Lignin-based polysaccharide sensing hydrogel with adjustable toughness and rigidity and preparation method of lignin-based polysaccharide sensing hydrogel

By adopting a dual network structure in the hydrogel, lignin and polymer monomers form a hydrophobic network, and forming an ionic bond network through polysaccharides and calcium salts, the problem of inverse proportionality of traditional hydrogels is solved, and the problem of inverse proportionality of traditional hydrogels is achieved. Hydrogels with high tear energy and high elastic modulus have excellent sensing performance.

CN119081165AInactive Publication Date: 2024-12-06SHAANXI UNIV OF SCI & TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411173748.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional hydrogels usually sacrifice toughness when pursuing high stiffness, resulting in brittleness; conversely, when pursuing ultra-toughness, it is difficult to achieve mechanical properties with high tear energy and high elastic modulus.

Method used

Using a dual network hydrogel structure, a first network of hydrophobic bonding is formed through lignin and polymer monomers, and a second network is formed by regulating the cross-linking density of polysaccharides and calcium salts, thereby achieving adjustable toughness.

Benefits of technology

The high tearing energy (50,000~100,000J m-2) and high elastic modulus (6~12MPa) of the hydrogel are achieved, and excellent strain sensitivity and sensing performance are also provided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081165A_ABST
    Figure CN119081165A_ABST
Patent Text Reader

Abstract

The invention discloses toughness and rigidity adjustable lignin-based polysaccharide sensing hydrogel and a preparation method thereof.The preparation method specifically comprises the steps that a polymer monomer, polysaccharide and a solvent A are mixed and stirred, an initiator is added, and a polymer monomer solution B is obtained; carrying out free radical polymerization reaction on the polymer monomer solution B under UV, and drying by distillation to obtain a polymer solid C; fully mixing the polymer solid C with a solvent B, adding lignin, and drying by distillation after complete mixing to obtain lignin-based polysaccharide xerogel D; and soaking the lignin-based polysaccharide xerogel D in a calcium salt solution to obtain the toughness and rigidity adjustable lignin-based polysaccharide sensing hydrogel. The lignin-based polysaccharide sensing hydrogel is a double-network hydrogel, and lignin and a polymer monomer are hydrophobically combined to form a first layer of network. And the crosslinking density of the second-layer network is regulated and controlled by regulating and controlling the variety and proportion of the polysaccharide and the calcium salt, so that high toughness, high rigidity and excellent sensing performance are realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of fabric preparation, and in particular relates to a method for preparing a lignin-based polysaccharide sensing hydrogel with adjustable toughness and stiffness, and also relates to the lignin-based polysaccharide sensing hydrogel with adjustable toughness and stiffness. Background Art

[0002] Hydrogels are three-dimensional polymer networks made of natural or synthetic materials. Due to their hydrophilicity, high flexibility, and biocompatibility, they are widely used in agriculture, food engineering, drug delivery, and other fields. In other application areas, the required hydrogels also need to have other corresponding properties. For example, in tissue engineering, hydrogels used as scaffolds need to meet good tearing energy requirements. In emerging fields such as soft electronics, hydrogels with mechanical properties are also required to have good sensing properties. Therefore, for these fields, it is crucial to develop a hydrogel with comprehensive mechanical properties.

[0003] Traditional single-network hydrogels often have poor mechanical properties, which are mainly affected by their swelling ratio, which is determined by the balance between osmotic pressure and network elasticity. Therefore, the stiffness of the hydrogel network can be increased by adjusting the crosslinking density, thereby affecting the swelling ratio. Although this method improves the stiffness, it causes the hydrogel to be brittle; to solve this problem, researchers have improved the toughness of hydrogels by adding nanomaterials or using dynamic crosslinks (such as ionic bonds, hydrogen bonds, coordination complexes, and hydrophobic interactions). However, stiffness and toughness in polymer networks are often inversely proportional. Most conventional hydrogels sacrifice toughness to obtain high rigidity, making the hydrogel brittle (low tear energy, ~10Jm-2), or sacrifice stiffness to obtain super toughness, making the hydrogel soft and unable to resist external forces (low elastic modulus, ~10kPa). Therefore, it is still a major challenge to achieve super toughness and high stiffness of hydrogels. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing a lignin-based polysaccharide sensing hydrogel with adjustable toughness and stiffness. The hydrogel has toughness with high tearing energy and rigidity with high elastic modulus.

