Polyethylene modified foamed cotton and preparation method thereof
By introducing flame-retardant modified aerogels and composite metal oxides into polyethylene foam, the problem of insufficient insulation and flame retardant performance of traditional polyethylene foam is solved, and its insulation and flame retardant properties are significantly improved. and heat resistance.
Patent Information
- Application Number
- CN202411232049.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional polyethylene foam has poor performance in the field of thermal insulation, high thermal conductivity and poor flame retardant performance, which poses a fire safety hazard.
By depositing composite metal oxides on the surface of silica aerogel and reacting with phosphorus oxychloride and DOPO, it is added to low-density polyethylene, with ethylene-vinyl acetate copolymer, ethylene-acrylic acid copolymer, sensitizer, Polyethylene wax is mixed, radiation cross-linked foaming is performed to prepare polyethylene modified foam with flame retardant modified aerogel.
It significantly improves the thermal insulation, flame retardant and heat resistance of polyethylene modified foam, reduces the flame spreading speed, reduces the generation of toxic smoke, and enhances the mechanical properties and economic durability of the material.
Smart Images

Figure BDA0005026471850000181
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyethylene, and in particular to polyethylene modified foamed cotton and a preparation method thereof. Background Art
[0002] Polyethylene foam is a non-cross-linked closed-cell structure, also known as EPE pearl cotton, which is a new type of environmentally friendly packaging material. It is composed of countless independent bubbles produced by physical foaming of low-density polyethylene. It overcomes the shortcomings of ordinary foam rubber, such as fragility, deformation, and poor recovery. It has many advantages such as waterproof and moisture-proof, shockproof, sound insulation, heat preservation, strong toughness, recycling, environmental protection, and strong impact resistance. It also has good chemical resistance and is an ideal substitute for traditional packaging materials.
[0003] However, there are still some problems in the application of traditional polyethylene foam in the field of thermal insulation. On the one hand, the bubble structure obtained by physical foaming of low-density polyethylene is a non-cross-linked closed-cell structure with a size in the micron range, which is larger than the mean free path of air molecules, so the heat transfer inhibition effect on gas molecules is not ideal. Therefore, the thermal insulation effect of polyethylene foam is not ideal and the thermal conductivity is high (the thermal conductivity at room temperature is about 0.041W / m·K). On the other hand, the component of polyethylene foam is organic polyethylene. When used as a thermal insulation material, it has poor flame retardant properties. As long as it encounters a fire source, it is easy to burn, posing a huge threat and harm to people's lives. If it is possible to prepare a polyethylene foam material with extremely low thermal conductivity, good thermal insulation effect, good mechanical properties, certain flame retardancy, and economic and durable properties, the above problems will be solved to a large extent. Summary of the invention
[0004] The purpose of the present invention is to provide a polyethylene modified foam cotton and a preparation method thereof. The preparation method is simple and the raw material source is wide. The prepared polyethylene modified foam cotton has good mechanical properties, good resilience, good thermal insulation and flame retardant properties, good temperature and heat resistance, is economical and durable, and has broad application prospects.
[0005] The technical solution of the present invention is achieved in this way:
[0006] The invention provides a preparation method of polyethylene modified foamed cotton, comprising the steps of depositing composite metal oxide on the surface of silicon dioxide aerogel, modifying the surface with a silane coupling agent, reacting with phosphorus oxychloride and DOPO in sequence, adding the aerogel into low-density polyethylene, mixing with ethylene-vinyl acetate copolymer, ethylene-acrylic acid copolymer, a sensitizer and polyethylene wax, refining the mixture, adding a foaming agent, plasticizing, sheeting, radiation crosslinking, foaming and cooling to obtain the polyethylene modified foamed cotton.
[0007] As a further improvement of the present invention, the following steps are included:
[0008] S1. Preparation of silica aerogel: alkyl orthosilicate, ethanol and water were mixed uniformly, the pH value of the solution was adjusted to be alkaline, stirred to form a gel, ethanol was added for aging, and dried to obtain silica aerogel;
[0009] S2. Deposition of composite metal oxides: dissolving silica aerogel, magnesium nitrate and aluminum nitrate in water, adding alkali solution, heating and crystallizing the deposited silica aerogel, filtering, washing, drying and calcining to obtain composite metal oxide deposited silica aerogel;
[0010] S3. Modification: adding the composite metal oxide deposited silica aerogel to ethanol, adding a composite silane coupling agent, heating and stirring the reaction, centrifuging, washing, and drying to obtain a modified aerogel;
[0011] S4. Reaction with phosphorus oxychloride: adding the modified aerogel to acetonitrile, adding a catalyst, stirring and mixing, adding phosphorus oxychloride, heating to reflux and stirring the reaction, centrifuging, washing, and drying to obtain a primary flame-retardant modified aerogel;
[0012] S5. Reaction with DOPO: adding the primary flame retardant modified aerogel and DOPO to toluene, heating under reflux and stirring for reaction, centrifuging, washing, and drying to obtain a flame retardant modified aerogel;
[0013] S6. Preparation of polyethylene modified foam cotton: melt low-density polyethylene, add ethylene-vinyl acetate copolymer and ethylene-acrylic acid copolymer, stir and mix evenly, add sensitizer, butyl stearate, polyethylene wax and flame retardant modified aerogel and start refining, then add foaming agent, plasticize, sheet out, radiate cross-linking, foam, cool, and obtain polyethylene modified foam cotton.
[0014] As a further improvement of the present invention, in step S1, the mass ratio of alkyl orthosilicate, ethanol and water is 15-20:110-130:40-60, the pH value of the adjusted solution is 9.5-10.5, and the aging time is 24-28 hours.
[0015] As a further improvement of the present invention, the mass ratio of the silica aerogel, magnesium nitrate and aluminum nitrate in step S2 is 100:10-12:12-15, the alkali solution is ammonia water, the temperature of the heated deposition crystallization is 85-95°C, the time is 20-40min, and the calcination temperature is 600-700°C, and the time is 2-4h.
[0016] As a further improvement of the present invention, in step S3, the mass ratio of the composite metal oxide deposited silica aerogel and the composite silane coupling agent is 10:1-2, the composite silane coupling agent is a mixture of KH560 and KH570, the mass ratio is 3-5:10, the temperature of the heating and stirring reaction is 40-50°C, and the time is 1-3h.
[0017] As a further improvement of the present invention, in step S4, the mass ratio of the modified aerogel, the catalyst and phosphorus oxychloride is 10:0.01-0.015:1-2, the time of the heating reflux stirring reaction is 1-2h, and the catalyst is TiCl4.
[0018] As a further improvement of the present invention, in step S5, the mass ratio of the primary flame retardant modified aerogel to DOPO is 10:3-4, and the heating reflux stirring reaction is performed for 2-4 hours.
