Adsorption type master batch, preparation method thereof and adsorption type biological membrane modified filler

By using masterbatches of high-content ammonia nitrogen adsorbent materials in sewage treatment and compacting and exhausting, the problems of low inorganic material content and difficulty in air discharge in traditional biofilm fillers are solved, and efficient and uniform sewage treatment effect and fillers are achieved. performance.

CN119081264APending Publication Date: 2024-12-06SDIC XINKAI WATER ENVIRONMENT INVESTMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411308271.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In the existing wastewater treatment, when traditional biofilm fillers are added with inorganic materials during the manufacturing process, the content is low and it is difficult to discharge internal and external air, which affects the integrity, uniformity and mechanical strength of the extruded filler, resulting in limited treatment effect.

Method used

By adding high-content ammonia nitrogen adsorption material during masterbatch preparation and compacting and exhausting during melt extrusion, an adsorption masterbatch with a density of 1.00-1.05g/mL is prepared for high-performance adsorption The biofilm modified filler ensures high material content, uniform and compact structure, and simplifies the process flow.

Benefits of technology

It improves the mechanical strength, durability and treatment efficiency of the filler, reduces bubble content and voids, enhances molding quality and adhesion of biofilm, and significantly improves the sewage treatment effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081264A_ABST
    Figure CN119081264A_ABST
Patent Text Reader

Abstract

The adsorption type master batch comprises the following raw materials in parts by weight: 50-70 parts of polyolefin, 20-30 parts of an ammonia nitrogen adsorption material and 5-16 parts of an auxiliary material, polyolefin, which is a homopolymer selected from one of ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-octene and 4-methyl-1-pentene, or a copolymer of a combination of two or more of ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-octene and 4-methyl-1-pentene; the ammonia nitrogen adsorption material comprises molecular sieve powder, the particle size is higher than 300 meshes, and the water content is lower than 10%; the auxiliary material comprises polyolefin wax of which the melting point is higher than 100 DEG C; the adsorption type master batch is prepared through raw material melt extrusion, compaction exhaust and grain-sized dicing, the length of the master batch is 10-40 mm, the diameter is smaller than 6 mm, and the density is 1-1.05 g / mL. The adsorption type master batch and the biological membrane modified filler thereof have the advantages of high adsorption material content, uniform and compact structure, high efficiency, durability, simple and easy-to-control preparation process and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sewage treatment, and in particular to an adsorption-type masterbatch and a preparation method thereof, and an adsorption-type biofilm modified filler. Background Art

[0002] Moving bed biofilm reactors are increasingly being used in urban sewage treatment due to their low sludge production, the formation of dominant bacteria in each functional zone, and strong shock load. Biofilm fillers are the key materials of this process, providing a suitable space and environment for microbial attachment and growth.

[0003] Traditional biofilm fillers are made of pure polyethylene or polypropylene, which have no enrichment or promotion effect on functional microorganisms, resulting in limited treatment effects. Studies have shown that modified fillers, especially ammonia nitrogen adsorption fillers, have obvious enrichment and promotion effects on nitrifying bacteria, which can effectively improve the treatment effect.

[0004] Invention patent application CN117683315A discloses a method for preparing a masterbatch and an MBBR filler, wherein the masterbatch is obtained by mixing amino graphene, aminoanthraquinone and maleic anhydride grafted polyolefin, and then melt-extruding and granulating. The masterbatch, polyolefin and optional inorganic materials are then used as raw materials for melting, extruding and granulating to obtain an MBBR filler. The biofilm filler has good mechanical strength and wear resistance, as well as good sewage treatment effect. However, the invention adds inorganic materials when manufacturing the biofilm filler, and the content of the inorganic materials is low. The air adsorbed on the surface and inside of the inorganic materials is difficult to be discharged during the preparation process, which easily affects the integrity, uniformity and mechanical strength of the extruded filler.

[0005] Invention patent CN117720198B discloses a composite modified MBBR filler and its preparation method and application. The composite modified MBBR filler includes the following components by mass: 80-180 parts of HDPE, 1-8 parts of ferroferric oxide magnetic powder, 1-8 parts of PAM powder, 1-6 parts of amino-modified activated carbon powder, 1-5 parts of carboxyl-modified zeolite powder, 1-5 parts of calcium carbonate powder, 1-3 parts of silicone powder, and 1-3 parts of paraffin oil. Its preparation method includes:

[0006] S1. Put the raw materials into a mixer and stir to obtain a mixture; hot-melt granulate the mixture to obtain mixture particles;

[0007] S2, hot-melting the mixed material particles and then extruding them, cooling and shaping them, and then cutting them to obtain fillers;

[0008] S3, soaking the filler obtained by cutting in step S2 in an acid solution, rinsing and drying, and then magnetizing to obtain a composite modified MBBR filler.

[0009] Although this invention adds inorganic ingredients such as activated carbon powder, zeolite powder, and calcium carbonate powder when preparing the mixed material particles, and then hot-melt extrude the mixed material particles, the hot-melt granulation process does not have an exhaust step, resulting in a large amount of air in the mixed material particles. The hot-melt extruded filler will also have defects such as incompleteness and unevenness, resulting in insufficient comprehensive performance such as mechanical strength and durability.

[0010] It can be seen from the above that although modified fillers can improve the treatment effect, there are many problems in the current processing process, such as small amount of adsorption material added and many bubbles, long processing flow, difficult process control, and poor filler molding effect.

