Through the combination of high-white conductive particles and porous foam structure, the problem of insufficient thermal control and electrostatic protection in high-orbit environments of traditional phase change radiators is solved, and more efficient heat dissipation and electrostatic protection are achieved, which improves the spacecraft's Performance and reliability.

CN119081233APending Publication Date: 2024-12-06NANJING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411064842.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Traditional phase change radiators have insufficient thermal conductivity and risk of electrostatic accumulation in thermal control and electrostatic protection in high-orbit environments, and cannot effectively deal with rapid temperature changes and high-charge environments, affecting the performance and reliability of the spacecraft.

Method used

High whiteness conductive particles are prepared by mixing sintering of trivalent dopant ions and metal oxides, and mixed with binder or high transparent crystalline polymer to form antistatic thermally controlled coatings or Films, combined with porous foam structure, prepare anti-static phase change radiation devices.

Benefits of technology

It significantly improves the thermal response speed and electrostatic protection capabilities of the spacecraft in extreme environments, reduces the risk of static accumulation, enhances the heat dissipation and dispersion capabilities, and ensures the stability and durability of the system.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081233A_ABST
    Figure CN119081233A_ABST
Patent Text Reader

Abstract

The invention discloses a high-whiteness conductive particle as well as a preparation method and application thereof, and belongs to the technical field of thermal control and static prevention of spacecrafts. The anti-static phase change radiator prepared by the invention is obtained by compounding a high-reflection and high-emission shell structure consisting of an anti-static thermal control layer based on high-whiteness conductive particles and a composite phase change material core material based on a porous foam structure. The prepared anti-static phase change radiator has the advantages of being high in anti-static capacity, heat collection capacity, heat transmission capacity and heat dissipation capacity, short in assembly period, easy to construct and capable of being prepared in a large area, and the anti-static and heat dissipation requirements of high-orbit operation spacecrafts can be met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of thermal control and anti-static technology of spacecraft, and specifically relates to high-whiteness conductive particles and a preparation method and application thereof. Background Art

[0002] In the design and operation of modern spacecraft, thermal control and anti-static are key factors to ensure equipment performance and stability. Especially in high-orbit environments, spacecraft must face extreme temperature changes and highly charged plasma environments, which put forward higher requirements for thermal control systems and anti-static systems.

[0003] Although traditional phase change radiators play an important role in spacecraft thermal management, their technical limitations are becoming increasingly prominent. First, the phase change materials that these devices rely on generally have low thermal conductivity, which limits their response speed in rapidly changing ambient temperatures. In aerospace environments, especially when faced with rapid temperature changes caused by solar radiation, this thermal control method may not be able to adjust the internal temperature in a timely manner, thus affecting the overall performance and reliability of the spacecraft system. Secondly, in today's electronic device design that is increasingly pursuing miniaturization and high-functionality integration, electrostatic control is particularly critical. As circuit board density increases and component size decreases, the risk of electrostatic discharge (ESD) increases accordingly, and even extremely low charge accumulation may cause damage to sensitive components. Therefore, designing efficient electrostatic protection measures to reduce these risks is crucial to maintaining the performance and reliability of equipment. Summary of the invention

[0004] The purpose of this section is to summarize some aspects of embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.

[0005] Based on the above problems, the present invention proposes a porous foam structure with efficient thermal buffering and energy storage and heat absorption functions under extreme temperature fluctuations. This porous foam structure is coated with an anti-static, highly reflective and highly emissive shell structure composed of high-whiteness conductive particles, achieving excellent thermal control and electrostatic protection dual functions. This integrated design significantly enhances the operational performance and reliability of spacecraft in complex space environments, ensuring higher system stability and long-term durability.

[0006] In view of the above problems and / or the problems existing in the prior art, the present invention is proposed.

[0007] Therefore, the object of the present invention is to overcome the deficiencies in the prior art and provide a method for preparing high-whiteness conductive particles.

[0008] In order to solve the above technical problems, the present invention provides the following technical solutions, including:

[0009] After two or more trivalent dopant ions and metal oxides are uniformly mixed, they are washed, dried, ground, and sintered at 100-400° C. for 1-6 hours in an inert atmosphere to prepare high-whiteness conductive particles.