[0005] Another object of the present invention is to provide a lignin-based polysaccharide sensing hydrogel with adjustable toughness and stiffness.

[0006] The technical solution adopted by the present invention is a method for preparing a lignin-based polysaccharide sensing hydrogel with adjustable toughness and stiffness, which is specifically implemented according to the following steps:

[0007] Step 1, mixing polymer monomers, polysaccharides and solvent A, stirring them thoroughly to make them uniformly mixed, and then adding an initiator to obtain a polymer monomer solution B;

[0008] Step 2, subjecting the polymer monomer solution B to a free radical polymerization reaction under UV to obtain a polymer long chain solution, which is evaporated to dryness to obtain a polymer solid C;

[0009] Step 3, fully mixing the polymer solid C and the solvent B, then adding lignin, mixing completely and evaporating to dryness to obtain a lignin-based polysaccharide xerogel D;

[0010] Step 4, soaking the lignin-based polysaccharide dry gel D in a calcium salt solution to obtain a lignin-based polysaccharide sensing hydrogel with adjustable toughness and stiffness.

[0011] The present invention is also characterized in that:

[0012] In step 1, the mass volume ratio of the polymer monomer, the initiator, the polysaccharide and the solvent A is 0.01-10:0.001-0.01:0.005-2:5-15.

[0013] In step 1, the polymer monomer is any one or two of n-isopropylacrylamide, methacrylic acid, acrylic acid, acrylamide, and N,N-dimethylacrylamide; the solvent A is any one or two of water, N,N-dimethylformamide, N,N-dimethylacetamide, and dimethyl sulfoxide; the initiator is any one of α-ketoglutaric acid and azobisisobutyronitrile; the polysaccharide is any one or two of gelatin, carrageenan, gellan gum, chitosan, and sodium alginate.

[0014] In step 2, the polymerization reaction time is 1 h to 24 h, and the evaporation temperature is 10° C. to 100° C.

[0015] In step 3, solvent B is any one or two of water, formic acid, acetic acid, methanol, ethanol, acetone, N,N-dimethylformamide, N,N-dimethylacetamide, and dimethyl sulfoxide; and lignin is any one of acetic acid lignin, acetylated lignin, sulfate lignin, formic acid lignin, and dioxane lignin.

[0016] In step 4, the soaking time is 1 hour to 1 week; the calcium salt is any one of CaCO3, Ca(HCO3)2, CaSO4, CaCl2, and Ca(NO3)2.

[0017] Another technical solution adopted by the present invention is that the lignin-based polysaccharide sensing hydrogel with adjustable toughness and stiffness is prepared by the above method.

[0018] The beneficial effects of the present invention are:

[0019] The lignin-based polysaccharide sensing hydrogel with adjustable toughness and stiffness of the present invention is a double network hydrogel, in which lignin and polymer monomers are hydrophobically combined to form a first layer of network. By adjusting the type and proportion of polysaccharides and calcium salts, the cross-linking density of the second layer of network is adjusted to achieve high toughness, high rigidity and excellent sensing performance; the hydrogel has a tensile modulus of 6 to 12 MPa, a thermal conductivity of 50,000 to 100,000 J m -2 The tearing energy is 15~20MJ m -3 It has a tensile function and exhibits excellent strain sensitivity with a measurement factor (GF) of 1 to 10. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 is a tensile test diagram of the lignin-based polysaccharide hydrogel prepared in an embodiment of the present invention;

[0021] Figure 2 is a toughness test graph of the lignin-based polysaccharide hydrogel prepared in an embodiment of the present invention;

[0022] Figure 3 is a test graph of the elastic modulus of the lignin-based polysaccharide hydrogel prepared in the embodiment of the present invention;

[0023] Figure 4 This is a tearing energy test diagram of the lignin-based polysaccharide hydrogel prepared in the embodiment of the present invention;

[0024] Figure 5 It is a test graph of the measurement factor (GF) of the lignin-based polysaccharide hydrogel prepared in the example of the present invention. DETAILED DESCRIPTION

[0025] The present invention is described in detail below in conjunction with specific implementation modes and accompanying drawings.