[0011] Therefore, it is an urgent problem to be solved by technicians in this field to provide an adsorption-type masterbatch and a preparation method thereof with high adsorption material content, uniform and compact structure, high efficiency and durability, and simple and easy-to-control preparation process, and use it to prepare high-quality adsorption-type biofilm modified fillers. Summary of the invention

[0012] In view of the defects existing in the above-mentioned prior art, the present invention provides an adsorption type masterbatch and a preparation method thereof and an adsorption type biofilm modified filler. By adding adsorption material during the masterbatch preparation process and compacting and venting the masterbatch, an adsorption type masterbatch with high adsorption material content and low gas content is obtained, and the masterbatch is used to prepare high-performance adsorption type biofilm modified fillers with high adsorption material content, uniform and compact structure, high efficiency and durability, and simple and easy-to-control preparation process.

[0013] In a first aspect, the present invention provides an adsorption-type masterbatch, wherein the raw materials thereof include, by weight:

[0014] Polyolefin 50-70 parts

[0015] 20-30 copies of ammonia nitrogen adsorption material

[0016] 5-16 parts of auxiliary materials

[0017] Polyolefin, a homopolymer of one selected from ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-octene and 4-methyl-1-pentene, or a copolymer of two or more thereof;

[0018] Ammonia nitrogen adsorption materials, including molecular sieve powder, with a particle size greater than 300 mesh and a moisture content less than 10%;

[0019] Auxiliary materials, including polyolefin waxes with a melting point above 100°C;

[0020] The adsorption type masterbatch is prepared by melt-extruding the raw materials, compacting and exhausting, and pelletizing, and the masterbatch density is 1.00-1.05 g / mL.

[0021] The content of ammonia nitrogen adsorption material in the adsorption masterbatch is preferably greater than 20% and less than 35wt%, providing an adsorption masterbatch with a high content of ammonia nitrogen adsorption material, which is beneficial for subsequent further processing to prepare high-performance adsorption biofilm modified fillers. However, too high ammonia nitrogen adsorption material content is not conducive to its uniform mixing in the masterbatch. In the compaction and exhaust stage, the exhaust is not thorough due to the large difference in force, and a large amount of adsorption material is distributed on the surface of the masterbatch. The subsequent molding process will bring in new gas, resulting in bubbles in the molded product being difficult to remove. Therefore, the present invention comprehensively considers the content of each component, and controls the density of the masterbatch to 1.00-1.05g / mL through compaction and exhaust and other means, and prepares the masterbatch as 10-40mm in length and less than 6mm in diameter as needed, which is more conducive to storage, transportation and subsequent molding processing.

[0022] The polyolefin is preferably polyethylene and / or polypropylene, more preferably high-density polyethylene.

[0023] The particle size of the molecular sieve powder is higher than 300 mesh, preferably higher than 500 mesh, and the moisture content is lower than 10%. If the moisture content is higher than 10%, it needs to be dried in advance.

[0024] The auxiliary materials, in addition to including polyolefin wax with a melting point higher than 100°C as a flux, may also include lubricants, such as zinc stearate, to ensure uniform mixing of the raw materials during stirring, reduce friction with the extruder, improve the quality of masterbatch output and reduce waste.

[0025] Preferably, the molecular sieve powder includes at least one of molecular sieve activated powder, natural zeolite or synthetic zeolite, with a specific surface area of ​​50m 2 / g to 500m 2 / g;

[0026] The molecular sieve powder includes at least one of unmodified molecular sieve powder, acid-modified molecular sieve powder, alkali-modified molecular sieve powder, and salt-modified molecular sieve powder, and optionally, high temperature combined modification is applied. Among them, the acid modification can be hydrochloric acid modification, and the salt modification includes salt modification using ferric chloride, sodium citrate, sodium metaaluminate, etc. It is preferred to use sodium hydroxide for alkali modification. For example, the alkali-modified molecular sieve powder is prepared by the following steps:

[0027] 1) Soak the molecular sieve powder in distilled water, ultrasonically treat for 1-3 hours, filter, and dry at 100-110°C;

[0028] 2) Soak the dried molecular sieve powder in a NaOH solution with a concentration of 1-2 mol / L, heating the solution at 70-90°C for 5-8 hours;

[0029] 3) microwave at 500-700 W for 1-3 min, and filter;

[0030] 4) Repeatedly washing the molecular sieve powder with distilled water, drying and crushing at 100-110°C after the filtrate is neutral, to obtain the alkali-modified molecular sieve powder with a particle size of more than 300 mesh, preferably more than 500 mesh, and a moisture content of less than 10%. Further, the modified molecular sieve powder is calcined at a high temperature of 200-400°C to obtain a high-performance molecular sieve powder. Due to the high-temperature combined modification treatment, the moisture and volatile components in the molecular sieve powder are better removed, and the amount of gas generated during subsequent molding is further reduced.

[0031] After modification with hydrochloric acid, sodium hydroxide or salts, the removal efficiency of molecular sieve powder for pollutants such as ammonia nitrogen can be significantly improved. These modification methods not only enhance the adsorption and ion exchange capacity and accelerate the biofilm formation speed, but also promote the enrichment of specific functional microorganisms such as ammonia oxidizing bacteria (AOB) and nitrifying bacteria, thereby improving the biological denitrification performance of the system. In addition, modified molecular sieve powder can also change the microbial community structure in the biofilm system and enrich specific microbial groups, such as heterotrophic nitrification-aerobic denitrification bacteria Acinetobacter, denitrifying bacteria Thauera and Zoogloea, etc. These microorganisms play a key role in sewage treatment. At the same time, the addition of modified molecular sieve powder will also affect the microbial biomass and enzyme activity in the filler, further improving the sewage treatment efficiency, showing the many benefits of using modified molecular sieve powder in biofilm systems.

