Flame-retardant polyurethane composition as well as preparation method and application thereof
By using a flame-retardant polyurethane composition combining polyether polyol and crosslinking agent in the potting glue, the problems of flame retardant performance, fluidity and temperature fluctuations in potting glue in new energy vehicles are solved, and efficient flame retardant performance is achieved and stable foam density.
Patent Information
- Application Number
- CN202411424984.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-07-24
- Filing Date
- 2024-10-12
- Publication Date
- 2024-12-06
AI Technical Summary
In the application of new energy vehicles, existing potting adhesives have insufficient flame retardant performance, fluidity, shear strength and foam density with temperature variation, especially the poor compatibility and deterioration of component compatibility of solid flame retardants. question.
Using a flame retardant polyurethane composition, the structure and composition of the first, second and third polyether polyols, crosslinking agents and composite flame retardants are optimized to improve fluidity, flame retardant properties and shearing Strength and temperature fluctuations in foaming density are reduced by gelability and permeability of the third polyether polyol.
The good fluidity, flame retardant performance, shear strength and foam density of potting adhesives are achieved, meeting the application needs of new energy vehicles.
Smart Images

Figure BDA0005081896710000021 
Figure BDA0005081896710000051 
Figure BDA0005081896710000091
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of potting adhesives, and more specifically, to a flame retardant polyurethane composition and a preparation method and application thereof. Background Art
[0002] Potting compound is a material used to close, seal and fix electronic components. When in use, the potting compound needs to flow evenly into a narrow gap, so the fluidity of the potting compound is required to be high. In recent years, when applied to batteries, especially new energy vehicle batteries, higher requirements have been put forward for the flame retardancy and shear strength of the potting compound.
[0003] The safety of new energy vehicles is particularly important, among which, potting glue with good flame retardant properties is crucial for new energy vehicles. In order to improve the flame retardant properties of potting glue in the prior art, the main method is to add flame retardants. Flame retardants include solid flame retardants and liquid flame retardants. Solid flame retardants have poor compatibility with the components of potting glue and are prone to stratification of the potting glue. Their addition will cause the fluidity of the potting glue to deteriorate and may have a certain negative impact on the shear strength of the potting glue. Therefore, solid flame retardants are rarely used at this stage. Liquid flame retardants have good compatibility with the components of potting glue, which can keep the potting glue in good fluidity, but liquid flame retardants need to be added in large quantities to achieve a good flame retardant effect.
[0004] It is also worth noting that with the development of the lightweight trend of new energy vehicles, low-density potting glue is more suitable for new energy vehicles. Among them, the density of foaming potting glue is lower and more competitive. However, during the use of foaming potting glue, it mainly contacts with large metal parts of the car. Large metal parts absorb heat quickly and absorb a lot of heat, which causes the foaming density of the potting glue to be greatly affected by the ambient temperature. For example, the workshop temperature in summer is high (28°C), and the foaming ratio of the existing potting glue is about 5 times, which makes the foaming density small; the workshop temperature in winter is low (18°C), and the foaming ratio of the same potting glue is about 3.5 times, which makes the foaming density large. The foaming density of the potting glue fluctuates greatly with the change of ambient temperature, which affects the fit and precision of the components, brings difficulties to the design of the components and the assembly of the whole vehicle, and may even cause quality problems of the whole vehicle.
[0005] The potting compound mentioned in patent CN110392945A has good flame retardancy, but it does not pay attention to the fluctuation of the foaming density of the potting compound with the change of ambient temperature.
[0006] Therefore, it is necessary to develop a potting compound with good flame retardancy, good fluidity, good shear strength and small fluctuation of foaming density with temperature to meet its application in the field of new energy vehicles. Summary of the invention
[0007] The primary purpose of the present invention is to overcome the problem of poor or inadequate performance of the above-mentioned prior art potting glue and provide a flame retardant polyurethane composition.
[0008] A further object of the present invention is to provide a method for preparing the flame retardant polyurethane composition.
[0009] A further object of the present invention is to provide use of the flame retardant polyurethane composition in preparing a potting compound.