[0026] The preparation method of the lignin-based polysaccharide sensing hydrogel with adjustable toughness and stiffness of the present invention is specifically implemented according to the following steps:

[0027] Step 1, mixing polymer monomers, polysaccharides and solvent A, stirring them thoroughly to make them uniformly mixed, and then adding an initiator to obtain a polymer monomer solution B;

[0028] The mass volume ratio of polymer monomer, initiator, polysaccharide and solvent A is 0.01g-10g: 0.001g-0.01g: 0.005g-2g: 5mL-15mL;

[0029] The stirring time is 10min~24h;

[0030] The polymer monomer is any one or two of n-isopropylacrylamide, methacrylic acid, acrylic acid, acrylamide, and N,N-dimethylacrylamide;

[0031] Solvent A is any one or two of water, N,N-dimethylformamide, N,N-dimethylacetamide, and dimethyl sulfoxide;

[0032] The initiator is any one of α-ketoglutaric acid and azobisisobutyronitrile;

[0033] The polysaccharide is any one or two of gelatin, carrageenan, gellan gum, chitosan and sodium alginate;

[0034] Step 2, subjecting the polymer monomer solution B to a free radical polymerization reaction under UV to obtain a polymer long chain solution, and then evaporating the polymer long chain solution to dryness to obtain a polymer solid C;

[0035] The polymerization reaction time is 1h to 24h, and the evaporation temperature is 10°C to 100°C;

[0036] Step 3, fully mixing the polymer solid C and the solvent B, then adding lignin, mixing completely and evaporating to dryness to obtain a lignin-based polysaccharide xerogel D;

[0037] Solvent B is any one or two of water, formic acid, acetic acid, methanol, ethanol, acetone, N,N-dimethylformamide, N,N-dimethylacetamide, and dimethyl sulfoxide;

[0038] The lignin is any one of acetic lignin, acetylated lignin, sulfate lignin, formic acid lignin, and dioxane lignin;

[0039] The amount of solvent B is 2 mL to 10 mL; the amount of lignin is 0.2 g to 8 g;

[0040] The mixing time is 10min to 12h; the evaporation temperature is 10℃ to 100℃;

[0041] Step 4, soaking the lignin-based polysaccharide dry gel D in a calcium salt solution to obtain a lignin-based polysaccharide sensing hydrogel with adjustable toughness and stiffness;

[0042] The soaking time is 1 hour to 1 week;

[0043] The calcium salt is any one of CaCO3, Ca(HCO3)2, CaSO4, CaCl2, and Ca(NO3)2.

[0044] The preparation method of the lignin-based polysaccharide sensing hydrogel with adjustable toughness and stiffness of the present invention adopts a solvent exchange method to prepare a double cross-linked polymer network hydrogel; wherein lignin and polymer monomers form a phase separation network, and then the pre-interpenetrating polysaccharide chains are fully swollen in a calcium salt solution. In this structure, the combination between lignin and polymer monomers stabilizes the lignin / polymer network, and the polysaccharide forms an ionic bond with the calcium salt to form a second network. The lignin-based polysaccharide hydrogel has both high tear energy toughness and high elastic modulus rigidity. In addition, due to the introduction of calcium salts and the narrowing of ion transmission channels during stretching, the lignin hydrogel exhibits excellent strain sensitivity.