[0032] In a second aspect, the present invention further provides a method for preparing the aforementioned adsorption-type masterbatch, comprising the following steps:

[0033] S1, melt extrusion: After the raw materials are stirred and mixed, they are melt extruded through a twin-screw extruder to obtain masterbatch strips, which are transported by a conveying mechanism;

[0034] S2, controlled cooling: using the first cooling mechanism to perform controlled cooling and pre-forming on the masterbatch strips on the conveying mechanism;

[0035] S3, compaction and exhaust: use the extrusion mechanism to extrude the predetermined masterbatch strips to expel air bubbles and obtain solid masterbatch strips;

[0036] S4, cooling and cutting: using the second cooling mechanism to cool the solid masterbatch strips, and then cutting them into pellets to obtain adsorption-type masterbatch.

[0037] Preferably, in step S1, the speed of the mixer for mixing the raw materials is 200-500 rpm. According to the selection of polyolefin materials, the twin-screw extruder adopts a multi-channel heating device to control the melting temperature of the extruder barrel in sections between 130-210°C, preferably between 140-200°C.

[0038] Preferably, the conveying mechanism includes a conveyor belt with a length greater than 10m. Along the running direction of the conveyor belt, the first cooling mechanism and the second cooling mechanism are respectively arranged upstream and downstream of the extrusion mechanism. The first cooling mechanism includes several fans and a first temperature monitor, and the second cooling mechanism includes several fans and a second temperature monitor.

[0039] Preferably, the first cooling mechanism cools the masterbatch strips to 70-80° C.; more preferably, the first cooling mechanism includes 4-8 cooling fans and 1-2 spare fans.

[0040] Among them, the first temperature monitor measures the temperature of the masterbatch strips cooled by each cooling fan and the standby fan:

[0041] When it is detected that the temperature of the masterbatch strip after passing through a cooling fan is lower than or equal to 75-80°C, the subsequent cooling fan and / or standby fan is not started;

[0042] When the masterbatch bar temperature is higher than 80℃ after passing the last cooling fan, the standby fan is started.

[0043] Preferably, the second cooling mechanism cools the masterbatch strips to below 40° C.; more preferably, the second cooling mechanism includes 1-5 cooling fans and a second temperature monitor.

[0044] The first cooling mechanism arranged along the running direction of the conveyor belt is used to cool the masterbatch strips entering the extrusion mechanism to 70-80°C so as to facilitate the effective and smooth implementation of the compaction and exhaust operation. If the temperature is too high, the pre-forming of the masterbatch strips is insufficient, and the compaction and exhaust operation will cause the masterbatch strips to deform seriously, and the extrusion force cannot be effectively applied to exhaust; if the temperature is too low, the masterbatch strips are cooled and shaped, and the gas is sealed in the masterbatch strips, making it difficult to exhaust by simple external extrusion. The second cooling mechanism downstream of the extrusion mechanism is used to quickly cool and shape the masterbatch strips that have been compacted and exhausted, so that the subsequent pelletizing process can be carried out smoothly. The spacing between the fans in the cooling mechanism is 0.5-1.5 meters along the running direction of the conveyor belt, preferably 0.8-1.2 meters.

[0045] On the basis of this empirical cooling range, the present invention sets a temperature monitor, and monitors and adjusts each step in the preparation method accordingly according to different raw material compositions and process conditions, as well as factors such as processing seasons. For example, a first temperature monitor is used to measure the temperature of the masterbatch strips cooled by each cooling fan and standby fan, and the activation or shutdown of the cooling fan and the standby fan is determined according to the temperature feedback of the masterbatch strips, so as to perform real-time precise regulation; the fan activation setting can also be performed in advance according to empirical data, for example, when the processing time is winter and the indoor temperature is slightly lower, the first cooling mechanism along the masterbatch strip conveyor belt only turns on cooling fans No. 1, 3, 5, and 7, and then turns off some cooling fans according to the monitoring results, and generally there is no need to turn on the standby fan, and the second cooling mechanism only turns on 1-2 cooling fans. When the processing time is summer, the indoor temperature is higher, and the number of cooling fans and standby fans can be increased accordingly according to the temperature monitoring results.

[0046] Preferably, the extrusion mechanism includes n groups of extrusion units, where 1≤n≤6, and each group of extrusion units has a pressure roller group and an adjusting spring. The pressure roller group includes a pressure roller An and a pressure roller Bn. The adjusting spring adjusts the distance between the pressure roller An and the pressure roller Bn so that the pressure roller An and the pressure roller Bn apply an extrusion effect perpendicular to the length direction of the pressure roller to the masterbatch strip, thereby squeezing out the bubbles in the masterbatch strip.

[0047] Preferably, the pressing rollers An and Bn of the n groups of pressing units are arranged in the horizontal direction; or the pressing mechanism includes at least two groups of pressing units, and the pressing rollers of each pressing unit are evenly arranged at an angle of 180° / n.

[0048] The present invention uses a roller group to extrude the masterbatch strip to discharge bubbles, which is a simple and easy-to-control exhaust method. The number and arrangement of the extrusion units are set according to the content of the adsorbent material, processing conditions, and filler product requirements. When one group of extrusion units is set, it can be arranged in the horizontal direction. The exhaust and normal transportation of the masterbatch strip can be guaranteed by the weight of the masterbatch strip and the clamping of the extrusion unit. When the exhaust requirement is increased, multiple groups of extrusion units can be set. For example, the roller groups of each extrusion unit are arranged in the horizontal direction to enhance the exhaust effect. It is particularly suitable for extruding multiple masterbatch strips at the same time. The masterbatch strips are transported forward in parallel along the conveyor belt. The roller groups of each extrusion unit can also be evenly arranged at a certain angle to enhance the compressed exhaust of the masterbatch strip from multiple angles. Optionally, conveying rollers are arranged between each extrusion unit and below the masterbatch strip to facilitate smooth transportation of the masterbatch strip and reduce deformation.