[0019] As a further improvement of the present invention, the mass ratio of the low-density polyethylene, ethylene-vinyl acetate copolymer, ethylene-acrylic acid copolymer, sensitizer, butyl stearate, polyethylene wax, flame retardant modified aerogel, and foaming agent in step S6 is 100:7-9:3-5:1-2:3-5:1-3:7-10:12-17, the radiation crosslinking is an absorbed dose of 75-95 kGy radiation crosslinking for 4-7 minutes, the foaming temperature is 180-200°C, the time is 7-10 minutes, the sensitizer is a mixture of zinc stearate and ZnO in a mass ratio of 1:3-5, and the foaming agent is azodicarbonamide.
[0020] As a further improvement of the present invention, the present invention specifically comprises the following steps:
[0021] S1. Preparation of silica aerogel: 15-20 parts by weight of alkyl orthosilicate, 110-130 parts by weight of ethanol and 40-60 parts by weight of water were mixed uniformly, the pH value of the solution was adjusted to 9.5-10.5, stirred to form a gel, 100-200 parts by weight of ethanol was added, aged for 24-28h, dried, and ball-milled for 1h to obtain silica aerogel;
[0022] S2. Deposition of composite metal oxides: 100 parts by weight of silica aerogel, 10-12 parts by weight of magnesium nitrate, and 12-15 parts by weight of aluminum nitrate were dissolved in water, and aqueous ammonia was added dropwise until the solution had a pH value of 8.5-9.5, heated to 85-95°C, deposited and crystallized for 20-40min, filtered, washed, dried, and calcined at 600-700°C for 2-4h to obtain composite metal oxide deposited silica aerogel;
[0023] S3. Modification: 10 parts by weight of composite metal oxide deposited silica aerogel was added to ethanol, 1-2 parts by weight of composite silane coupling agent was added, heated to 40-50°C, stirred for 1-3h, centrifuged, washed, and dried to obtain a modified aerogel;
[0024] The composite silane coupling agent is a mixture of KH560 and KH570, with a mass ratio of 3-5:10;
[0025] S4 reaction with phosphorus oxychloride: 10 parts by weight of the modified aerogel was added to acetonitrile, 0.01-0.015 parts by weight of the catalyst TiCl4 was added, stirred and mixed, 1-2 parts by weight of phosphorus oxychloride was added, the reaction was heated to reflux with stirring for 1-2h, centrifuged, washed, and dried to obtain a primary flame-retardant modified aerogel;
[0026] S5. Reaction with DOPO: 10 parts by weight of primary flame retardant modified aerogel and 3-4 parts by weight of DOPO were added to toluene, heated to reflux with stirring for 2-4h, centrifuged, washed, and dried to obtain a flame retardant modified aerogel;
[0027] S6. Preparation of polyethylene modified foam cotton: 100 parts by weight of low-density polyethylene is heated to 110-115°C and melted for 2-4 minutes, 7-9 parts by weight of ethylene-vinyl acetate copolymer and 3-5 parts by weight of ethylene-acrylic acid copolymer are added and melted, stirred and mixed for 1-3 minutes, 1-2 parts by weight of sensitizer, 3-5 parts by weight of butyl stearate, 1-3 parts by weight of polyethylene wax and 7-10 parts by weight of flame retardant modified aerogel are added and melted for 1-3 minutes, and then 12-17 parts by weight of foaming agent are added, and the mixture is plasticized for 2-4 minutes by repeatedly beating the triangle, and the sheet is produced, and the sheet is melted on a flat vulcanizer at 110-115°C at a pressure of 12-15MPa for 4-6 minutes, and then the pressure is released, and the sheet is cooled and molded at 10MPa. The absorbed dose is 75-95kGy for radiation cross-linking for 4-7 minutes, and the sheet is foamed at 180-200°C for 7-10 minutes, and then cooled to obtain polyethylene modified foam cotton;
[0028] The sensitizer is a mixture of zinc stearate and ZnO, with a mass ratio of 1:3-5.
[0029] The present invention further protects a polyethylene modified foamed cotton prepared by the above preparation method.
[0030] The present invention has the following beneficial effects:
[0031] The present invention prepares a polyethylene modified foam cotton partially filled with flame retardant modified aerogel and butyl stearate. On the one hand, through radiation cross-linking, the pore structure of the polyethylene modified foam cotton can be refined to improve the thermal insulation performance of the foam cotton. At the same time, the filled butyl stearate is a better phase change material, and a composite fixed phase change material is generated in situ, which further enhances the thermal insulation performance of the material, improves the resilience of the material, and reduces permanent deformation.
[0032] On the other hand, by adding flame-retardant modified aerogel, the microporous structure of aerogel can also improve the thermal insulation performance of foam. At the same time, the composite magnesium oxide and aluminum oxide are deposited on the surface of silica aerogel by co-precipitation. Magnesium oxide has high fire-resistant insulation performance and can be transformed into a crystalline form after high-temperature burning. At higher temperatures, magnesium oxide can become magnesia or sintered magnesium oxide, which further enhances its fire resistance. Alumina decomposes at high temperatures to produce aluminum oxide smoke, forming a flame-retardant layer, which plays a role in isolating air and burning substances. The coordinated effect of the two improves the flame retardancy and temperature resistance of the material.
[0033] However, the flame retardant effect of the prepared composite metal oxide deposited silica aerogel directly added to polyethylene foam is not very perfect. Therefore, the inventors carried out further modification treatment, and after surface modification of the silane coupling agent KH570 with double bonds and the silane coupling agent KH560 with epoxy groups, the epoxy group-containing part was first reacted and connected with phosphorus oxychloride in the presence of a catalyst, and then the double bond-containing part was reacted and connected with DOPO (9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide), so that it has a phosphorus-based flame retardant, has high-efficiency flame retardant properties, can effectively inhibit the spread of flames, slow down the burning speed, and reduce the generation of toxic smoke in fire accidents, greatly improving the flame retardant properties of the prepared polyethylene foam.
[0034] The polyethylene modified foamed cotton prepared by the invention has a simple preparation method and a wide source of raw materials. The prepared polyethylene modified foamed cotton has good mechanical properties, good resilience, good thermal insulation and flame retardancy, good temperature and heat resistance, is economical and durable, and has broad application prospects. DETAILED DESCRIPTION
[0035] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0036] Low-density polyethylene, brand 2426H, was purchased from Sinopec Maoming Branch.