[0010] As a preferred embodiment of the method for preparing high-whiteness conductive particles of the present invention, the molar ratio of the trivalent dopant ions to the metal oxide is 1:20-100, and the inert atmosphere includes one or more of high-purity nitrogen, high-purity argon, and high-purity helium.

[0011] As a preferred embodiment of the method for preparing the high-whiteness conductive particles of the present invention, the trivalent dopant ions include one or more of aluminum ions, gallium ions, indium ions, tin ions or gadolinium ions; and the metal oxide includes oxides of Zn, Al, Zr, Mg and Y.

[0012] The purpose of the present invention is to overcome the deficiencies in the prior art and provide a high-whiteness conductive particle.

[0013] The purpose of the present invention is to overcome the deficiencies in the prior art and provide an antistatic thermal control coating prepared by using high-whiteness conductive particles.

[0014] In order to solve the above technical problems, the present invention provides the following technical solutions, a method for preparing an antistatic thermal control coating, comprising:

[0015] The high whiteness conductive particles and the binder are uniformly mixed in a mass ratio of 2 to 4:1 and fully stirred to obtain an antistatic thermal control coating.

[0016] As a preferred embodiment of the preparation method of the antistatic thermal control coating of the present invention, the binder includes an organic binder or an inorganic binder; the organic binder includes one or more of silicone resin, acrylic resin, fluorocarbon resin, and polyurethane; the inorganic binder includes one or more of potassium silicate, lithium silicate, sodium silicate, and aluminum dihydrogen phosphate.

[0017] As a preferred solution of the method for preparing the antistatic thermal control coating of the present invention, the uniform mixing is performed by vacuum stirring at a speed of 1500 rpm to 2000 rpm under -70 kPa to -90 kPa.

[0018] The purpose of the present invention is to overcome the deficiencies in the prior art and provide an antistatic thermal control film, comprising:

[0019] The high whiteness conductive particles and the high transparency crystalline polymer are fully mixed in a mass ratio of 1:1 to 4, and then kneaded at a high temperature of 150°C to 300°C to obtain hybrid particles; the hybrid particles are extruded at a high temperature of 150°C to 300°C to form a film, thereby obtaining an antistatic thermal control film;

[0020] The highly transparent crystalline polymer includes one or more of polyurethane polymer particles, polytetrafluoroethylene polymer particles, 4-methylpentene polymer particles, thermoplastic elastomer particles, and polypropylene polymer particles.

[0021] The purpose of the present invention is to overcome the deficiencies in the prior art and provide an antistatic phase change radiator prepared by an antistatic thermal control coating or an antistatic thermal control film.

[0022] In order to solve the above technical problems, the present invention provides the following technical solutions: a method for preparing an anti-static phase change radiator, comprising:

[0023] The porous foam is immersed in the phase change material, and after being completely immersed for 1 to 5 hours, it is dried at 40 to 60° C. for 12 to 24 hours to prepare a composite phase change material;

[0024] Attaching an antistatic thermal control film to the surface of the shell or spraying or brushing an antistatic thermal control coating onto the surface of the shell to form an antistatic thermal control layer on the surface of the shell;

[0025] The anti-static phase change radiator can be obtained by filling the composite phase change material into the shell.

[0026] As a preferred embodiment of the preparation method of the anti-static phase change radiator of the present invention, the porous foam includes one or more of carbon foam, copper foam, and aluminum foam, and the phase change material includes one or more of paraffin, fatty acids, and polyols.

[0027] As a preferred solution of the method for preparing the antistatic phase change radiator of the present invention, the thickness of the antistatic thermal control layer is 100-500 μm.

[0028] As a preferred embodiment of the method for preparing the antistatic phase change radiator of the present invention, the highly transparent crystalline polymer comprises one or more of polyurethane polymer particles, polytetrafluoroethylene polymer particles, 4-methylpentene polymer particles, thermoplastic elastomer particles, and polypropylene polymer particles;

[0029] The shell includes one or more of aluminum alloy, titanium alloy and magnesium alloy.

[0030] Beneficial effects of the present invention:

[0031] (1) The antistatic thermal control layer of the present invention greatly reduces the risk of static electricity accumulation due to the introduction of high-whiteness conductive particles, and has high reflection in the solar band and high emission in the wide infrared band, thereby improving the heat dissipation capacity and static electricity dissipation capacity of the system in a high-orbit environment.