[0049] Preferably, an exhaust unit is provided in at least one of the extruder and the extrusion mechanism to further reduce the gas content in the masterbatch strips and improve the compaction uniformity. Specifically, an exhaust unit connected to the barrel can be provided in the extruder. The exhaust unit of the extrusion mechanism, for example, includes an exhaust hood in which the extrusion unit is accommodated and a suction machine connected to the exhaust hood, which reduces the air pressure in the exhaust hood and exhausts the gas faster in conjunction with the compaction operation of the extrusion unit.

[0050] Preferably, the adjustment spring is directly or indirectly arranged at at least one end of the pressure roller group, so that the deformation of the masterbatch strip passing through the pressure roller group in the extrusion direction is 1-10%. More preferably, the adjustment spring is designed to be installed at both ends of the pressure roller group. Such a layout can ensure that the pressure roller group obtains a more uniform and stable adjustment force during operation, thereby improving the overall adjustment accuracy and response speed.

[0051] As for the roller structure, they can be designed as standard cylindrical rollers or non-uniform rollers, for example, a concave arc cross-section is used in the middle of the roller to change the point contact of the extrusion force into surface contact. This design method can better control the deformation degree of the masterbatch strip when applying pressure. This concave arc cross-section can increase the contact and extrusion area between the roller and the masterbatch strip, and also help to improve the exhaust effect, avoiding the quality and uniformity of the masterbatch strip affected by gas accumulation.

[0052] In a third aspect, the present invention further provides an adsorption-type biofilm-modified filler, comprising the adsorption-type masterbatch, or the adsorption-type masterbatch prepared by the preparation method, wherein the raw materials of the adsorption-type biofilm-modified filler include, by weight:

[0053] Polyolefin 60-80 parts

[0054] Adsorption masterbatch 20-40 parts

[0055] Wherein, the weight percentage of ammonia nitrogen adsorption material is 5-12%;

[0056] The adsorption type biofilm modified filler is prepared by melt extrusion of the raw materials.

[0057] Due to the use of adsorption-type masterbatch with moderate adsorption material content, low gas content, and compactness and uniformity, the adsorption-type biofilm modified filler product of the present invention has a complete structure and uniform material, and is not prone to problems such as mold clogging, filler rib defect and fracture during the production process.

[0058] The present invention has at least the following beneficial effects:

[0059] (1) The present invention prepares an adsorption-type biofilm-modified filler by melt-extruding a masterbatch containing an ammonia nitrogen adsorption material and polyolefin, and the high-content molecular sieve powder can be evenly dispersed in the masterbatch and the biofilm-modified filler, while improving the adsorption performance of the filler and the adhesion of the biofilm.

[0060] (2) The preparation process of the masterbatch and biofilm modified filler of the present invention is simple. Only partial adjustments are made without replacing the original production line, and the bubbles and voids in the masterbatch can be significantly reduced, and the density and uniformity of the material can be improved. Not only the mechanical strength and durability of the masterbatch are enhanced, its fluidity and molding quality are improved, but also a good foundation is laid for the subsequent preparation of high-quality and high-performance biofilm modified fillers.

[0061] (3) The present invention is the key to reducing the bubble content of the masterbatch and improving the comprehensive performance of the masterbatch and biofilm modified filler, such as the compaction uniformity and structural integrity, by using cooling mechanism, extrusion mechanism and monitoring and control means to effectively control the pre-forming degree and compaction and exhaust effect, improve the yield rate and effectively reduce the cost, which has the value of promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0062] Figure 1 It is a flow chart of the method for preparing the adsorption type masterbatch of the present invention;

[0063] Figure 2 It is a schematic diagram of equipment for the controlled cooling, compaction and exhaust steps of one embodiment of the present invention;

[0064] Figure 3 This is a schematic diagram of the layout of the present invention using three groups of extrusion units;

[0065] Figure 4a This is a physical picture of the adsorption-type masterbatch according to an embodiment of the present invention;

[0066] Figure 4b This is a physical picture of the masterbatch of Comparative Example 1;

[0067] Figure 4c This is a physical picture of the masterbatch of Comparative Example 2;

[0068] Figure 4d This is a physical picture of the masterbatch of Comparative Example 3;

[0069] Figure 5a This is a physical picture of the adsorption-type biofilm modified filler according to an embodiment of the present invention;

[0070] Figure 5b This is a physical picture of the filler in Comparative Example 1.

[0071] Explanation of the reference numerals: 10 - masterbatch strip, 11 - conveyor belt, 12 - first cooling mechanism, 13 - second cooling mechanism 13, 121, 131 - cooling fan 121, 122 - standby fan 122, 14 - extrusion unit, 141 - pressure roller group 141, 142 - adjustment spring. DETAILED DESCRIPTION

[0072] In order to better understand the above technical solution, the above technical solution will be described in detail below in combination with the specification and specific implementation methods. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0073] The terms used in the embodiments of the present invention are only for the purpose of describing specific embodiments, and are not intended to limit the present invention. The singular forms "a", "said" and "the" used in the embodiments of the present invention and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings, and "multiple" generally includes at least two.

[0074] It should also be noted that the term "includes", "comprising" or any other variation thereof is intended to cover non-exclusive inclusion, so that a commodity or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such commodity or device. In the absence of more restrictions, the elements defined by the sentence "comprising a ..." do not exclude the existence of other identical elements in the commodity or device including the elements.