[0037] Example 1
[0038] This embodiment provides a method for preparing polyethylene modified foam cotton, which specifically comprises the following steps:
[0039] S1. Preparation of silica aerogel: 15 g of methyl orthosilicate, 110 g of ethanol and 40 mL of water were mixed, the pH value of the solution was adjusted to 9.5, stirred to form a gel, 100 g of ethanol was added, aged for 24 h, dried, and ball-milled for 1 h to obtain silica aerogel;
[0040] S2. Deposition of composite metal oxides: 100 g of silica aerogel, 10 g of magnesium nitrate, and 12 g of aluminum nitrate were added to 500 mL of water, and aqueous ammonia was added dropwise until the solution had a pH value of 8.5, heated to 85 ° C, deposited and crystallized for 20 min, filtered, washed, dried, and calcined at 600 ° C for 2 h to obtain composite metal oxide deposited silica aerogel;
[0041] S3. Modification: 10 g of composite metal oxide deposited silica aerogel was added to 200 mL of ethanol, 1 g of composite silane coupling agent was added, heated to 40 ° C, stirred for 1 h, centrifuged, washed, and dried to obtain a modified aerogel;
[0042] The composite silane coupling agent is a mixture of KH560 and KH570, with a mass ratio of 3:10;
[0043] S4 reaction with phosphorus oxychloride: 10g of the modified aerogel was added to 200mL of acetonitrile, 0.01g of the catalyst TiCl4 was added, the mixture was stirred and mixed, 1g of phosphorus oxychloride was added, the reaction was heated to reflux with stirring for 1h, centrifuged, washed, and dried to obtain a primary flame-retardant modified aerogel;
[0044] S5. Reaction with DOPO: 10 g of primary flame retardant modified aerogel and 3 g of DOPO were added to 200 mL of toluene, heated under reflux and stirred for reaction for 2 h, centrifuged, washed, and dried to obtain flame retardant modified aerogel;
[0045] S6. Preparation of polyethylene modified foam cotton: 100g low-density polyethylene was heated to 110°C and melted for 2min, 7g ethylene-vinyl acetate copolymer and 3g ethylene-acrylic acid copolymer were added and melted, stirred and mixed for 1min, 1g sensitizer, 3g butyl stearate, 1g polyethylene wax and 7g flame retardant modified aerogel were added and melted for 1min, and then 12g azodicarbonamide was added, and the mixture was plasticized for 2min by repeatedly beating the triangle, and the sheet was produced. After pressurizing to 12MPa on a flat vulcanizer at 110°C for 4min, the pressure was released, and the temperature was maintained at 10MPa for cooling and molding. The absorbed dose was 75kGy for radiation cross-linking for 4min, and the mixture was foamed at 180°C for 7min, and cooled to obtain polyethylene modified foam cotton;
[0046] The sensitizer is a mixture of zinc stearate and ZnO, with a mass ratio of 1:3.
[0047] Example 2
[0048] This embodiment provides a method for preparing polyethylene modified foam cotton, which specifically comprises the following steps:
[0049] S1. Preparation of silica aerogel: 20 g of tetraethyl orthosilicate, 130 g of ethanol and 60 mL of water were mixed evenly, the pH value of the solution was adjusted to 10.5, stirred to form a gel, 200 g of ethanol was added, aged for 28 h, dried, and ball-milled for 1 h to obtain silica aerogel;
[0050] S2. Deposition of composite metal oxides: 100 g of silica aerogel, 12 g of magnesium nitrate, and 15 g of aluminum nitrate were added to 500 mL of water, and aqueous ammonia was added dropwise until the solution had a pH value of 9.5, heated to 95 ° C, deposited and crystallized for 40 min, filtered, washed, dried, and calcined at 700 ° C for 4 h to obtain composite metal oxide deposited silica aerogel;
[0051] S3. Modification: 10 g of composite metal oxide deposited silica aerogel was added to 200 mL of ethanol, 2 g of composite silane coupling agent was added, heated to 50 ° C, stirred for 3 h, centrifuged, washed, and dried to obtain a modified aerogel;
[0052] The composite silane coupling agent is a mixture of KH560 and KH570, with a mass ratio of 5:10;
[0053] S4 reaction with phosphorus oxychloride: 10g of the modified aerogel was added to 200mL of acetonitrile, 0.015g of the catalyst TiCl4 was added, the mixture was stirred and mixed, 2g of phosphorus oxychloride was added, the reaction was heated to reflux with stirring for 2h, centrifuged, washed, and dried to obtain a primary flame-retardant modified aerogel;
[0054] S5. Reaction with DOPO: 10 g of primary flame retardant modified aerogel and 4 g of DOPO were added to 200 mL of toluene, heated under reflux and stirred for 4 h, centrifuged, washed, and dried to obtain flame retardant modified aerogel;
[0055] S6. Preparation of polyethylene modified foam cotton: 100g of low-density polyethylene was heated to 115°C and melted for 4min, 9g of ethylene-vinyl acetate copolymer and 5g of ethylene-acrylic acid copolymer were added and melted, stirred and mixed for 3min, 2g of sensitizer, 5g of butyl stearate, 3g of polyethylene wax and 10g of flame-retardant modified aerogel were added and melted for 3min, and then 17g of azodicarbonamide was added, and the mixture was plasticized for 4min by repeatedly beating the triangle, and the sheet was produced. After pressurizing to 15MPa on a flat vulcanizer at 115°C for 6min, the pressure was released, and the temperature was maintained at 10MPa for cooling and molding. The absorbed dose was 95kGy for radiation cross-linking for 7min, foaming at 200°C for 10min, and cooling was performed to obtain polyethylene modified foam cotton;
[0056] The sensitizer is a mixture of zinc stearate and ZnO, with a mass ratio of 1:5.
[0057] Example 3
[0058] This embodiment provides a method for preparing polyethylene modified foam cotton, which specifically comprises the following steps:
[0059] S1. Preparation of silica aerogel: 17 g of tetraethyl orthosilicate, 120 g of ethanol and 50 mL of water were mixed, the pH value of the solution was adjusted to 10, stirred to form a gel, 150 g of ethanol was added, aged for 26 h, dried, and ball-milled for 1 h to obtain silica aerogel;
[0060] S2. Deposition of composite metal oxides: 100 g of silica aerogel, 11 g of magnesium nitrate, and 13 g of aluminum nitrate were added to 500 mL of water, and aqueous ammonia was added dropwise until the pH value of the solution was 9, heated to 90 ° C, deposited and crystallized for 30 min, filtered, washed, dried, and calcined at 650 ° C for 3 h to obtain composite metal oxide deposited silica aerogel;
[0061] S3. Modification: 10 g of composite metal oxide deposited silica aerogel was added to 200 mL of ethanol, 1.5 g of composite silane coupling agent was added, heated to 45 ° C, stirred for 2 h, centrifuged, washed, and dried to obtain a modified aerogel;
[0062] The composite silane coupling agent is a mixture of KH560 and KH570, with a mass ratio of 4:10;
[0063] S4 reaction with phosphorus oxychloride: 10g of the modified aerogel was added to 200mL of acetonitrile, 0.012g of the catalyst TiCl4 was added, the mixture was stirred and mixed, 1.5g of phosphorus oxychloride was added, the reaction was heated to reflux with stirring for 1.5h, centrifuged, washed, and dried to obtain a primary flame-retardant modified aerogel;
[0064] S5. Reaction with DOPO: 10 g of primary flame retardant modified aerogel and 3.5 g of DOPO were added to 200 mL of toluene, heated under reflux and stirred for 3 h, centrifuged, washed, and dried to obtain flame retardant modified aerogel;
[0065] S6. Preparation of polyethylene modified foam cotton: 100g of low-density polyethylene was heated to 112°C and melted for 3min, 8g of ethylene-vinyl acetate copolymer and 4g of ethylene-acrylic acid copolymer were added and melted, stirred and mixed for 2min, 1.5g of sensitizer, 4g of butyl stearate, 3g of polyethylene wax and 8g of flame-retardant modified aerogel were added and melted for 2min, and then 15g of azodicarbonamide was added, and the mixture was plasticized for 3min by repeatedly beating the triangle, and the sheet was produced. After pressurizing to 13MPa on a flat vulcanizer at 112°C for 5min, the pressure was released, and the temperature was maintained at 10MPa for cooling and molding. The absorbed dose was 85kGy for radiation cross-linking for 5min, and the mixture was foamed at 190°C for 8min, and cooled to obtain polyethylene modified foam cotton;
[0066] The sensitizer is a mixture of zinc stearate and ZnO, with a mass ratio of 1:4.