[0010] The above-mentioned object of the present invention is achieved by the following technical solutions:
[0011] A flame retardant polyurethane composition, comprising component A and component B in a mass ratio of 1:(1-1.2);
[0012] The component A comprises the following components in parts by weight:
[0013]
[0014] The first polyether polyol is prepared using sucrose and / or sorbitol as an initiator; the second polyether polyol is prepared using diol as an initiator; the third polyether polyol is prepared using castor oil as an initiator;
[0015] The composite flame retardant comprises a liquid flame retardant and a solid flame retardant in a mass ratio of 1: (0.5-3);
[0016] The component B comprises the following components in parts by weight: 90 to 100 parts of NCO-containing polyurethane prepolymer.
[0017] The inventor of the present invention has found through research that the first polyether polyol is used as the main polyol of component A, which is prepared with sucrose and / or sorbitol as an initiator, has a high functionality and a strong reaction network skeleton, so it has little dependence on external energy during the reaction, thereby reducing the fluctuation of the foaming density of the flame retardant polyurethane composition with temperature to a certain extent. On this basis, a certain amount of the third polyether polyol is also added. Since the third polyether polyol is prepared with castor oil as an initiator, it has good gelation and permeability, so it can preferentially penetrate into the surface of the substrate to be bonded during foaming, blocking the substrate to be bonded from absorbing heat of the flame retardant polyurethane composition, thereby making the temperature change of the flame retardant polyurethane composition during foaming small, and the foaming density remains stable. In addition, the addition of the third polyether polyol can also significantly improve the shear strength of the flame retardant polyurethane composition.
[0018] The addition of the cross-linking agent can not only improve the shear strength of the flame retardant polyurethane composition, but also promote the reaction during the foaming of the flame retardant polyurethane composition, thereby reducing the fluctuation of the foaming density with temperature.
[0019] If only the first polyether polyol and the second polyether polyol are used in component A, the fluidity of the flame retardant polyurethane composition will be poor. In the present invention, the fluidity of the flame retardant polyurethane composition is improved by further adding the second polyether polyol.
[0020] The inventors of the present invention have also found that the composite flame retardant obtained by compounding the liquid flame retardant and the solid flame retardant has good dispersibility in the polyether polyol system of the present invention, which is conducive to exerting the flame retardant effect of the composite flame retardant and improving the flame retardant properties of the flame retardant polyurethane composition. In addition, by replacing the liquid flame retardant with part of the solid flame retardant, the temperature change of the flame retardant polyurethane composition during foaming is smaller, which is conducive to reducing the fluctuation of the foaming density of the flame retardant polyurethane composition with temperature.
[0021] That is, the flame-retardant polyurethane composition obtained by the combination of three polyether polyols, a crosslinking agent and a composite flame retardant has good fluidity, good flame retardant properties, good shear strength and small fluctuation of foaming density with temperature when used as a potting glue.
[0022] In the present invention:
[0023] In component A: the amount of the first polyether polyol can be 30, 32, 35, 36, 38 or 40 parts; the amount of the second polyether polyol can be 5, 6, 7, 8, 9 or 10 parts; the amount of the third polyether polyol can be 10, 12, 14 or 15 parts; the amount of the cross-linking agent can be 5, 6, 8, 9, 10, 12 or 15 parts; the amount of the catalyst can be 0.3, 0.5, 0.8 or 1 part; the amount of the foaming agent can be 0.3, 0.5, 0.8 or 1 part; the amount of the composite flame retardant can be 10, 12, 15, 18, 20, 25, 28 or 30 parts.
[0024] In component B: the amount of the NCO-containing polyurethane prepolymer can be 90, 92, 94, 95, 96, 98 or 100 parts.
[0025] Preferably, in the flame retardant polyurethane composition, the mass percentage of the composite flame retardant is not higher than 15%.
[0026] The flame retardant polyurethane composition of the present invention can achieve good flame retardant effect (6mmV-0 / 8mmV-0) under the condition of low content of composite flame retardant.
[0027] Preferably, the viscosity of the first polyether polyol at 25° C. is 4000 to 20000 mPa·s, and specifically may be 4000, 5000, 6000, 8000, 10000, 12000, 15000, 18000, or 20000 mPa·s.
[0028] Preferably, the viscosity of the second polyether polyol at 25° C. is 100 to 1000 mPa·s, and may specifically be 100, 300, 500, 800 or 1000 mPa·s.
[0029] More preferably, the viscosity of the second polyether polyol at 25° C. is 100 to 500 mPa·s.