[0032] (2) The anti-static phase change radiator of the present invention has the characteristics of anti-static ability, strong heat collection, transmission and dissipation capabilities, which can dissipate the heat on the surface of the device to the external environment and ensure the safe operation of the spacecraft.

[0033] (3) Compared with traditional thermal control coatings and phase change materials, the anti-static phase change radiator of the present invention has significantly enhanced heat dissipation efficiency. Compared with traditional thermal control coatings, this technology not only reduces static electricity accumulation, but also utilizes phase change materials to enhance the rapid dispersion of thermal energy, allowing the spacecraft to maintain a safe and stable working state under extreme environmental conditions such as direct sunlight; compared with traditional phase change materials, the present invention significantly improves the thermal response speed and thermal conductivity by combining porous foam structure and phase change material. This structure not only accelerates the absorption and release of thermal energy, but also ensures that heat is more evenly distributed throughout the system through efficient heat conduction, thereby improving the performance and reliability of the thermal management system under rapidly changing ambient temperatures.

[0034] (4) The antistatic thermal control layer of the present invention has the characteristics of short assembly cycle, simple construction, and large-area preparation, which can meet the antistatic and heat dissipation requirements of high-orbit spacecraft. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work. Among them:

[0036] Figure 1 It is a schematic diagram of the structure of the antistatic phase change radiator of the present invention; wherein 1 is an antistatic upper cover plate, 2 is a high thermal conductivity composite phase change material, and 3 is an antistatic lower shell.

[0037] Figure 2 It is a schematic diagram of the structure of the composite phase change material of the present invention.

[0038] Figure 3 The figure is a flow chart for preparing the anti-static phase change radiator of the present invention. DETAILED DESCRIPTION

[0039] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.

[0040] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0041] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.

[0042] The raw materials used in the present invention are all commercially available unless otherwise specified.

[0043] The material prepared in the embodiment of the present invention was tested for performance according to the following method. The measurement object of solar band reflectivity, infrared broadband emissivity and resistivity was the antistatic thermal control layer:

[0044] Solar band reflectivity: The equipment used is the American Agilent Cary5000 UV-visible-near infrared spectrophotometer, which can measure wavelengths from 190 to 3300 nm, with a wavelength resolution of 1 nm. The surface of the film sample measured is diffuse reflection, and the surface reflectivity measurement needs to be completed with the help of an integrating sphere accessory. Test conditions: atmospheric environment, room temperature (~25°C), relative humidity of 30% to 40%.

[0045] Infrared wide-band emissivity: The equipment used is the V80v Fourier infrared spectrometer from Bruker, Germany, with a test wavelength range of 4000-400 (2.5-25 μm) and a resolution of 64 cm -1 The surface of the film sample to be measured is diffuse reflection, and the surface emissivity measurement needs to be completed with the help of an integrating sphere accessory. Test conditions: atmospheric environment, room temperature (~25°C), relative humidity of 30%~40%.

[0046] Volume resistivity: Refer to GB / T 1410-2006 test standard.

[0047] Whiteness: Take 5-10g of powder and press it into a disc with a thickness of 5-10mm and a diameter of 5cm; place the disc at the light outlet of the Beiguang WSD-3C fully automatic whiteness meter and measure it multiple times to get the average whiteness value.

[0048] Example 1

[0049] This embodiment provides a method for preparing an anti-static phase change radiator. Figures 1 to 3 , specifically:

[0050] 1) Take 50g of solid paraffin in a glass container, and then heat the container at 100℃ in a water bath to completely melt the paraffin. Then, the soft, lightweight, porous carbon foam is completely immersed in the paraffin solution under vacuum conditions. During the entire immersion process, the paraffin diffuses into the foamed aluminum and is encapsulated into its porous structure;

[0051] After being completely immersed for 1 hour, the material was taken out of the solution and dried at 40°C for 12 hours, and finally a paraffin / carbon foam composite phase change material with porous carbon foam as the skeleton material and paraffin as the phase change core material was prepared.