[0067] Comparative Example 1
[0068] Compared with Example 3, the difference is that magnesium nitrate is not added in step S2.
[0069] The details are as follows:
[0070] S1. Preparation of silica aerogel: 17 g of tetraethyl orthosilicate, 120 g of ethanol and 50 mL of water were mixed, the pH value of the solution was adjusted to 10, stirred to form a gel, 150 g of ethanol was added, aged for 26 h, dried, and ball-milled for 1 h to obtain silica aerogel;
[0071] S2. Deposition of metal oxides: 100 g of silica aerogel and 24 g of aluminum nitrate were added to 500 mL of water, aqueous ammonia was added dropwise until the pH value of the solution was 9, heated to 90 ° C, deposited and crystallized for 30 min, filtered, washed, dried, and calcined at 650 ° C for 3 h to obtain metal oxide-deposited silica aerogel;
[0072] S3. Modification: 10 g of metal oxide-precipitated silica aerogel was added to 200 mL of ethanol, 1.5 g of a composite silane coupling agent was added, the mixture was heated to 45 ° C, stirred for 2 h, centrifuged, washed, and dried to obtain a modified aerogel;
[0073] The composite silane coupling agent is a mixture of KH560 and KH570, with a mass ratio of 4:10;
[0074] S4 reaction with phosphorus oxychloride: 10g of the modified aerogel was added to 200mL of acetonitrile, 0.012g of the catalyst TiCl4 was added, the mixture was stirred and mixed, 1.5g of phosphorus oxychloride was added, the reaction was heated to reflux with stirring for 1.5h, centrifuged, washed, and dried to obtain a primary flame-retardant modified aerogel;
[0075] S5. Reaction with DOPO: 10 g of primary flame retardant modified aerogel and 3.5 g of DOPO were added to 200 mL of toluene, heated under reflux and stirred for 3 h, centrifuged, washed, and dried to obtain flame retardant modified aerogel;
[0076] S6. Preparation of polyethylene modified foam cotton: 100g of low-density polyethylene was heated to 112°C and melted for 3min, 8g of ethylene-vinyl acetate copolymer and 4g of ethylene-acrylic acid copolymer were added and melted, stirred and mixed for 2min, 1.5g of sensitizer, 4g of butyl stearate, 3g of polyethylene wax and 8g of flame-retardant modified aerogel were added and melted for 2min, and then 15g of azodicarbonamide was added, and the mixture was plasticized for 3min by repeatedly beating the triangle, and the sheet was produced. After pressurizing to 13MPa on a flat vulcanizer at 112°C for 5min, the pressure was released, and the temperature was maintained at 10MPa for cooling and molding. The absorbed dose was 85kGy for radiation cross-linking for 5min, and the mixture was foamed at 190°C for 8min, and cooled to obtain polyethylene modified foam cotton;
[0077] The sensitizer is a mixture of zinc stearate and ZnO, with a mass ratio of 1:4.
[0078] Comparative Example 2
[0079] Compared with Example 3, the difference is that aluminum nitrate is not added in step S2.
[0080] The details are as follows:
[0081] S1. Preparation of silica aerogel: 17 g of tetraethyl orthosilicate, 120 g of ethanol and 50 mL of water were mixed, the pH value of the solution was adjusted to 10, stirred to form a gel, 150 g of ethanol was added, aged for 26 h, dried, and ball-milled for 1 h to obtain silica aerogel;
[0082] S2. Deposition of metal oxides: 100 g of silica aerogel and 24 g of magnesium nitrate were added to 500 mL of water, and aqueous ammonia was added dropwise until the pH value of the solution was 9, heated to 90 ° C, deposited and crystallized for 30 min, filtered, washed, dried, and calcined at 650 ° C for 3 h to obtain metal oxide-deposited silica aerogel;
[0083] S3. Modification: 10 g of metal oxide-precipitated silica aerogel was added to 200 mL of ethanol, 1.5 g of a composite silane coupling agent was added, the mixture was heated to 45 ° C, stirred for 2 h, centrifuged, washed, and dried to obtain a modified aerogel;
[0084] The composite silane coupling agent is a mixture of KH560 and KH570, with a mass ratio of 4:10;
[0085] S4 reaction with phosphorus oxychloride: 10g of the modified aerogel was added to 200mL of acetonitrile, 0.012g of the catalyst TiCl4 was added, the mixture was stirred and mixed, 1.5g of phosphorus oxychloride was added, the reaction was heated to reflux with stirring for 1.5h, centrifuged, washed, and dried to obtain a primary flame-retardant modified aerogel;
[0086] S5. Reaction with DOPO: 10 g of primary flame retardant modified aerogel and 3.5 g of DOPO were added to 200 mL of toluene, heated under reflux and stirred for 3 h, centrifuged, washed, and dried to obtain flame retardant modified aerogel;
[0087] S6. Preparation of polyethylene modified foam cotton: 100g of low-density polyethylene was heated to 112°C and melted for 3min, 8g of ethylene-vinyl acetate copolymer and 4g of ethylene-acrylic acid copolymer were added and melted, stirred and mixed for 2min, 1.5g of sensitizer, 4g of butyl stearate, 3g of polyethylene wax and 8g of flame-retardant modified aerogel were added and melted for 2min, and then 15g of azodicarbonamide was added, and the mixture was plasticized for 3min by repeatedly beating the triangle, and the sheet was produced. After pressurizing to 13MPa on a flat vulcanizer at 112°C for 5min, the pressure was released, and the temperature was maintained at 10MPa for cooling and molding. The absorbed dose was 85kGy for radiation cross-linking for 5min, and the mixture was foamed at 190°C for 8min, and cooled to obtain polyethylene modified foam cotton;
[0088] The sensitizer is a mixture of zinc stearate and ZnO, with a mass ratio of 1:4.
[0089] Comparative Example 3
[0090] Compared with Example 3, the difference is that step S2 is not performed.