[0030] Preferably, the viscosity of the third polyether polyol at 25° C. is 3000 to 10000 mPa·s, and specifically may be 3000, 4000, 5000, 6000, 8000 or 10000 mPa·s.
[0031] More preferably, the viscosity of the third polyether polyol at 25° C. is 3500-5000 mPa·s.
[0032] Preferably, the hydroxyl value of the first polyether polyol is 250-500 mgKOH / g, and can be specifically 250, 280, 300, 320, 350, 400 or 500 mgKOH / g.
[0033] Preferably, the hydroxyl value of the second polyether polyol is 50-200 mgKOH / g, and can be 50, 80, 100, 120, 150, 180 or 200 mgKOH / g.
[0034] Preferably, the hydroxyl value of the third polyether polyol is 150-400 mgKOH / g, and specifically may be 150, 180, 200, 250, 280, 300, 320, 350 or 400 mgKOH / g.
[0035] Preferably, the first polyether polyol, the second polyether polyol and the third polyether polyol are independently EO polyether, PO polyether or EO / PO copolymer polyether.
[0036] Preferably, the diol is at least one of diethylene glycol, ethylene glycol or propylene glycol.
[0037] Preferably, the crosslinking agent is bisphenol A polyether.
[0038] More preferably, the bisphenol A polyether is at least one of bisphenol-A polyoxypropylene ether or bisphenol-A polyoxyethylene ether.
[0039] Preferably, the catalyst is at least one of a tertiary amine catalyst or a delayed catalyst.
[0040] More preferably, the tertiary amine catalyst is at least one of triethylenediamine or pentamethyldialkylenetriamine.
[0041] More preferably, the delayed catalyst is at least one of C225 produced by Tonglan Chemical or A-300 produced by Maitu.
[0042] Preferably, the composite flame retardant comprises a liquid flame retardant and a solid flame retardant in a mass ratio of 1:(1-1.5).
[0043] Preferably, the liquid flame retardant is at least one of triethyl phosphate, triphenyl phosphate, dimethyl methylphosphonate, diethyl ethylphosphonate, tris(2-chloropropyl)phosphate or tris(2,3-dichloropropyl)phosphate.
[0044] The addition of solid flame retardant can effectively prevent the hydrolysis of the flame retardant and improve the stability of the flame retardant polyurethane composition.
[0045] Preferably, the solid flame retardant has a reactive active group hydroxyl group, and crystallizes at room temperature (20-35° C.) or is solid at room temperature (20-35° C.).
[0046] Preferably, the solid flame retardant is at least one of polyalkoxy alcohol phosphate, pentaerythritol phosphate or halogen-containing aromatic diphenol diglycerol ether.
[0047] More preferably, the solid flame retardant is pentaerythritol phosphate. When pentaerythritol phosphate is used as the solid flame retardant, the obtained flame retardant polyurethane composition has better fluidity and smaller fluctuation of foaming density with temperature.
[0048] More preferably, the halogen-containing aromatic diphenol diglycerol ether is
[0049]
[0050] wherein X represents Cl or Br or H, and at least one X is Cl or Br.
[0051] Preferably, the polyalkoxy alcohol phosphate is at least one of methoxy polyethylene glycol phosphate or ethoxy polyethylene glycol phosphate.
[0052] Preferably, the component A further comprises 1 to 5 parts of a surfactant.
[0053] More preferably, the surfactant is at least one of a polyol surfactant or a silicone surfactant.
[0054] Preferably, the blowing agent is water.
[0055] Preferably, the component B further comprises 0.3 to 1 part of a silane coupling agent.
[0056] More preferably, the silane coupling agent includes but is not limited to isocyanate silane.
[0057] Preferably, the NCO-containing polyurethane prepolymer is obtained by reacting isocyanate and a fourth polyether polyol; and the fourth polyether polyol is prepared using castor oil as an initiator.
[0058] More preferably, the isocyanate is at least one of diphenylmethane diisocyanate (MDI), polymethylene polyphenyl polyisocyanate, isophorone diisocyanate (IPDI), hexamethylene diisocyanate (HDI) or polymeric MDI.
[0059] More preferably, the mass ratio of the fourth polyether polyol to isocyanate is 1:(8-12).