[0052] 2) 1 kg of zinc oxide, 40 g of aluminum nitrate nonahydrate and 40 g of gallium chloride were dissolved in 2 L of deionized water, i.e., the molar ratio of dopant to metal oxide was 1:36.8, mixed and stirred for 4 h, ultrasonically dispersed for 1 h, and vacuum dried for 24 h. The powder cake was taken out and ground for 1 h. The ground powder was sintered at low temperature in a nitrogen atmosphere at a reaction temperature of 300° C. for a reaction time of 6 h to obtain high whiteness conductive particles with a whiteness of 93;

[0053] The high whiteness conductive particles and the polypropylene particles are fully mixed at a mass ratio of 1:1.5, and kneaded at 180° C. to obtain hybrid particles;

[0054] The hybrid particles are extruded at 180° C. to form a film, thereby obtaining an antistatic thermal control film, namely, an antistatic thermal control layer, with a thickness of 200 μm.

[0055] 3) Using a coating machine to coat the surface of the film with silicone adhesive, curing at 130°C for 2 minutes, and compounding with an aluminum alloy shell after curing to obtain an anti-static, highly reflective, and highly emissive shell structure, and filling the composite phase change material obtained in step 1) into the shell to obtain an anti-static phase change radiator.

[0056] Example 2

[0057] The difference between this embodiment and embodiment 1 is that the mass ratio of high whiteness conductive particles to polypropylene particles is adjusted from 1:1.5 to 1:3, and the rest of the preparation process is the same as that of embodiment 1 to obtain an antistatic phase change radiator.

[0058] Example 3

[0059] The difference between this embodiment and embodiment 1 is that the mass ratio of high whiteness conductive particles to polypropylene particles is adjusted from 1:1.5 to 1:4, and the rest of the preparation process is the same as that of embodiment 1 to obtain an antistatic phase change radiator.

[0060] The performance of the material prepared in the above embodiment was tested, and the comparison results with those in Example 1 are shown in Table 1.

[0061] Table 1

[0062] Example 1 Example 2 Example 3 Whiteness of high whiteness conductive particles 93 93 93 Solar band reflectivity (%) 92 86 82 Infrared broadband emissivity (%) 96 95 95 Volume resistivity (Ω·m) <![CDATA[3.1×10 3 ]]> <![CDATA[2.5×10 5 ]]> <![CDATA[3.6×10 7 ]]>

[0063] It can be seen from the above table that adjusting the mixing mass ratio of high whiteness conductive particles to polypropylene particles has a significant effect on the performance of the antistatic phase change radiator. This is because the adjustment of the proportion of high whiteness conductive particles will change the solar reflectivity and volume resistivity of the film. Too high will lead to poor mechanical properties of the antistatic thermal control layer, and too low will lead to too low reflectivity of the film, absorbing too much sunlight and reducing the cooling effect. And the volume resistivity increases, resulting in a weakened antistatic effect; according to the results in the above table, the best technical effect can be obtained when the mixing mass ratio of high whiteness conductive particles to polypropylene particles in the present invention is 1:1.5.

[0064] Example 4

[0065] The difference between this embodiment and embodiment 1 is that the addition amount of trivalent dopant ions is adjusted to 20g aluminum nitrate nonahydrate and 20g gallium chloride, that is, the molar ratio of dopant to metal oxide is 1:73.6, and the rest of the preparation process is the same as embodiment 1 to obtain an antistatic phase change radiator.

[0066] Example 5

[0067] The difference between this embodiment and embodiment 1 is that the addition amount of trivalent dopant ions is adjusted to 60g aluminum nitrate nonahydrate and 60g gallium chloride, that is, the molar ratio of dopant to metal oxide is 1:24.5, and the rest of the preparation process is the same as embodiment 1 to obtain an antistatic phase change radiator.

[0068] The performance of the material prepared in the above embodiment was tested, and the comparison results with those in Example 1 are shown in Table 2.