[0091] The details are as follows:
[0092] S1. Preparation of silica aerogel: 17 g of tetraethyl orthosilicate, 120 g of ethanol and 50 mL of water were mixed, the pH value of the solution was adjusted to 10, stirred to form a gel, 150 g of ethanol was added, aged for 26 h, dried, and ball-milled for 1 h to obtain silica aerogel;
[0093] S2. Modification: 10 g of silica aerogel was added to 200 mL of ethanol, 1.5 g of a composite silane coupling agent was added, the mixture was heated to 45 ° C, stirred for 2 h, centrifuged, washed, and dried to obtain a modified aerogel;
[0094] The composite silane coupling agent is a mixture of KH560 and KH570, with a mass ratio of 4:10;
[0095] S3 reaction with phosphorus oxychloride: 10g of the modified aerogel was added to 200mL of acetonitrile, 0.012g of the catalyst TiCl4 was added, the mixture was stirred and mixed, 1.5g of phosphorus oxychloride was added, the reaction was heated to reflux with stirring for 1.5h, centrifuged, washed, and dried to obtain a primary flame-retardant modified aerogel;
[0096] S4. Reaction with DOPO: 10 g of primary flame retardant modified aerogel and 3.5 g of DOPO were added to 200 mL of toluene, heated under reflux and stirred for 3 h, centrifuged, washed, and dried to obtain flame retardant modified aerogel;
[0097] S5. Preparation of polyethylene modified foam cotton: 100g low-density polyethylene was heated to 112°C and melted for 3min, 8g ethylene-vinyl acetate copolymer and 4g ethylene-acrylic acid copolymer were added and melted, stirred and mixed for 2min, 1.5g sensitizer, 4g butyl stearate, 3g polyethylene wax and 8g flame retardant modified aerogel were added and melted for 2min, and then 15g azodicarbonamide was added, and the mixture was plasticized for 3min by repeatedly beating the triangle, and the sheet was produced. After pressurizing to 13MPa on a flat vulcanizer at 112°C for 5min, the pressure was released, and the temperature was maintained at 10MPa for cooling and molding. The absorbed dose was 85kGy for radiation cross-linking for 5min, and the mixture was foamed at 190°C for 8min, and cooled to obtain polyethylene modified foam cotton;
[0098] The sensitizer is a mixture of zinc stearate and ZnO, with a mass ratio of 1:4.
[0099] Comparative Example 4
[0100] Compared with Example 3, the difference is that steps S3, S4 and S5 are not performed.
[0101] The details are as follows:
[0102] S1. Preparation of silica aerogel: 17 g of tetraethyl orthosilicate, 120 g of ethanol and 50 mL of water were mixed, the pH value of the solution was adjusted to 10, stirred to form a gel, 150 g of ethanol was added, aged for 26 h, dried, and ball-milled for 1 h to obtain silica aerogel;
[0103] S2. Deposition of composite metal oxides: 100 g of silica aerogel, 11 g of magnesium nitrate, and 13 g of aluminum nitrate were added to 500 mL of water, and aqueous ammonia was added dropwise until the pH value of the solution was 9, heated to 90 ° C, deposited and crystallized for 30 min, filtered, washed, dried, and calcined at 650 ° C for 3 h to obtain composite metal oxide deposited silica aerogel;
[0104] S3. Preparation of polyethylene modified foam cotton: 100g of low-density polyethylene was heated to 112°C and melted for 3min, 8g of ethylene-vinyl acetate copolymer and 4g of ethylene-acrylic acid copolymer were added and melted, stirred and mixed for 2min, 1.5g of sensitizer, 4g of butyl stearate, 3g of polyethylene wax and 8g of composite metal oxide precipitated silica aerogel were added and melted for 2min, and then 15g of azodicarbonamide was added, and the mixture was plasticized for 3min by repeatedly beating the triangle, and the sheet was produced. After pressurizing to 13MPa on a flat vulcanizer at 112°C for 5min, the pressure was released, and the temperature was maintained at 10MPa for cooling and molding. The absorbed dose was 85kGy for radiation cross-linking for 5min, and the mixture was foamed at 190°C for 8min, and cooled to obtain polyethylene modified foam cotton;
[0105] The sensitizer is a mixture of zinc stearate and ZnO, with a mass ratio of 1:4.
[0106] Comparative Example 5
[0107] Compared with Example 3, the difference is that step S4 is not performed.
[0108] The details are as follows:
[0109] S1. Preparation of silica aerogel: 17 g of tetraethyl orthosilicate, 120 g of ethanol and 50 mL of water were mixed, the pH value of the solution was adjusted to 10, stirred to form a gel, 150 g of ethanol was added, aged for 26 h, dried, and ball-milled for 1 h to obtain silica aerogel;
[0110] S2. Deposition of composite metal oxides: 100 g of silica aerogel, 11 g of magnesium nitrate, and 13 g of aluminum nitrate were added to 500 mL of water, and aqueous ammonia was added dropwise until the pH value of the solution was 9, heated to 90 ° C, deposited and crystallized for 30 min, filtered, washed, dried, and calcined at 650 ° C for 3 h to obtain composite metal oxide deposited silica aerogel;
[0111] S3. Modification: 10 g of composite metal oxide deposited silica aerogel was added to 200 mL of ethanol, 1.5 g of composite silane coupling agent was added, heated to 45 ° C, stirred for 2 h, centrifuged, washed, and dried to obtain a modified aerogel;
[0112] The composite silane coupling agent is a mixture of KH560 and KH570, with a mass ratio of 4:10;
[0113] S4. Reaction with DOPO: 10 g of modified aerogel and 3.5 g of DOPO were added to 200 mL of toluene, heated under reflux and stirred for 3 h, centrifuged, washed, and dried to obtain a flame-retardant modified aerogel;
[0114] S5. Preparation of polyethylene modified foam cotton: 100g low-density polyethylene was heated to 112°C and melted for 3min, 8g ethylene-vinyl acetate copolymer and 4g ethylene-acrylic acid copolymer were added and melted, stirred and mixed for 2min, 1.5g sensitizer, 4g butyl stearate, 3g polyethylene wax and 8g flame retardant modified aerogel were added and melted for 2min, and then 15g azodicarbonamide was added, and the mixture was plasticized for 3min by repeatedly beating the triangle, and the sheet was produced. After pressurizing to 13MPa on a flat vulcanizer at 112°C for 5min, the pressure was released, and the temperature was maintained at 10MPa for cooling and molding. The absorbed dose was 85kGy for radiation cross-linking for 5min, and the mixture was foamed at 190°C for 8min, and cooled to obtain polyethylene modified foam cotton;
[0115] The sensitizer is a mixture of zinc stearate and ZnO, with a mass ratio of 1:4.
[0116] Comparative Example 6
[0117] Compared with Embodiment 3, the difference is that step S5 is not performed.