[0060] More preferably, the viscosity of the fourth polyether polyol at 25° C. is 3000-10000 mPa·s (specifically 3000, 4000, 5000, 6000, 8000 or 10000 mPa·s); the hydroxyl value of the fourth polyether polyol is 150-400 mgKOH / g (specifically 150, 180, 200, 250, 280, 300, 320, 350 or 400 mgKOH / g).
[0061] The method for preparing the flame retardant polyurethane composition comprises the following steps: mixing the components of component A to obtain component A; and mixing the components of component B to obtain component B.
[0062] The use of the flame retardant polyurethane composition in the preparation of potting glue is also within the protection scope of the present invention.
[0063] Compared with the prior art, the present invention has the following beneficial effects:
[0064] The flame-retardant polyurethane composition obtained by the present invention by combining three polyether polyols, a cross-linking agent and a composite flame retardant has good fluidity, good flame retardant properties, good shear strength and small fluctuation of foaming density with temperature when used as a potting glue, thereby meeting its application in the field of new energy vehicles. DETAILED DESCRIPTION
[0065] In order to more clearly and completely describe the technical solution of the present invention, the present invention is further described in detail through specific embodiments below. It should be understood that the specific embodiments described herein are only used to explain the present invention, and are not used to limit the present invention. Various changes can be made within the scope of the rights of the present invention.
[0066] Example 1
[0067] This embodiment provides a flame retardant polyurethane composition, comprising component A and component B in a mass ratio of 1:1.1;
[0068] Component A includes the following components in parts by weight: 35 parts of a first polyether polyol, 8 parts of a second polyether polyol, 12 parts of a third polyether polyol, 10 parts of a crosslinking agent, 0.6 parts of a catalyst, 25 parts of a composite flame retardant, 1 part of a surfactant, and 0.6 parts of a foaming agent;
[0069] Among them, in component A: the first polyether polyol is polyether polyol 380, which is prepared using sucrose as the initiator; the second polyether is polyether polyol 220, which is prepared using propylene glycol as the initiator; the third polyether polyol is Japan Ito AC-009, which is prepared using castor oil as the initiator; the cross-linking agent is bisphenol-A polyoxypropylene ether; the catalyst is triethylenediamine; the composite flame retardant includes a liquid flame retardant and a solid flame retardant in a mass ratio of 1:1.5, the liquid flame retardant is triethyl phosphate, and the solid flame retardant is pentaerythritol phosphate; the surfactant is Meside 8818; and the foaming agent is water.
[0070] Component B includes the following components in parts by weight: 99 parts of NCO-containing polyurethane prepolymer and 1 part of silane coupling agent;
[0071] Among them, in component B: the NCO-containing polyurethane prepolymer is obtained by reacting a fourth polyether polyol and isocyanate in a mass ratio of 1:11 at 80°C for 25 minutes, the fourth polyether polyol is Japan Ito AC-009, prepared with castor oil as an initiator; the isocyanate is polymerized MDI, Wanhua; the silane coupling agent is isocyanate silane.
[0072] The preparation method of the flame retardant polyurethane composition of this embodiment comprises the following steps:
[0073] Weigh each component of component A according to the formula, disperse and stir evenly at 30° C. to obtain component A; weigh each component of component B according to the formula, mix evenly in vacuum stirring to obtain component B, and then obtain a flame retardant polyurethane composition.
[0074] Example 2
[0075] This embodiment provides a flame retardant polyurethane composition, which is different from that of embodiment 1 in that the mass ratio of component A to component B is 1:1.2;
[0076] Component A includes the following components in parts by weight: 40 parts of a first polyether polyol, 5 parts of a second polyether polyol, 15 parts of a third polyether polyol, 5 parts of a crosslinking agent, 0.3 parts of a catalyst, 30 parts of a composite flame retardant, 1 part of a surfactant, and 1 part of a foaming agent;
[0077] Component B includes the following components in parts by weight: 90 parts of NCO-containing polyurethane prepolymer and 0.3 parts of silane coupling agent.
