight of polyether polyol II is 500~1000, the viscosity is 100~500mPa·s, the functionality is 2~4, and the molecular weight of polymer polyol is 6000~8000, the viscosity is 3000~5000mPa·s, and the functionality is 2~4.
[0009] (2) A continuous production line is used to foam the polyurethane sponge. The material enters the mixing foaming system through a metering pump, and a gas inert to the reaction materials is injected into the mixing gun head. The gas pressure is 1 to 2 bar.
[0010] (3) The polyurethane sponge obtained by foaming is matured for 48 to 84 hours; and sliced to obtain an inflated slow-rebound sponge material.
[0011] In the above technical solution, preferably, the polyether polyol I is selected from at least one of CHF-5120VE and CHE-204; the polyether polyol II is selected from at least one of CHE-307 and CHE-330N; and the polymer polyol is CHP-H45.
[0012] In the above technical solution, preferably, the component A further comprises a storage stabilizer, and 0.5 to 1 part of the storage stabilizer is added in parts by weight; the storage stabilizer is selected from one of phosphoric acid or benzoyl chloride.
[0013] In the above technical solution, preferably, the cell opener is selected from CHE-350D or SKC-1900; the catalyst is selected from at least one of complex amine or T19; the foam stabilizer is selected from at least one of B-8002, L-580 or HC-8240; the foaming agent is water; the cross-linking agent is DEVA; and the isocyanate is selected from at least one of 1100 or M20S.
[0014] In the above technical solution, preferably, the gas inert to the reaction materials is nitrogen with a purity of 99.99%, and the flow rate is controlled at 100±20 L / h.
[0015] In the above technical scheme, preferably, the foaming process of the continuous production line includes: foaming head control, constant temperature storage tank, premix, foaming production; the raw materials are put into the constant temperature storage tank for premixing through the foaming head control metering pump, component A controls the material temperature to about 25±3°C, the main stirring rate is 5000±200rpm, the silicone oil stirring is 5000±200rpm, and the mixing head pressure is set to 2.8±0.2kg / cm 2 .
[0016] In the present invention, the polyol mixture with a special structure in component A can neutralize aldehyde substances in the reaction process, reduce the generation of irritating odor, and the addition of nitrogen makes the foam more open-pore. After the polyurethane sponge is matured and sliced, the residual aldehyde substances can be volatilized for a second time, thereby achieving the effect of reducing aldehydes. The introduction of polyether polyol and an appropriate amount of polymer polyol greatly increases the content of polar groups in the polyol and increases the intermolecular force. Then, modified isocyanate is added to combine with it to prepare a slow-rebound sponge with inflation, which makes the supporting performance better. The inflation slow-rebound sponge has a 40% depression hardness greater than 65N and a 1cm cell number greater than 30. DETAILED DESCRIPTION
[0017] The present invention will be further described below by way of examples, but are not limited thereto.
[0018] Table 1 Raw material list and flow setting
[0019]
[0020]
[0021] [Example 1]
[0022] (1) Component preparation: Component A: 30 parts CHF-5120VE, 35 parts CHE-307, 35 parts CHP-H45, 0.6 parts complex amine, 0.2 parts T19, 1.2 parts B-8002, 1 part DEVA, 5 parts SKC-1900, 1 part water; Component B: 30 parts 1100.
[0023] (2) A continuous production line is used to foam the polyurethane sponge. The material enters the mixing foaming system through a metering pump, and a pressurized high-purity inert gas that does not participate in the reaction is injected into the mixing gun head. The gas pressure is 1 to 2 bar.
[0024] (3) The polyurethane sponge obtained by foaming is matured for 48 hours, and then sliced to obtain an inflated slow-rebound sponge material.
[0025] The performance test data of the prepared slow-rebound inflatable sponge are shown in Table 3.
[0026] [Examples 2 to 6]
[0027] Examples 2 to 6 follow the steps of Example 1, except that the reaction raw materials and raw material ratios are different, as shown in Table 2. The performance test results of the prepared slow-rebound inflatable sponge material are shown in Table 3.
[0028] [Comparative Example 1]
[0029] (1) Component preparation: Component A: 35 parts CHF-5120VE, 35 parts CHE-307, 30 parts CHP-H45, 0.8 parts complex amine, 1.4 parts HC-8240, 1.2 parts DEVA, 5 parts CHE-350D, 1.2 parts water; Component B: 40 parts LL.
[0030] (2) A continuous production line is used to foam the polyurethane sponge, and the material is fed into a mixing foaming system through a metering pump.
[0031] (3) The polyurethane sponge obtained by foaming is matured for 48 hours; and sliced to obtain an inflated slow-rebound sponge material.
[0032] The performance test data of the prepared slow-rebound inflatable sponge material are shown in Table 3.