[0118] The details are as follows:
[0119] S1. Preparation of silica aerogel: 17 g of tetraethyl orthosilicate, 120 g of ethanol and 50 mL of water were mixed, the pH value of the solution was adjusted to 10, stirred to form a gel, 150 g of ethanol was added, aged for 26 h, dried, and ball-milled for 1 h to obtain silica aerogel;
[0120] S2. Deposition of composite metal oxides: 100 g of silica aerogel, 11 g of magnesium nitrate, and 13 g of aluminum nitrate were added to 500 mL of water, and aqueous ammonia was added dropwise until the pH value of the solution was 9, heated to 90 ° C, deposited and crystallized for 30 min, filtered, washed, dried, and calcined at 650 ° C for 3 h to obtain composite metal oxide deposited silica aerogel;
[0121] S3. Modification: 10 g of composite metal oxide deposited silica aerogel was added to 200 mL of ethanol, 1.5 g of composite silane coupling agent was added, heated to 45 ° C, stirred for 2 h, centrifuged, washed, and dried to obtain a modified aerogel;
[0122] The composite silane coupling agent is a mixture of KH560 and KH570, with a mass ratio of 4:10;
[0123] S4 reaction with phosphorus oxychloride: 10g of the modified aerogel was added to 200mL of acetonitrile, 0.012g of the catalyst TiCl4 was added, the mixture was stirred and mixed, 1.5g of phosphorus oxychloride was added, the reaction was heated to reflux with stirring for 1.5h, centrifuged, washed, and dried to obtain a primary flame-retardant modified aerogel;
[0124] S5. Preparation of polyethylene modified foam cotton: 100g low-density polyethylene was heated to 112°C and melted for 3min, 8g ethylene-vinyl acetate copolymer and 4g ethylene-acrylic acid copolymer were added and melted, stirred and mixed for 2min, 1.5g sensitizer, 4g butyl stearate, 3g polyethylene wax and 8g primary flame retardant modified aerogel were added and melted for 2min, and then 15g azodicarbonamide was added, and the mixture was plasticized for 3min by repeatedly beating the triangle, and the sheet was produced. After pressurizing to 13MPa on a flat vulcanizer at 112°C for 5min, the pressure was released, and the temperature was maintained at 10MPa for cooling and molding. The absorbed dose was 85kGy for radiation cross-linking for 5min, and foaming was performed at 190°C for 8min, and cooling was performed to obtain polyethylene modified foam cotton;
[0125] The sensitizer is a mixture of zinc stearate and ZnO, with a mass ratio of 1:4.
[0126] Comparative Example 7
[0127] The details are as follows:
[0128] Compared with Example 3, the difference is that butyl stearate is not added in step S6.
[0129] The details are as follows:
[0130] S1. Preparation of silica aerogel: 17 g of tetraethyl orthosilicate, 120 g of ethanol and 50 mL of water were mixed, the pH value of the solution was adjusted to 10, stirred to form a gel, 150 g of ethanol was added, aged for 26 h, dried, and ball-milled for 1 h to obtain silica aerogel;
[0131] S2. Deposition of composite metal oxides: 100 g of silica aerogel, 11 g of magnesium nitrate, and 13 g of aluminum nitrate were added to 500 mL of water, and aqueous ammonia was added dropwise until the pH value of the solution was 9, heated to 90 ° C, deposited and crystallized for 30 min, filtered, washed, dried, and calcined at 650 ° C for 3 h to obtain composite metal oxide deposited silica aerogel;
[0132] S3. Modification: 10 g of composite metal oxide deposited silica aerogel was added to 200 mL of ethanol, 1.5 g of composite silane coupling agent was added, heated to 45 ° C, stirred for 2 h, centrifuged, washed, and dried to obtain a modified aerogel;
[0133] The composite silane coupling agent is a mixture of KH560 and KH570, with a mass ratio of 4:10;
[0134] S4 reaction with phosphorus oxychloride: 10g of the modified aerogel was added to 200mL of acetonitrile, 0.012g of the catalyst TiCl4 was added, the mixture was stirred and mixed, 1.5g of phosphorus oxychloride was added, the reaction was heated to reflux with stirring for 1.5h, centrifuged, washed, and dried to obtain a primary flame-retardant modified aerogel;
[0135] S5. Reaction with DOPO: 10 g of primary flame retardant modified aerogel and 3.5 g of DOPO were added to 200 mL of toluene, heated under reflux and stirred for 3 h, centrifuged, washed, and dried to obtain flame retardant modified aerogel;
[0136] S6. Preparation of polyethylene modified foam cotton: 100g of low-density polyethylene was heated to 112°C and melted for 3min, 8g of ethylene-vinyl acetate copolymer and 4g of ethylene-acrylic acid copolymer were added and melted, stirred and mixed for 2min, 1.5g of sensitizer, 3g of polyethylene wax and 8g of flame-retardant modified aerogel were added and melted for 2min, and then 15g of azodicarbonamide was added, and the mixture was plasticized for 3min by repeatedly beating the triangle, and the sheet was produced. After pressurizing to 13MPa on a flat vulcanizer at 112°C for 5min, the pressure was released, and the temperature was maintained at 10MPa for cooling and molding. The absorbed dose was 85kGy for radiation cross-linking for 5min, and the mixture was foamed at 190°C for 8min, and cooled to obtain polyethylene modified foam cotton;
[0137] The sensitizer is a mixture of zinc stearate and ZnO, with a mass ratio of 1:4.
[0138] Comparative Example 8
[0139] Compared with Example 3, the difference is that no flame retardant modified aerogel is added in step S6.
[0140] The details are as follows:
[0141] Preparation of polyethylene modified foam cotton: 100g low-density polyethylene was heated to 112°C and melted for 3min, 8g ethylene-vinyl acetate copolymer and 4g ethylene-acrylic acid copolymer were added and melted, stirred and mixed for 2min, 1.5g sensitizer, 4g butyl stearate, and 3g polyethylene wax were added and melted for 2min, and then 15g azodicarbonamide was added, and the mixture was plasticized for 3min by repeatedly beating the triangle, and the sheet was produced. After pressurizing to 13MPa on a flat vulcanizer at 112°C for 5min, the pressure was released, and the temperature was maintained at 10MPa for cooling and molding. The absorbed dose was 85kGy for radiation cross-linking for 5min, and the mixture was foamed at 190°C for 8min, and cooled to obtain polyethylene modified foam cotton;
[0142] The sensitizer is a mixture of zinc stearate and ZnO, with a mass ratio of 1:4.
[0143] Comparative Example 9
[0144] Compared with Example 3, the difference is that in step S4, phosphorus oxychloride and modified aerogel are mixed and no reaction occurs.