[0078] Example 3
[0079] This embodiment provides a flame retardant polyurethane composition, which is different from Embodiment 1 in that: the mass ratio of component A to component B is 1:1;
[0080] Component A includes the following components in parts by weight: 30 parts of a first polyether polyol, 10 parts of a second polyether polyol, 10 parts of a third polyether polyol, 15 parts of a crosslinking agent, 1 part of a catalyst, 15 parts of a composite flame retardant, 3 parts of a surfactant, and 0.3 parts of a foaming agent;
[0081] Component B includes the following components in parts by weight: 100 parts of NCO-containing polyurethane prepolymer and 0.3 parts of silane coupling agent.
[0082] Example 4
[0083] This embodiment provides a flame retardant polyurethane composition, which is different from Embodiment 1 in that triethyl phosphate is replaced by dimethyl methylphosphonate.
[0084] Example 5
[0085] This embodiment provides a flame retardant polyurethane composition, which is different from Embodiment 1 in that pentaerythritol phosphate is replaced by methoxy polyethylene glycol phosphate.
[0086] Example 6
[0087] This embodiment provides a flame retardant polyurethane composition, which is different from Embodiment 1 in that bisphenol-A polyoxypropylene ether is replaced by bisphenol-A polyoxyethylene ether.
[0088] Example 7
[0089] This embodiment provides a flame retardant polyurethane composition, which is different from Embodiment 1 in that: in the composite flame retardant, the mass ratio of the liquid flame retardant to the solid flame retardant is 1:1.
[0090] Example 8
[0091] This embodiment provides a flame retardant polyurethane composition, which is different from Embodiment 1 in that the amount of the composite flame retardant is 20 parts.
[0092] Example 9
[0093] This embodiment provides a flame retardant polyurethane composition, which is different from Embodiment 1 in that the first polyether polyol is polyether polyol YD-600, which is prepared using sorbitol as an initiator.
[0094] Comparative Example 1
[0095] This comparative example provides a flame retardant polyurethane composition, which is different from Example 1 in that: the first polyether polyol is not added to component A, the amount of the second polyether polyol is 28 parts, and the amount of the third polyether polyol is 27 parts.
[0096] Comparative Example 2
[0097] This comparative example provides a flame retardant polyurethane composition, which is different from Example 1 in that: the second polyether polyol is not added to component A, the amount of the first polyether polyol is 40 parts, and the amount of the third polyether polyol is 15 parts.
[0098] Comparative Example 3
[0099] This comparative example provides a flame retardant polyurethane composition, which is different from Example 1 in that: the third polyether polyol is not added to component A, the amount of the first polyether polyol is 40 parts, and the amount of the second polyether polyol is 15 parts.
[0100] Comparative Example 4
[0101] This comparative example provides a flame retardant polyurethane composition, which is different from Example 1 in that the composite flame retardant in component A is replaced by an equal amount of liquid flame retardant triethyl phosphate.
[0102] Comparative Example 5
[0103] This comparative example provides a flame retardant polyurethane composition, which is different from Example 1 in that no crosslinking agent is added to component A.
[0104] Performance Testing
[0105] The flame retardant polyurethane compositions of the embodiments and comparative examples were tested according to the following test standards and test methods.
[0106] Fluidity: Test temperature 25℃, flow interface aluminum sheet (3 series)-polycarbonate (aluminum sheet and polycarbonate are separated by copper wire), sample size 100mm±0.25mm in length, 25mm±0.25mm in width, 2.0mm±0.1mm in thickness. The aluminum sheet is placed horizontally and glue is dispensed at one end of the aluminum sheet (20g) to make the glue flow horizontally along the gap between the aluminum sheets and measure the flow distance. The flow gap is 1.0mm. The longer the flow distance, the better the fluidity.
[0107] Foaming density: GB / T 533-2008; the density of the test sample after foaming at 18°C and 28°C is then calculated, and the difference in density between the two temperatures (density difference) is used to measure the fluctuation of the foaming density with temperature; the larger the density difference, the greater the fluctuation of the foaming density with temperature, and vice versa.
[0108] Flame retardant properties: GB / T2408-2021 (UL94).
[0109] Shear strength: GB / T 7124-2008.
[0110] The test results of the flame retardant polyurethane compositions of various embodiments and comparative examples are shown in Table 1 below.