[0033] [Comparative Examples 2-3]
[0034] Comparative Examples 2 to 3 follow the steps of Comparative Example 1, except that the reaction raw materials and raw material ratios are different, as shown in Table 2. The performance test results of the prepared slow-rebound inflatable sponge material are shown in Table 3.
[0035] Table 2 Weight parts of raw materials of each component in Examples 1 to 6 and Comparative Examples 1 to 3
[0036]
[0037] Table 3 Inflatable slow rebound sponge material performance test data
[0038]
[0039]
[0040] Examples 1 to 6 are for preparing inflation slow-rebound sponge materials using component A and component B of the present invention, and comparative examples 1 to 3 are the preparation routes of conventional slow-rebound cushioning materials. From the data, it can be seen that the 40% depression hardness and surface hardness of comparative example 1 are better than those of examples 1 to 6, but the formaldehyde content is higher and the number of pores is smaller, resulting in a stronger sponge odor and an uneven pore structure, mainly because no gas inert to the reaction materials is used; the number of pores in comparative example 2 is similar to that of the embodiment, but the 40% depression hardness and surface hardness are lower, resulting in insufficient sponge support performance, and the depression hardness, surface hardness, and number of pores in comparative example 3 are all lower. The performances of examples 1 to 6 are relatively stable, and the comprehensive performance is relatively excellent. Among them, example 3 is the most preferred, and the formaldehyde of aldehyde substances is controlled to be 23ug / m 3 、 Acetaldehyde is 9ug / m 3 It has a finer pore size, 33 cells within 1 cm, a depression hardness of 72.1N and a surface hardness of 32.9F, which improves the pore structure and enhances the supporting performance.
[0041] The above content introduces in detail the preparation method of the slow-rebound sponge material provided by the present invention. The embodiments in this article illustrate the principle and implementation mode of the present invention. The introduction of the above embodiments is only for understanding the core idea of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the art shall make modifications to the present invention without departing from the principle of the present invention, and the modifications shall fall within the protection scope of the claims.
Claims
1. A method for preparing a slow-rebound sponge material comprising the following steps: (1) Preparation of components: by weight, component A: 30-50 parts of polyether polyol I, 20-40 parts of polyether polyol II, 30-50 parts of polymer polyol, 5-8 parts of cell opener, 1.2-1.8 parts of foam stabilizer, 0.5-1 parts of catalyst, 1-1.5 parts of foaming agent, 1-2 parts of crosslinking agent; component B: 30-50 parts of isocyanate; the weight ratio of polyol in component A to component B is 100 : 30~50; wherein, the molecular weight of polyether polyol I is 3000~5000, the viscosity is 1000~3000mPa·s, and the functionality is 2~4; the molecular weight of polyether polyol II is 500~1000, the viscosity is 100~500mPa·s, the functionality is 2~4, and the molecular weight of polymer polyol is 6000~8000, the viscosity is 3000~5000mPa·s, and the functionality is 2~4. (2) A continuous production line is used to foam the polyurethane sponge. The material enters the mixing foaming system through a metering pump, and a gas inert to the reaction materials is injected into the mixing gun head. The gas pressure is 1 to 2 bar. (3) The polyurethane sponge obtained by foaming is matured for 48 to 84 hours; and sliced to obtain an inflated slow-rebound sponge material.
2. The method for preparing the slow-rebound sponge material according to claim 1, characterized in that: The polyether polyol I is selected from at least one of CHF-5120VE and CHE-204; the polyether polyol II is selected from at least one of CHE-307 and CHE-330N; and the polymer polyol is CHP-H45.
3. The method for preparing the slow-rebound sponge material according to claim 1, characterized in that: The component A also includes a storage stabilizer, which is added in an amount of 0.5 to 1 part by weight; the storage stabilizer is selected from one of phosphoric acid and benzoyl chloride.
4. The method for preparing the slow-rebound sponge material according to claim 1, characterized in that: The cell opener is selected from at least one of CHE-350D and SKC-1900; the foam stabilizer is selected from at least one of B-8002, L-580 and HC-8240; the catalyst is selected from at least one of complex amine and T19; the foaming agent is water; the cross-linking agent is DEVA; and the isocyanate is selected from at least one of 1100 and M20S.
5. The method for preparing the slow-rebound sponge material according to claim 1, characterized in that: The gas inert to the reaction materials is nitrogen with a purity of 99.99%, and the flow rate is controlled at 100±20L / h.
6. The method for preparing the slow-rebound sponge material according to claim 1, characterized in that: The foaming process of the continuous production line includes: foaming head control, constant temperature storage tank, premix, foaming production; the raw materials are put into the constant temperature storage tank for premixing through the foaming head control metering pump, component A controls the material temperature to about 25±3°C, the main stirring rate is 5000±200rpm, the silicone oil stirring is 5000±200rpm, and the mixing head pressure is set to 2.8±0.2kg / cm 2 .