[0145] The details are as follows:
[0146] S1. Preparation of silica aerogel: 17 g of tetraethyl orthosilicate, 120 g of ethanol and 50 mL of water were mixed, the pH value of the solution was adjusted to 10, stirred to form a gel, 150 g of ethanol was added, aged for 26 h, dried, and ball-milled for 1 h to obtain silica aerogel;
[0147] S2. Deposition of composite metal oxides: 100 g of silica aerogel, 11 g of magnesium nitrate, and 13 g of aluminum nitrate were added to 500 mL of water, and aqueous ammonia was added dropwise until the pH value of the solution was 9, heated to 90 ° C, deposited and crystallized for 30 min, filtered, washed, dried, and calcined at 650 ° C for 3 h to obtain composite metal oxide deposited silica aerogel;
[0148] S3. Modification: 10 g of composite metal oxide deposited silica aerogel was added to 200 mL of ethanol, 1.5 g of composite silane coupling agent was added, heated to 45 ° C, stirred for 2 h, centrifuged, washed, and dried to obtain a modified aerogel;
[0149] The composite silane coupling agent is a mixture of KH560 and KH570, with a mass ratio of 4:10;
[0150] S4 reaction with phosphorus oxychloride: 10g of modified aerogel and 1.5g of phosphorus oxychloride were added to obtain a primary flame-retardant modified aerogel;
[0151] S5. Reaction with DOPO: 10 g of primary flame retardant modified aerogel and 3.5 g of DOPO were added to 200 mL of toluene, heated under reflux and stirred for 3 h, centrifuged, washed, and dried to obtain flame retardant modified aerogel;
[0152] S6. Preparation of polyethylene modified foam cotton: 100g of low-density polyethylene was heated to 112°C and melted for 3min, 8g of ethylene-vinyl acetate copolymer and 4g of ethylene-acrylic acid copolymer were added and melted, stirred and mixed for 2min, 1.5g of sensitizer, 4g of butyl stearate, 3g of polyethylene wax and 8g of flame-retardant modified aerogel were added and melted for 2min, and then 15g of azodicarbonamide was added, and the mixture was plasticized for 3min by repeatedly beating the triangle, and the sheet was produced. After pressurizing to 13MPa on a flat vulcanizer at 112°C for 5min, the pressure was released, and the temperature was maintained at 10MPa for cooling and molding. The absorbed dose was 85kGy for radiation cross-linking for 5min, and the mixture was foamed at 190°C for 8min, and cooled to obtain polyethylene modified foam cotton;
[0153] The sensitizer is a mixture of zinc stearate and ZnO, with a mass ratio of 1:4.
[0154] Comparative Example 10
[0155] Compared with Example 3, the difference is that in step S5, DOPO and the primary flame retardant modified aerogel are mixed and no reaction occurs.
[0156] The details are as follows:
[0157] S1. Preparation of silica aerogel: 17 g of tetraethyl orthosilicate, 120 g of ethanol and 50 mL of water were mixed, the pH value of the solution was adjusted to 10, stirred to form a gel, 150 g of ethanol was added, aged for 26 h, dried, and ball-milled for 1 h to obtain silica aerogel;
[0158] S2. Deposition of composite metal oxides: 100 g of silica aerogel, 11 g of magnesium nitrate, and 13 g of aluminum nitrate were added to 500 mL of water, and aqueous ammonia was added dropwise until the pH value of the solution was 9, heated to 90 ° C, deposited and crystallized for 30 min, filtered, washed, dried, and calcined at 650 ° C for 3 h to obtain composite metal oxide deposited silica aerogel;
[0159] S3. Modification: 10 g of composite metal oxide deposited silica aerogel was added to 200 mL of ethanol, 1.5 g of composite silane coupling agent was added, heated to 45 ° C, stirred for 2 h, centrifuged, washed, and dried to obtain a modified aerogel;
[0160] The composite silane coupling agent is a mixture of KH560 and KH570, with a mass ratio of 4:10;
[0161] S4 reaction with phosphorus oxychloride: 10g of the modified aerogel was added to 200mL of acetonitrile, 0.012g of the catalyst TiCl4 was added, the mixture was stirred and mixed, 1.5g of phosphorus oxychloride was added, the reaction was heated to reflux with stirring for 1.5h, centrifuged, washed, and dried to obtain a primary flame-retardant modified aerogel;
[0162] S5. Reaction with DOPO: 10 g of primary flame retardant modified aerogel and 3.5 g of DOPO were mixed to obtain flame retardant modified aerogel;
[0163] S6. Preparation of polyethylene modified foam cotton: 100g of low-density polyethylene was heated to 112°C and melted for 3min, 8g of ethylene-vinyl acetate copolymer and 4g of ethylene-acrylic acid copolymer were added and melted, stirred and mixed for 2min, 1.5g of sensitizer, 4g of butyl stearate, 3g of polyethylene wax and 8g of flame-retardant modified aerogel were added and melted for 2min, and then 15g of azodicarbonamide was added, and the mixture was plasticized for 3min by repeatedly beating the triangle, and the sheet was produced. After pressurizing to 13MPa on a flat vulcanizer at 112°C for 5min, the pressure was released, and the temperature was maintained at 10MPa for cooling and molding. The absorbed dose was 85kGy for radiation cross-linking for 5min, and the mixture was foamed at 190°C for 8min, and cooled to obtain polyethylene modified foam cotton;
[0164] The sensitizer is a mixture of zinc stearate and ZnO, with a mass ratio of 1:4.
[0165] Test Example 1
[0166] The polyethylene modified foamed cottons prepared in Examples 1-3 of the present invention and Comparative Examples 1-10 were subjected to performance tests, and the results are shown in Table 1.
[0167] The room temperature thermal conductivity was tested using the steady-state heat flow method (instrument model: NETZSCH HFM 446 Lambda).
[0168] The mechanical properties are tested according to GB / T 6669-2008 "Determination of permanent compression set of flexible foam", GB / T 10807-2006 "Determination of hardness of flexible polymeric foam materials (indentation method)" and GB / T 6344-2008 "Determination of tensile strength and elongation at break of flexible foam".
[0169] The test adopts GB / T2406.2-2009 "Determination of Combustion Behavior of Plastics by Oxygen Index Method Part 2: Room Temperature Test" to test the Limiting Oxygen Index (LOI).
[0170] Table 1
[0171]
[0172] It can be seen from the above table that the polyethylene modified foamed cotton prepared in Examples 1-3 of the present invention has better comprehensive properties.
[0173] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing polyethylene modified foamed cotton, characterized in that: Composite metal oxides are deposited on the surface of silica aerogel, which is modified with a silane coupling agent and then reacted with phosphorus oxychloride and DOPO in sequence. The surface is added to low-density polyethylene, mixed with ethylene-vinyl acetate copolymer, ethylene-acrylic acid copolymer, a sensitizer, and polyethylene wax, and then refined. A foaming agent is then added, plasticized, sheeted, radiation cross-linked, foamed, and cooled to produce polyethylene-modified foam.