[0111] Table 1
[0112]
[0113] From Table 1, we can see that:
[0114] The flowability of the flame retardant polyurethane compositions of Examples 1 to 9 was all above 63 mm, and the difference in foaming density after foaming at different temperatures was all within 0.013 g / cm 3 The flame retardant grades are all V-0 (6 mm) or V-0 (8 mm), and the shear strengths are all above 2.2 MPa, indicating that the flame retardant polyurethane composition of the present invention has good fluidity, good flame retardant properties, good shear strength, and small fluctuation of foaming density with temperature as a potting adhesive.
[0115] Component A of Comparative Example 1 does not contain the first polyether polyol, and the foaming density of the flame-retardant polyurethane composition obtained fluctuates greatly with changes in temperature, and the shear strength is poor. Component A of Comparative Example 2 does not contain the second polyether polyol, and the fluidity of the flame-retardant polyurethane composition obtained is poor. Component A of Comparative Example 3 does not contain the second polyether polyol, and the shear strength of the flame-retardant polyurethane composition obtained is poor, and the foaming density fluctuates greatly with changes in temperature. The flame retardant of Comparative Example 4 only uses liquid flame retardants, and the shear strength of the flame-retardant polyurethane composition obtained is poor, the foaming density fluctuates greatly with changes in temperature, and the flame retardant performance is poor. Component A of Comparative Example 5 does not add a cross-linking agent, and the shear strength of the flame-retardant polyurethane composition obtained is not as good as that of Example 1, and the foaming density fluctuates greatly with changes in temperature.
[0116] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A flame retardant polyurethane composition, characterized in that: It includes component A and component B in a mass ratio of 1:(1-1.2); The component A comprises the following components in parts by weight: The first polyether polyol is prepared using sucrose and / or sorbitol as an initiator; the second polyether polyol is prepared using diol as an initiator; the third polyether polyol is prepared using castor oil as an initiator; The composite flame retardant comprises a liquid flame retardant and a solid flame retardant in a mass ratio of 1: (0.5-3); The component B comprises the following components in parts by weight: 90 to 100 parts of NCO-containing polyurethane prepolymer.
2. The flame retardant polyurethane composition according to claim 1, characterized in that: In the flame retardant polyurethane composition, the mass percentage of the composite flame retardant is not higher than 15%.
3. The flame retardant polyurethane composition according to claim 1, characterized in that: The viscosity of the first polyether polyol at 25° C. is 4000-20000 mPa·s; the viscosity of the second polyether polyol at 25° C. is 100-1000 mPa·s; and the viscosity of the third polyether polyol at 25° C. is 3000-10000 mPa·s.
4. The flame retardant polyurethane composition according to claim 1, characterized in that: The hydroxyl value of the first polyether polyol is 250-500 mgKOH / g; the hydroxyl value of the second polyether polyol is 50-200 mgKOH / g; and the hydroxyl value of the third polyether polyol is 150-400 mgKOH / g.
5. The flame retardant polyurethane composition according to claim 1, characterized in that: The crosslinking agent is bisphenol A polyether.
6. The flame retardant polyurethane composition according to claim 1, characterized in that: The liquid flame retardant is at least one of triethyl phosphate, triphenyl phosphate, dimethyl methylphosphonate, diethyl ethylphosphonate, tris(2-chloropropyl)phosphate or tris(2,3-dichloropropyl)phosphate.
7. The flame retardant polyurethane composition according to claim 1, characterized in that: The solid flame retardant is at least one of polyalkoxy alcohol phosphate, pentaerythritol phosphate or halogen-containing aromatic diphenol diglycerol ether.
8. The flame retardant polyurethane composition according to claim 1, characterized in that: The NCO-containing polyurethane prepolymer is obtained by reacting isocyanate and a fourth polyether polyol; the fourth polyether polyol is prepared using castor oil as an initiator.
9. The method for preparing the flame retardant polyurethane composition according to any one of claims 1 to 8, characterized in that: The method comprises the following steps: mixing the components of component A to obtain component A; and mixing the components of component B to obtain component B.
10. Use of the flame retardant polyurethane composition according to any one of claims 1 to 8 in the preparation of potting glue.
Citation Information
Patent Citations
Polyurethane foam material and application thereof
CN117820596A
Resin composition
JP2012102324A
Polyethyleneglycolphosphate and methods ofsynthesizing the same and utilizing the same as aradioprotectant
KR1020010048958A
Multi-part polyurethane compositions, articles thereof, and method of making
US20160145476A1
Process for the preparation of polyether phosphates
US6500917B1