[0075] refer to Figure 4a The adsorption masterbatch of the present invention has a length of 10-40 mm, a diameter of less than 6 mm, and a density of 1-1.05 g / mL. The raw materials of the adsorption masterbatch include:

[0076] (1) 50-70 parts of a polyolefin, selected from a homopolymer of one of ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-octene and 4-methyl-1-pentene, or a copolymer of two or more thereof, preferably polyethylene or polypropylene, more preferably high-density polyethylene (HDPE);

[0077] (2) 20-30 parts of ammonia nitrogen adsorption material, with a particle size of more than 300 mesh, preferably more than 500 mesh, and a moisture content of less than 10%; the molecular sieve powder includes at least one of molecular sieve activation powder, natural zeolite or synthetic zeolite, with a specific surface area of ​​50m 2 / g to 500m 2 / g; the molecular sieve powder may be unmodified original powder, or may be subjected to at least one of acid modification, alkali modification and salt modification, and optionally, high temperature combined modification.

[0078] (3) 5-16 parts of auxiliary materials, including a polyolefin wax flux with a melting point higher than 100°C, and a zinc stearate lubricant.

[0079] The present invention provides a device for preparing an adsorption-type masterbatch, comprising:

[0080] (1) High-speed mixer, used for mixing raw materials of adsorption masterbatch;

[0081] (2) A twin-screw extruder is used to melt and extrude the mixed raw materials. Optionally, the twin-screw extruder uses a multi-channel heating device to control the barrel melting temperature in sections at 130-210° C., preferably 140-200° C.; the extruder barrel is connected to a vacuum unit to reduce the air pressure in the barrel, which is beneficial to the discharge of air and water vapor during the melting process of the raw materials, thereby improving the extrusion quality of the masterbatch strip 10;

[0082] (3) A conveying mechanism, used to receive the masterbatch strips 10 extruded by the extruder, including a conveyor belt 11 with a length greater than 10 m.

[0083] (4) A cooling mechanism is arranged along the running direction of the conveyor belt, comprising a first cooling mechanism 12 and a second cooling mechanism 13, wherein:

[0084] (4.1) A first cooling mechanism 12, comprising: 4-8 cooling fans 121, 1-2 standby fans 122 and a first temperature monitor (omitted), wherein the first temperature monitor measures the temperature of the masterbatch strip 10 cooled by each cooling fan 121 and the standby fan 122;

[0085] (4.2) The second cooling mechanism 13 includes: 1 to 5 cooling fans 131 and a second temperature monitor (omitted), wherein the second temperature monitor measures the temperature of the masterbatch strip 10 passing through each cooling fan 131 .

[0086] (5) An extrusion mechanism, which is arranged between the first cooling mechanism and the second cooling mechanism, and includes an extrusion unit 14 and an optional exhaust unit. Specifically, it includes n groups of extrusion units 14, where 1≤n≤6, and each group of extrusion units 14 has a pressure roller group 141 and an adjusting spring 142. The pressure roller group 141 includes a pressure roller An and a pressure roller Bn. The adjusting spring 142 adjusts the distance between the pressure roller An and the pressure roller Bn, so that the pressure roller An and the pressure roller Bn exert an extrusion effect on the masterbatch strip perpendicular to the length direction of the pressure roller, and the bubbles in the masterbatch strip 10 are squeezed out; the adjusting spring 142 is directly or indirectly arranged at at least one end of the pressure roller group 141, and the adjusting spring 142 is preferably respectively arranged at both ends of the pressure roller group 141. The pressure roller can be set as a cylindrical pressure roller, or a cross-sectional shape with a concave arc in the middle. Optional:

[0087] (5.1) The squeezing mechanism includes a squeezing unit 14 having a squeezing roller A1, a squeezing roller B1 and an adjusting spring 142. The squeezing roller A1 and the squeezing roller B1 are arranged in a horizontal direction (see Figure 2 );or

[0088] (5.2) The extrusion mechanism comprises n groups of extrusion units 14, n≥2, and the pressure rollers An and Bn of all the extrusion units are arranged in the horizontal direction to enhance the exhaust, which is particularly suitable for the simultaneous extrusion of multiple groups of masterbatch strips; or

[0089] (5.3) The extrusion mechanism comprises n groups of extrusion units 14, n ≥ 2, and the pressure roller groups 141 of each extrusion unit 14 are evenly arranged at an angle of 180° / n (when three groups of extrusion units are used, see Figure 3 ).

[0090] The air extraction unit comprises an air extraction hood for accommodating the extrusion unit therein and a suction machine connected to the air extraction hood.

[0091] (6) Pellet cutting mechanism: It is arranged downstream of the second cooling mechanism and is used to cut the masterbatch strips shaped after extrusion to obtain adsorption-type masterbatch products.

[0092] refer to Figure 1 , the preparation method of the above-mentioned adsorption masterbatch comprises the following steps:

[0093] S1. Melt extrusion: After the raw materials are stirred and mixed, they are melt-extruded through a twin-screw extruder to obtain masterbatch strips, which are transported by a conveying mechanism; wherein the speed of the mixer for stirring and mixing the raw materials is 200-500rpm; according to the selection of polyolefin materials, the twin-screw extruder adopts a multi-channel heating device to control the melting temperature of the extruder barrel in sections between 130-210°C, and preferably adopts a nine-channel heating device to control the temperature of the barrel in nine sections between 140-200°C, for example: the first section is 150-160°C, the second section is 160-180°C, the third section is 170-200°C, the fourth section is 165-190°C, the fifth section is 160-180°C, the sixth section is 165-185°C, the seventh section is 170-190°C, the eighth section is 175-200°C, and the ninth section is 140-150°C.

[0094] The conveying mechanism preferably comprises a conveyor belt having a length greater than 10 m.

[0095] S2, controlled cooling: the masterbatch strips on the conveying mechanism are subjected to controlled cooling and pre-forming by using the first cooling mechanism; the first cooling mechanism includes 4-8 cooling fans, 1-2 spare fans and a first temperature monitor, and cools the masterbatch strips to 70-80°C;

[0096] Among them, the first temperature monitor measures the temperature of the masterbatch strips cooled by each cooling fan and the standby fan, and performs real-time precise control:

[0097] (2.1) When it is detected that the temperature of the masterbatch strip after passing through a cooling fan is lower than or equal to 75-80°C, the subsequent cooling fan and / or standby fan is not started;

[0098] (2.2) When the masterbatch bar temperature is higher than 80°C after passing through the last cooling fan, start the standby fan.