[0045] Example 1

[0046] The preparation method of the lignin-based polysaccharide sensing hydrogel with adjustable toughness and stiffness of the present invention is specifically implemented according to the following steps:

[0047] Step 1, 0.52 g of methacrylic acid and 0.15 g of gelatin were added to 10 mL of N,N-dimethylacetamide at the same time, stirred on a magnetic stirrer for 10 min, and then 0.005 g of α-ketoglutaric acid was added after mixing to obtain a polymer monomer solution B;

[0048] Step 2, subjecting the obtained polymer monomer solution B to a free radical polymerization reaction under UV for 12 hours to obtain a polymer long-chain solution; evaporating the polymer long-chain solution to dryness at a drying temperature of 55° C. to obtain a polymer solid C;

[0049] Step 3, the polymer solid C was fully mixed with 5 mL of methanol for 10 min, and then 4.4 g of sulfate lignin was added, and the mixture was further fully mixed for 4 h and then evaporated to dryness at a temperature of 70° C. to obtain lignin-based polysaccharide xerogel D;

[0050] Step 4, soaking the lignin-based polysaccharide dry gel D in a CaSO4 solution for 2 days to obtain a lignin-based polysaccharide hydrogel; wherein the mass ratio of CaSO4 to gelatin is 1:25.

[0051] Example 2

[0052] The preparation method of the lignin-based polysaccharide sensing hydrogel with adjustable toughness and stiffness of the present invention is specifically implemented according to the following steps:

[0053] Step 1, 3.5 g acrylamide and 0.5 g chitosan were added to 8 mL N,N-dimethylformamide at the same time, and stirred on a magnetic stirrer for 4 h. After mixing evenly, 0.007 g α-ketoglutaric acid was added to obtain a polymer monomer solution B;

[0054] Step 2, subjecting the obtained polymer monomer solution B to a free radical polymerization reaction under UV for 15 hours to obtain a polymer long-chain solution; evaporating the polymer long-chain solution to dryness at a drying temperature of 65° C. to obtain a polymer solid C;

[0055] Step 3, the polymer solid C was fully mixed with 7 mL of acetone for 6 h, and then 4 g of acetic lignin was added, and the mixture was further fully mixed for 2 h and then evaporated to dryness at a temperature of 55° C. to obtain a lignin-based polysaccharide dry gel D;

[0056] Step 4, soaking the lignin-based polysaccharide dry gel D in a CaCO3 solution for 3 days to obtain a lignin-based polysaccharide hydrogel; wherein the mass ratio of CaCO3 to chitosan is 1:50.

[0057] Example 3

[0058] The preparation method of the lignin-based polysaccharide sensing hydrogel with adjustable toughness and stiffness of the present invention is specifically implemented according to the following steps:

[0059] Step 1, 5 g of N,N-dimethylacrylamide and 0.75 g of gellan gum were added to 12 mL of water at the same time, and the mixture was stirred on a magnetic stirrer for 3 h. After the mixture was evenly mixed, 0.008 g of azobisisobutyronitrile was added to obtain a polymer monomer solution B;

[0060] Step 2, subjecting the obtained polymer monomer solution B to a free radical polymerization reaction under UV for 16 hours to obtain a polymer long-chain solution; evaporating the polymer long-chain solution to dryness at a drying temperature of 65° C. to obtain a polymer solid C;

[0061] Step 3, the polymer solid C was fully mixed with 7 mL of dimethyl sulfoxide for 1 hour, and then acetylated lignin was added, and the mixture was further fully mixed for 10 hours and then evaporated to dryness at a temperature of 65° C. to obtain lignin-based polysaccharide xerogel D;

[0062] Step 4, soaking the lignin-based polysaccharide dry gel D in a CaCl2 solution for 3 days to obtain a lignin-based polysaccharide hydrogel; wherein the mass ratio of CaCl2 to gellan gum is 1:50.

[0063] Example 4

[0064] The preparation method of the lignin-based polysaccharide sensing hydrogel with adjustable toughness and stiffness of the present invention is specifically implemented according to the following steps:

[0065] Step 1, 2.8 g of N-isopropylacrylamide and 1.6 g of sodium alginate were added to 12 mL of dimethyl sulfoxide at the same time, and the mixture was stirred on a magnetic stirrer for 9 h. After the mixture was evenly mixed, 0.002 g of α-ketoglutaric acid was added to obtain a polymer monomer solution B;

[0066] Step 2, subjecting the obtained polymer monomer solution B to a free radical polymerization reaction under UV for 16 hours to obtain a polymer long-chain solution; evaporating the polymer long-chain solution to dryness at a drying temperature of 45° C. to obtain a polymer solid C;

[0067] Step 3, the polymer solid C was fully mixed with 6 mL of acetic acid for 1 hour, and then 4.8 g of formic acid lignin was added, and the mixture was further fully mixed for 6.5 hours and then evaporated to dryness at a temperature of 60° C. to obtain lignin-based polysaccharide xerogel D;

[0068] Step 4, soaking the lignin-based polysaccharide dry gel D in a Ca(NO3)2 solution for 3 days to obtain a lignin-based polysaccharide hydrogel; wherein the mass ratio of Ca(NO3)2 to sodium alginate is 1:75.