2. The preparation method according to claim 1, characterized in that The following steps are involved: S1. Preparation of silica aerogel: alkyl orthosilicate, ethanol and water were mixed uniformly, the pH of the solution was adjusted to alkaline, stirred to form a gel, ethanol was added for aging, and dried to obtain silica aerogel; S2. Deposition of composite metal oxides: Silica aerogel, magnesium nitrate, and aluminum nitrate were dissolved in water, alkali solution was added dropwise, and the deposition was heated for crystallization, filtered, washed, dried, and calcined to obtain composite metal oxide deposited silica aerogel; S3 modification: adding the composite metal oxide deposited silica aerogel to ethanol, adding a composite silane coupling agent, heating and stirring the reaction, centrifuging, washing, and drying to obtain a modified aerogel; S4 reaction with phosphorus oxychloride: The modified aerogel was added to acetonitrile, a catalyst was added, stirred and mixed, phosphorus oxychloride was added, the reaction was heated under reflux with stirring, centrifuged, washed, and dried to obtain a primary flame-retardant modified aerogel; S5. Reaction with DOPO: adding the primary flame-retardant modified aerogel and DOPO to toluene, heating and stirring under reflux, centrifuging, washing, and drying to obtain a flame-retardant modified aerogel; S6. Preparation of polyethylene modified foam cotton: melt low-density polyethylene in a mill, add ethylene-vinyl acetate copolymer and ethylene-acrylic acid copolymer, stir and mix evenly, add sensitizer, butyl stearate, polyethylene wax and flame retardant modified aerogel and start milling, then add foaming agent, plasticize, sheet out, radiation cross-link, foam, cool, and obtain polyethylene modified foam cotton.
3. The preparation method according to claim 2, characterized in that In step S1, the mass ratio of alkyl orthosilicate, ethanol and water is 15-20:110-130:40-60, the pH value of the adjusted solution is 9.5-10.5, and the aging time is 24-28 hours.
4. The preparation method according to claim 2, characterized in that In step S2, the mass ratio of the silica aerogel, magnesium nitrate, and aluminum nitrate is 100:10-12:12-15, the alkali solution is ammonia water, the temperature of the heating deposition crystallization is 85-95° C., the time is 20-40 minutes, and the temperature of the calcination is 600-700° C., and the time is 2-4 hours.
5. The preparation method according to claim 2, characterized in that In step S3, the mass ratio of the composite metal oxide deposited silica aerogel and the composite silane coupling agent is 10:1-2, the composite silane coupling agent is a mixture of KH560 and KH570, and the mass ratio is 3-5:
10. The temperature of the heating and stirring reaction is 40-50°C, and the time is 1-3h.
6. The preparation method according to claim 2, characterized in that In step S4, the mass ratio of the modified aerogel, the catalyst, and phosphorus oxychloride is 10:0.01-0.015:1-2, the heating reflux stirring reaction time is 1-2h, and the catalyst is TiCl4.
7. The preparation method according to claim 2, characterized in that In step S5, the mass ratio of the primary flame-retardant modified aerogel to DOPO is 10:3-4, and the heating reflux stirring reaction is carried out for 2-4 hours.
8. The preparation method according to claim 2, characterized in that The mass ratio of the low-density polyethylene, ethylene-vinyl acetate copolymer, ethylene-acrylic acid copolymer, sensitizer, butyl stearate, polyethylene wax, flame retardant modified aerogel, and foaming agent in step S6 is 100:7-9:3-5:1-2:3-5:1-3:7-10:12-17, the radiation crosslinking is an absorbed dose of 75-95 kGy radiation crosslinking for 4-7 minutes, the foaming temperature is 180-200 ° C, the time is 7-10 minutes, the sensitizer is a mixture of zinc stearate and ZnO in a mass ratio of 1:3-5, and the foaming agent is azodicarbonamide.
9. The preparation method according to claim 2, characterized in that The specific steps include: S1. Preparation of silica aerogel: 15-20 parts by weight of alkyl orthosilicate, 110-130 parts by weight of ethanol and 40-60 parts by weight of water were mixed, the pH of the solution was adjusted to 9.5-10.5, stirred to form a gel, 100-200 parts by weight of ethanol was added, aged for 24-28h, dried, and ball-milled for 1h to obtain silica aerogel; S2. Deposition of a composite metal oxide: 100 parts by weight of silica aerogel, 10-12 parts by weight of magnesium nitrate, 12-15 parts by weight of aluminum nitrate were dissolved in water, aqueous ammonia was added dropwise to a pH value of 8.5-9.5, heated to 85-95 ° C, deposited and crystallized for 20-40 min, filtered, washed, dried, and calcined at 600-700 ° C for 2-4 h to obtain a composite metal oxide deposited silica aerogel; S3 modification: 10 parts by weight of the composite metal oxide deposited silica aerogel was added to ethanol, 1-2 parts by weight of the composite silane coupling agent was added, heated to 40-50 ° C, stirred for 1-3h, centrifuged, washed, and dried to obtain a modified aerogel; The composite silane coupling agent is a mixture of KH560 and KH570, with a mass ratio of 3-5:10; S4 reaction with phosphorus oxychloride: 10 parts by weight of the modified aerogel was added to acetonitrile, 0.01-0.015 parts by weight of the catalyst TiCl4 was added, stirred and mixed, 1-2 parts by weight of phosphorus oxychloride was added, the reaction was heated under reflux with stirring for 1-2h, centrifuged, washed, and dried to obtain a primary flame-retardant modified aerogel; S5 reaction with DOPO: 10 parts by weight of the primary flame retardant modified aerogel and 3-4 parts by weight of DOPO were added to toluene, heated to reflux with stirring for 2-4h, centrifuged, washed, and dried to obtain a flame retardant modified aerogel; S6. Preparation of polyethylene modified foam: 100 parts by weight of low-density polyethylene is heated to 110-115 ° C and melted for 2-4 minutes, 7-9 parts by weight of ethylene-vinyl acetate copolymer and 3-5 parts by weight of ethylene-acrylic acid copolymer are added and the mixture is stirred for 1-3 minutes, 1-2 parts by weight of sensitizer, 3-5 parts by weight of butyl stearate, 1-3 parts by weight of polyethylene wax and 7-10 parts by weight of flame retardant modified aerogel are added and the mixture is melted for 1-3 minutes, and then 12-17 parts by weight of foaming agent is added. The mixture is plasticized for 2-4 minutes by repeatedly beating in a triangle manner, and the sheet is produced. After pressurizing to 12-15 MPa on a flat vulcanizing agent at 110-115 ° C and melting for 4-6 minutes, the pressure is released, and the mixture is cooled and molded at 10 MPa. The absorbed dose is 75-95 kGy and radiation cross-linked for 4-7 minutes. The mixture is foamed at 180-200 ° C for 7-10 minutes and cooled to obtain polyethylene modified foam; The sensitizer is a mixture of zinc stearate and ZnO, with a mass ratio of 1:3-5.
10. A polyethylene modified foam obtained by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Sulfonated polyether-ether-ketone / phosphorylated mesoporous silica hybrid membrane preparation and application
CN103897336A
Blister sheets of flame-retardant and heat insulation and preparing method thereof
CN106349539A
DOPO-based silicon-phosphorus synergistic flame retardant as well as preparation method and application thereof
CN111793090A
KH550 modified nano silicon dioxide and hydrotalcite / quadripolymer composite leather finishing agent and preparation method thereof
CN116333548A
PET environment-friendly material and preparation method thereof
CN118085515A