[0099] In addition, the number and position of cooling fans to be started can be preset based on stored empirical data, such as seasonal changes and indoor problems, and then the first temperature detector can be used for real-time monitoring and regulation when necessary, which is simpler and more energy-saving.

[0100] S3, compaction and exhaust: use an extrusion mechanism to extrude and expel bubbles from the predetermined masterbatch strips to obtain solid masterbatch strips; the extrusion mechanism includes n groups of extrusion units, where 1≤n≤6, each group of extrusion units has a pressure roller group and an adjusting spring, the pressure roller group includes a pressure roller An and a pressure roller Bn, wherein the two pressure rollers can be set to be movable and adjustable, or one can be set to be fixed and the other movable and adjustable, the adjusting spring adjusts the distance between the pressure roller An and the pressure roller Bn, so that the pressure roller An and the pressure roller Bn exert an extrusion effect perpendicular to the length direction of the pressure roller on the masterbatch strip, and the bubbles in the masterbatch strip are squeezed out; the adjusting spring is directly or indirectly arranged at at least one end of the pressure roller group, preferably, adjusting springs are respectively arranged at both ends of the pressure roller group, so that the deformation of the masterbatch strip passing through the pressure roller group in the extrusion direction is 1-10%.

[0101] Specifically, the extrusion mechanism includes a group of extrusion units, including a pressure roller A1, a pressure roller B1 and an adjustment spring, and the pressure roller A1 and the pressure roller B1 are arranged in a horizontal direction. Figure 2 ; or the extrusion mechanism includes n groups of extrusion units 14, when n≥2, the pressure rollers An and Bn of all the extrusion units are arranged in the horizontal direction to strengthen the exhaust, which is particularly suitable for the simultaneous extrusion of multiple groups of masterbatch strips; or the extrusion mechanism includes at least 2 groups of extrusion units, and the pressure rollers of each extrusion unit are evenly arranged at an angle of 180° / n, reference Figure 3 .

[0102] S4, cooling and cutting: using the second cooling mechanism to cool the solid masterbatch strips, and then cutting them into pellets to obtain adsorption-type masterbatch; the second cooling mechanism includes 1-5 cooling fans and a second temperature monitor, which cools the masterbatch strips to below 40°C and feeds them into the pelletizing mechanism to obtain the adsorption-type masterbatch.

[0103] The above-mentioned adsorption masterbatch is further prepared into an adsorption biofilm modified filler product, referring to Figure 5a The filler has a clear and complete structure and uniform texture.

[0104] The raw materials of the adsorption-type biofilm modified filler include, by weight:

[0105] Polyolefin 60-80 parts

[0106] Adsorption masterbatch 20-40 parts;

[0107] Wherein, the weight percentage of ammonia nitrogen adsorption material is 5-12%;

[0108] The adsorption-type biofilm modified filler is prepared by melt extrusion of the raw materials. Among them, the polyolefin is preferably at least one of polyethylene and polypropylene, and more preferably high-density polyethylene (HDPE). Optionally, the above raw materials are fully dried and mixed, and a gas extraction unit connected to the barrel is provided in the extruder to prevent gas from mixing.

[0109] Example 1

[0110] The raw materials of the adsorption masterbatch of this embodiment include, by weight:

[0111] HDPE 60 parts

[0112] 30 copies of ammonia nitrogen adsorption material

[0113] 10 parts of high melting point polyethylene wax

[0114] The ammonia nitrogen adsorption material is molecular sieve activated powder, the particle size screening is about 500 mesh, and the specific surface area is 200m 2 / g to 350m 2 / g, and the moisture content is about 8%.

[0115] The adsorption masterbatch is prepared by melt extrusion, compaction and evacuation of the raw materials, and pelletization. The masterbatch length is 30 mm, the diameter is about 5 mm, the density is about 1.02 g / mL, and the masterbatch is regular and compact (see Figure 4a ).

[0116] The adsorption-type biofilm modified filler containing the above-mentioned adsorption-type masterbatch comprises, by weight, the following raw materials:

[0117] HDPE 70 parts

[0118] 30 parts of adsorption masterbatch;

[0119] Wherein, the weight percentage of ammonia nitrogen adsorption material is about 9.0%;

[0120] The adsorption-type biofilm modified filler is prepared by mixing its raw materials and then melt-extruding to prepare a 37-pore filler with a complete structure and a uniform and smooth filler wall (see Figure 5a ), the yield rate is above 96%. In order to facilitate statistical comparison, the yield rate of the present invention is obtained by randomly sampling 1000 adsorption-type biofilm modified fillers from the products made from the same batch of raw materials, and the ones with complete structures are regarded as finished products, that is:

[0121]

[0122] The adsorption-type masterbatch and the adsorption-type biofilm modified filler of this embodiment are prepared by the following steps:

[0123] S1, melt extrusion: the raw materials were stirred and mixed in a mixer with a rotation speed of 300 rpm, and then melt-extruded through a twin-screw extruder to obtain masterbatch strips. The extruder used a nine-way heating device to control the barrel temperature in nine sections as follows: the first section was 155°C, the second section was 170°C, the third section was 170°C, the fourth section was 170°C, the fifth section was 165°C, the sixth section was 165°C, the seventh section was 175°C, the eighth section was 150°C, and the ninth section was 140°C;

[0124] The masterbatch strips are transported by a conveyor belt with a length of about 15m.