[0069] Example 5

[0070] The preparation method of the lignin-based polysaccharide sensing hydrogel with adjustable toughness and stiffness of the present invention is specifically implemented according to the following steps:

[0071] Step 1, 6.8 g of acrylic acid and 0.8 g of carrageenan are added to 10 ml of dimethyl sulfoxide at the same time, and stirred on a magnetic stirrer for 14 hours. After mixing evenly, 0.005 g of azobisisobutyronitrile is added to obtain a polymer monomer solution B;

[0072] Step 2, subjecting the obtained polymer monomer solution B to a free radical polymerization reaction under UV for 18 hours to obtain a polymer long-chain solution; evaporating the polymer long-chain solution to dryness at a drying temperature of 65° C. to obtain a polymer solid C;

[0073] Step 3, the polymer solid C was fully mixed with 5 ml of acetone for 1 hour, and then 7.2 g of formic acid lignin was added, and the mixture was further fully mixed for 1.5 hours and then evaporated to dryness at a temperature of 50° C. to obtain lignin-based polysaccharide xerogel D;

[0074] Step 4, soaking the lignin-based polysaccharide dry gel D in a CaCl2 solution for 4 days to obtain a lignin-based polysaccharide hydrogel; wherein the mass ratio of CaCl2 to carrageenan is 1:50.

[0075] Example 6

[0076] The preparation method of the lignin-based polysaccharide sensing hydrogel with adjustable toughness and stiffness of the present invention is specifically implemented according to the following steps:

[0077] Step 1, 5.8 g of N,N-dimethylacrylamide and 1.8 g of gelatin were added to 12 ml of water at the same time, and the mixture was stirred on a magnetic stirrer for 5 h. After the mixture was evenly mixed, 0.006 g of α-ketoglutaric acid was added to obtain a polymer monomer solution B;

[0078] Step 2, subjecting the obtained polymer monomer solution B to a free radical polymerization reaction under UV for 10 hours to obtain a polymer long-chain solution; evaporating the polymer long-chain solution to dryness at a drying temperature of 65° C. to obtain a polymer solid C;

[0079] Step 3, the polymer solid C was fully mixed with 8 ml of N,N-dimethylformamide for 2 hours, and then 6.6 g of formic acid lignin was added, and the mixture was further fully mixed for 1 hour and then evaporated to dryness at a temperature of 45° C. to obtain lignin-based polysaccharide xerogel D;

[0080] Step 4, soaking the lignin-based polysaccharide dry gel D in a CaSO4 solution for 4 days to obtain a lignin-based polysaccharide hydrogel; wherein the mass ratio of CaSO4 to gelatin is 1:100.

[0081] Figure 1 is a tensile test curve of the lignin-based polysaccharide hydrogel prepared in the embodiment of the present invention; Figure 1 It can be seen that the stress of the hydrogel in the embodiment is between 1 and 4 MPa, and the strain is between 700% and 1500%, and has good mechanical properties; Figure 2 is a bar graph of the toughness of the lignin-based polysaccharide hydrogel prepared in the embodiment of the present invention; Figure 2 It can be seen that the hydrogel in the embodiment has a relatively large toughness, ranging from 15 to 20 MJm -3 between; Figure 3 is a test graph of the elastic modulus of the lignin-based polysaccharide hydrogel prepared in the embodiment of the present invention; Figure 3 It can be seen that the elastic modulus of the hydrogel in the embodiment is between 5 and 8 MPa; Figure 4 is a tearing energy test diagram of the lignin-based polysaccharide hydrogel prepared in the embodiment of the present invention. Figure 4 It can be seen that the tearing energy of the hydrogel in the embodiment is between 60000 and 100000 Jm -2 between; Figure 5 is a test graph of the measurement factor (GF) of the lignin-based polysaccharide hydrogel prepared in the embodiment of the present invention, from Figure 5 It can be seen that the measurement factor (GF) of the hydrogel in the embodiment is between 6 and 8;

[0082] According to the above performance test results, the lignin-based polysaccharide sensing hydrogel of the present invention has both high tear energy toughness and high elastic modulus rigidity.