[0069] Table 2

[0070] Example 1 Example 4 Example 5 Whiteness of high whiteness conductive particles 93 94 85 Solar band reflectivity (%) 92 92 87 Infrared broadband emissivity (%) 96 96 95 Volume resistivity (Ω·m) <![CDATA[3.1×10 3 ]]> <![CDATA[4.5×10 5 ]]> <![CDATA[2.0×10 3 ]]>

[0071] As can be seen from the above table, the adjustment of the ratio of dopant to metal oxide has a significant effect on the performance of the antistatic phase change radiator, because the adjustment of the ratio of dopant to metal oxide will affect the whiteness and conductivity of high whiteness conductive particles. Too high will lead to a decrease in particle whiteness, thereby causing a decrease in solar reflectivity, and too low will lead to an increase in volume resistivity and a deterioration in antistatic effect; according to the results in the above table, the best technical effect can be obtained when the molar ratio of dopant to metal oxide in the present invention is 1:36.8.

[0072] Example 6

[0073] In this embodiment, the high-whiteness conductive particles prepared in Example 1 are uniformly mixed with a potassium silicate aqueous solution with a mass fraction of 40% in a mass ratio of 2.5:1, and stirred sufficiently to obtain an antistatic thermal control coating. The coating is sprayed on an aluminum alloy shell to form an antistatic protective layer; the rest of the preparation process is the same as in Example 1 to obtain an antistatic phase change radiator.

[0074] The coating has a reflectivity of 92%, an infrared broadband emissivity of 93%, and a volume resistivity of 3.6×10 3 Ω·m.

[0075] Comparative Example 1

[0076] In this comparative example, gallium-indium-tin alloy is selected as the phase change material, and a thin copper plate is selected as the packaging material, and ordinary thermal control white paint is compounded on the shell surface. The rest of the preparation process is the same as that in Example 1. In order to utilize the high thermal conductivity of copper, the gallium-based alloy is heated to a temperature above the melting point to completely liquefy it. Design a copper plate of appropriate size and reserve a welding edge, and then inject the liquid gallium-based alloy between the two copper plates, paying attention to avoid bubble generation. Use fine laser welding technology to weld the seal at the edge of the copper plate to ensure the sealing strength and integrity of the package.

[0077] Ordinary thermal control layer has no antistatic effect. The volume resistivity of the thermal control layer is ≥10 10 Ω·m, and the solar reflectivity is 85%, and the infrared wide-band emissivity is 92%. The experiment was conducted in a simulated high-orbit space environment. Both samples were above a stable heat source. After a long period of testing, the heat dissipation efficiency of the sample in Example 1 was 32% higher than that of the comparative example. There was static electricity accumulation on the surface of the sample in Comparative Example 1, and the effect was significantly worse than that of Example 1.

[0078] Comparative Example 2

[0079] The difference between this comparative example and Example 1 is that the mass ratio of high whiteness conductive particles to polypropylene particles is adjusted from 1:1.5 to 1:1, and the rest of the preparation process is the same as that of Example 1.

[0080] The anti-static thermal control film was poorly formed and the preparation of the anti-static phase change radiator failed.

[0081] Comparative Example 3

[0082] The difference between this comparative example and Example 1 is that the mass ratio of high whiteness conductive particles to polypropylene particles is adjusted from 1:1.5 to 1:5, and the rest of the preparation process is the same as that of Example 1.

[0083] Comparative Example 4

[0084] The difference between this comparative example and Example 1 is that the addition amount of trivalent dopant ions is adjusted to 90g aluminum nitrate nonahydrate and 90g gallium chloride, that is, the molar ratio of dopant to metal oxide is 1:16.35, and the rest of the preparation process is the same as Example 1 to obtain an antistatic phase change radiator.

[0085] Comparative Example 5

[0086] The difference between this comparative example and Example 1 is that the addition amount of trivalent dopant ions is adjusted to 10g aluminum nitrate nonahydrate and 10g gallium chloride, that is, the molar ratio of dopant to metal oxide is 1:147, and the rest of the preparation process is the same as Example 1 to obtain an antistatic phase change radiator.

[0087] Comparative Example 6

[0088] The difference between this comparative example and Example 1 is that the method for preparing the conductive particles is adjusted, and the rest of the preparation process is the same as that of Example 1. Specifically:

[0089] Zinc sulfate heptahydrate and gallium chloride are prepared into a 1.5 mol / L mixed salt solution, and a coprecipitation reaction occurs under the action of 1.6 mol / L ammonium bicarbonate solution. The temperature of the reaction system is maintained at 40°C, the pH value is within the range of 6.5±0.1, and strong stirring is performed to generate a white precipitated basic zinc carbonate precursor. The reaction is aged for 1.0 h to complete the reaction. The precipitate is washed and separated and then dried at 60°C to obtain a white basic zinc carbonate precursor powder. The obtained precursor powder is then calcined in a hydrogen atmosphere to obtain a conductive powder. The calcination temperature is 500°C and the constant temperature time is 2.0 h.