[0125] S2. Controlled cooling: The masterbatch strips on the conveyor belt are controlled to be cooled and pre-shaped by the first cooling mechanism; the first cooling mechanism is provided with 8 cooling fans and 2 spare fans, with a fan spacing of 1 meter. When the room temperature is 20°C, cooling fans 1, 3, 5 and 7 can be started. At the same time, the first temperature monitor is used to measure the temperature of the masterbatch strips passing through the cooling fan. Once the temperature fluctuates greatly, the cooling setting is readjusted to stably cool the masterbatch strips to 75±2°C.

[0126] S3. Compacting and exhausting: Use an extrusion mechanism including a group of extrusion units to extrude the predetermined masterbatch strips to expel bubbles. The pressing roller A1 and the pressing roller B1 are arranged in the horizontal direction. By adjusting the adjustment springs at both ends of the pressing roller group, the deformation of the masterbatch strips passing through the pressing rollers A1 and B1 in the extrusion direction is set to about 8%, thereby obtaining solid masterbatch strips.

[0127] S4, cooling and cutting: Use the two cooling fans of the second cooling mechanism to cool the solid masterbatch strips to about 35°C, and then cut them into pellets to obtain adsorption-type masterbatch.

[0128] S5. Preparation of adsorption-type biofilm modified filler:

[0129] 5.1 Mix the raw materials of the adsorption type biofilm modified filler evenly;

[0130] 5.2 Add the uniformly mixed raw materials into a single screw extruder and melt extrude to prepare a 37-hole filler.

[0131] Example 2

[0132] The preparation process of the adsorption type masterbatch and the adsorption type biofilm modified filler in this embodiment is the same as that in Example 1, except that the raw material composition is different.

[0133] The raw materials of adsorption masterbatch, in parts by weight, include:

[0134] HDPE 70 parts

[0135] 20 copies of ammonia nitrogen adsorption material

[0136] 10 parts of high melting point polyethylene wax

[0137] The ammonia nitrogen adsorption material is molecular sieve activated powder, the particle size screening is about 500 mesh, and the specific surface area is 200m 2 / g to 350m 2 / g, and the moisture content is about 8%.

[0138] The adsorption type masterbatch is prepared by melt extrusion of the raw materials, compaction and degassing, and pelletizing. The masterbatch has a length of 30 mm, a diameter of about 5 mm, a density of about 1.00 g / mL, and is regular and compact.

[0139] The adsorption-type biofilm modified filler containing the above-mentioned adsorption-type masterbatch comprises, by weight, the following raw materials:

[0140] HDPE 75 parts

[0141] 25 parts of adsorption masterbatch;

[0142] Wherein, the weight percentage of ammonia nitrogen adsorption material is about 5%;

[0143] The adsorption-type biofilm modified filler is prepared by mixing its raw materials and then melt-extruding to prepare a 37-hole filler with a complete structure, a uniform and smooth filler wall, and a finished product rate of more than 97%.

[0144] Example 3

[0145] The preparation process of the adsorption type masterbatch and the adsorption type biofilm modified filler in this embodiment is the same as that in Example 1, except that the raw material composition is different.

[0146] The raw materials of adsorption masterbatch, in parts by weight, include:

[0147]

[0148] The ammonia nitrogen adsorption material is molecular sieve activated powder, the particle size screening is about 500 mesh, and the specific surface area is 200m 2 / g to 350m 2 / g, and the moisture content is about 8%.

[0149] The adsorption type masterbatch is prepared by melt extrusion of the raw materials, compaction and degassing, and pelletizing. The masterbatch has a length of 30 mm, a diameter of about 5 mm, a density of about 1.04 g / mL, and is regular and compact.

[0150] The adsorption-type biofilm modified filler containing the above-mentioned adsorption-type masterbatch comprises, by weight, the following raw materials:

[0151] HDPE 65 parts

[0152] 35 parts of adsorption masterbatch;

[0153] Among them, the weight percentage of ammonia nitrogen adsorption material is about 11.0%;

[0154] The adsorption-type biofilm modified filler is prepared by mixing its raw materials and then melt-extruding to prepare a 37-hole filler with a complete structure, a uniform and smooth filler wall, and a finished product rate of more than 95%.

[0155] Example 4

[0156] The raw material ratio and preparation process of the adsorption type masterbatch and adsorption type biofilm modified filler in this embodiment are the same as those in Example 1, except that natural zeolite powder is used, the particle size screening is about 500 mesh, and the specific surface area is 300m 2 / g to 400m 2 / g, the moisture content is about 8%. The adsorption masterbatch and adsorption biofilm modified filler have uniform and compact texture, high quality, and the finished product rate is above 96%.

[0157] Example 5

[0158] The raw material ratio and preparation process of the adsorption-type masterbatch and adsorption-type biofilm modified filler of this embodiment are the same as those of Example 1, except that the zeolite powder is subjected to high-temperature combined alkali modification treatment to make its moisture content about 1%.

[0159] The alkali-modified molecular sieve activated powder is prepared by the following steps:

[0160] 1) The molecular sieve activated powder was ultrasonically treated in distilled water for 1.5 h, filtered, and dried at 105 °C;

[0161] 2) Soak the dried molecular sieve activation powder in a 1.5 mol / L NaOH solution at 80°C for 6 h;

[0162] 3) microwave at 600 W for 2 min and filter;

[0163] 4) Repeatedly washing the molecular sieve activation powder with distilled water, drying at 105°C after the filtrate is neutral, crushing, and screening to obtain the alkali-modified molecular sieve activation powder with a particle size of about 500 mesh and a moisture content of about 8%. The modified molecular sieve activation powder is calcined at 350°C to obtain a high-performance molecular sieve activation powder with a moisture content of about 1%.