Claims

1. A method for preparing a lignin-based polysaccharide sensing hydrogel with adjustable toughness and stiffness, characterized in that: Follow the steps below to implement it: Step 1, mixing polymer monomers, polysaccharides and solvent A, stirring them thoroughly to make them uniformly mixed, and then adding an initiator to obtain a polymer monomer solution B; Step 2, subjecting the polymer monomer solution B to a free radical polymerization reaction under UV to obtain a polymer long chain solution, which is evaporated to dryness to obtain a polymer solid C; Step 3, fully mixing the polymer solid C and the solvent B, then adding lignin, mixing completely and evaporating to dryness, to obtain a lignin-based polysaccharide xerogel D; Step 4, soaking the lignin-based polysaccharide dry gel D in a calcium salt solution to obtain a lignin-based polysaccharide sensing hydrogel with adjustable toughness and stiffness.

2. The method for preparing the lignin-based polysaccharide sensing hydrogel with adjustable toughness and stiffness as claimed in claim 1, characterized in that: In the step 1, the mass volume ratio of the polymer monomer, the initiator, the polysaccharide and the solvent A is 0.01-10: 0.001-0.01: 0.005-2: 5-15.

3. The method for preparing the lignin-based polysaccharide sensing hydrogel with adjustable toughness and stiffness as claimed in claim 1, characterized in that: In the step 1, the polymer monomer is any one or two of n-isopropylacrylamide, methacrylic acid, acrylic acid, acrylamide, and N,N-dimethylacrylamide; the solvent A is any one or two of water, N,N-dimethylformamide, N,N-dimethylacetamide, and dimethyl sulfoxide; the initiator is any one of α-ketoglutaric acid and azobisisobutyronitrile; and the polysaccharide is any one or two of gelatin, carrageenan, gellan gum, chitosan, and sodium alginate.

4. The method for preparing the lignin-based polysaccharide sensing hydrogel with adjustable toughness and stiffness as claimed in claim 1, characterized in that: In the step 2, the polymerization reaction time is 1 h to 24 h, and the evaporation temperature is 10° C. to 100° C.

5. The method for preparing the lignin-based polysaccharide sensing hydrogel with adjustable toughness and stiffness as claimed in claim 1, characterized in that: In the step 3, the solvent B is any one or two of water, formic acid, acetic acid, methanol, ethanol, acetone, N,N-dimethylformamide, N,N-dimethylacetamide, and dimethyl sulfoxide; and the lignin is any one of acetic lignin, acetylated lignin, sulfate lignin, formic acid lignin, and dioxane lignin.

6. The method for preparing the lignin-based polysaccharide sensing hydrogel with adjustable toughness and stiffness as claimed in claim 1, characterized in that: In step 4, the soaking time is 1 hour to 1 week; the calcium salt is any one of CaCO3, Ca(HCO3)2, CaSO4, CaCl2, and Ca(NO3)2.

7. Lignin-based polysaccharide sensing hydrogel with adjustable toughness and stiffness, characterized in that: The method is prepared by any one of claims 1 to 6.

Citation Information

Patent Citations

  • Method for preparing high-strength lignin hydrogel with adjustable mechanical properties

    CN110092921A

  • Method for preparing high-strength high-toughness gelatin-based hydrogel

    CN110157012A

  • Telescopic anti-freezing full-physical crosslinked hydrogel material for multi-mode flexible sensor and preparation method thereof

    CN111548513A

  • Full-biomass sodium alginate / lignin water-retaining slow-release hydrogel as well as preparation method and application thereof

    CN117624647A