[0090] The performance of the material prepared in the above embodiment was tested, and the comparison results with those in Example 1 are shown in Table 3.

[0091] Table 3

[0092]

[0093]

[0094] It can be seen from the above that the antistatic effect of ordinary phase change radiators is poor, and the heat dissipation is far behind that of the antistatic phase change radiator prepared by the present invention. Compared with the current conventional preparation scheme of conductive powder, the preparation of high whiteness conductive particles proposed by the present invention is simpler, and the particles have higher whiteness, and the prepared thermal control film or thermal control coating has higher solar reflectivity.

[0095] In summary, the anti-static phase change radiator prepared by the present invention is composed of a high-reflection and high-emission shell structure composed of an anti-static thermal control layer based on high-whiteness conductive particles and a composite phase change material core based on a porous foam structure. The anti-static phase change radiator prepared by the present invention has the characteristics of strong anti-static ability, heat collection, transmission and dissipation ability, short assembly cycle, simple construction, and large-area preparation, which can meet the anti-static and heat dissipation needs of high-orbit spacecraft.

[0096] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.

Claims

1. A method for preparing high whiteness conductive particles, Features: include, After two or more trivalent dopant ions and metal oxides are uniformly mixed, they are washed, dried, ground, and sintered at 100-400° C. for 1-6 hours in an inert atmosphere to prepare high-whiteness conductive particles.

2. The method for preparing high whiteness conductive particles according to claim 1, Features: The molar ratio of the trivalent dopant ions to the metal oxide is 1:20-100, and the inert atmosphere includes one or more of high-purity nitrogen, high-purity argon, and high-purity helium.

3. The method for preparing high whiteness conductive particles according to claim 1, Features: The trivalent dopant ions include one or more of aluminum ions, gallium ions, indium ions, tin ions or gadolinium ions; the metal oxides include oxides of Zn, Al, Zr, Mg and Y.

4. A high-whiteness conductive particle prepared by the preparation method according to any one of claims 1 to 3.

5. An antistatic thermal control coating prepared using the high whiteness conductive particles as claimed in claim 4, Features: include, The high whiteness conductive particles and the binder are uniformly mixed in a mass ratio of 2 to 4:1 and fully stirred to obtain an antistatic thermal control coating.

6. The method for preparing the antistatic thermal control coating according to claim 5, Features: The binder includes an organic binder or an inorganic binder; wherein the organic binder includes one or more of silicone resin, acrylic resin, fluorocarbon resin, and polyurethane; the inorganic binder includes one or more of potassium silicate, lithium silicate, sodium silicate, and aluminum dihydrogen phosphate.

7. An antistatic thermal control film prepared by using the high whiteness conductive particles as claimed in claim 4, Features: include, The high whiteness conductive particles and the high transparency crystalline polymer are fully mixed in a mass ratio of 1:1 to 4 to obtain hybrid particles; the hybrid particles are extruded to obtain an antistatic thermal control film; The highly transparent crystalline polymer includes one or more of polyurethane polymer particles, polytetrafluoroethylene polymer particles, 4-methylpentene polymer particles, thermoplastic elastomer particles, and polypropylene polymer particles.

8. An antistatic phase change radiator prepared using the antistatic thermal control coating as claimed in claim 5 or the antistatic thermal control film as claimed in claim 7.

9. A method for preparing an anti-static phase change radiator, Features: include, The porous foam is completely immersed in the phase change material to prepare a composite phase change material; An antistatic thermal control film is attached to the shell surface or an antistatic thermal control coating is sprayed or brushed onto the shell surface to form an antistatic thermal control layer on the shell surface; a composite phase change material is filled into the shell to obtain an antistatic phase change radiator.

10. The method for preparing the anti-static phase change radiator according to claim 9, Features: The porous foam includes one or more of carbon foam, copper foam, and aluminum foam; the phase change material includes one or more of paraffin, fatty acids, and polyols.