[0164] The adsorption type masterbatch and adsorption type biofilm modified filler prepared from the above raw materials have uniform and compact texture, high quality and a finished product rate of more than 98%.

[0165] Example 6

[0166] The raw material composition ratio and preparation steps of the adsorption-type masterbatch and the adsorption-type biofilm modified filler in this embodiment are the same as those in Example 1, except that:

[0167] Step S3 compaction and exhaust: The extrusion mechanism of this embodiment includes 3 groups of extrusion units, and the pressure roller groups of each extrusion unit are evenly arranged at an angle of 60°. By adjusting the adjusting springs at both ends of the pressure roller groups, the deformation of the masterbatch strips passing through each pressure roller group in the extrusion direction is made to be about 5%, and solid masterbatch strips are obtained. The masterbatch is prepared by pelletizing. The masterbatch length is 30 mm, the diameter is about 5 mm, and the density is about 1.03 g / mL. Compared with Example 1 with the same composition, the masterbatch density is further improved, the masterbatch is regular and compact, and the adsorption-type biofilm modified filler prepared using the masterbatch has a uniform and compact texture, high quality, and a yield rate of more than 97%.

[0168] Comparative Example 1

[0169] The difference between this comparative example and Example 1 is that the method for preparing the masterbatch in Comparative Example 1 does not include a compaction and exhaust step, and the raw materials are prepared by melt extrusion and pelletizing. The masterbatch has a length of 30 mm, a diameter of about 5 mm, a density of about 0.988 g / mL, and is fluffy and has many bubbles (see Figure 4b ).

[0170] The 37-hole filler prepared by melt extrusion of the adsorption-type biofilm modified filler including the above masterbatch has an incomplete structure and a rough and incomplete filler wall (see Figure 5b ), the yield rate is less than 10%, and the die is blocked during the extrusion process and needs to be cleaned frequently, making continuous processing impossible.

[0171] Comparative Example 2

[0172] The difference between this comparative example and Example 1 is that in the preparation method of the masterbatch in Comparative Example 2, the temperature is lowered too low during the controlled cooling process.

[0173] S2, controlled cooling: The masterbatch strips on the conveyor belt are controlled to be cooled and pre-shaped by the first cooling mechanism; the first cooling mechanism is equipped with 8 cooling fans and 2 spare fans, with a fan spacing of 1 meter. When the room temperature is 20°C, all cooling fans are started to cool the masterbatch strips to 65±1°C, and then enter the compaction and exhaust step. Since the surface hardening degree of the masterbatch strips in comparative example 2 is higher than that in example 1, the pre-shaping is excessive, resulting in difficulty in the diffusion of internal bubbles, poor compaction and exhaust effect, and the masterbatch is relatively fluffy with a high bubble content (see Figure 4c ), the integrity and uniformity of the prepared biofilm modified filler are slightly better than those of Comparative Example 1, but are still insufficient compared to the other embodiments, with a yield rate of less than 80%.

[0174] Comparative Example 3

[0175] The raw material types and preparation processes of the adsorption type masterbatch and the adsorption type biofilm modified filler in this comparative example are the same as those in Example 1, except that the raw material ratios of the adsorption type masterbatch are different.

[0176] The raw materials of adsorption masterbatch, in parts by weight, include:

[0177] Polyethylene 47 parts

[0178] 35 copies of ammonia nitrogen adsorption material

[0179] 15 parts of high melting point polyethylene wax

[0180] The content of ammonia nitrogen adsorption material is about 36.1wt%;

[0181] The adsorption type masterbatch is prepared by melt extrusion of the raw materials, compaction and degassing, and pelletizing. The masterbatch has a length of 30 mm, a diameter of about 5 mm, and a density of about 1.06 g / mL.

[0182] The adsorption-type biofilm modified filler containing the above-mentioned adsorption-type masterbatch comprises, by weight, the following raw materials:

[0183] Polyolefin 60 parts

[0184] 30 parts of adsorption masterbatch;

[0185] Among them, the weight percentage of ammonia nitrogen adsorption material is about 11.6%;

[0186] The adsorption type biofilm modified filler is prepared by mixing its raw materials and then melt extruding it to prepare a 37-hole filler. Due to the high content of ammonia nitrogen adsorption material in the masterbatch, it is difficult to exhaust well during the melt mixing and compaction exhaust process, and the uniformity and smoothness of the masterbatch are poor (see Figure 4d ), the integrity and uniformity of the prepared biofilm modified filler are slightly better than those of comparative example 1, but are still insufficient compared to the various embodiments, with a yield rate of less than 50%, and the die is blocked during the extrusion process and needs to be cleaned frequently, making continuous processing impossible.

[0187] Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they are aware of the basic creative concepts. Therefore, the present invention is intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention. Obviously, those skilled in the art may make various changes and modifications to the present invention without departing from the spirit and scope of the present invention.

Claims

1. An adsorption type masterbatch, characterized in that: The raw materials include, by weight: Polyolefin 50-70 parts 20-30 copies of ammonia nitrogen adsorption material 5-16 parts of auxiliary materials Polyolefin, a homopolymer of one selected from ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-octene and 4-methyl-1-pentene, or a copolymer of two or more thereof; Ammonia nitrogen adsorption materials, including molecular sieve powder, with a particle size greater than 300 mesh and a moisture content less than 10%; Auxiliary materials, including polyolefin waxes with a melting point above 100°C; The adsorption type masterbatch is prepared by melt-extruding the raw materials, compacting and exhausting, and pelletizing, and the masterbatch density is 1.00-1.05 g / mL.

2. The adsorption type masterbatch according to claim 1, characterized in that: The molecular sieve powder includes at least one of molecular sieve activation powder, natural zeolite or synthetic zeolite, and has a specific surface area of ​​50 m 2 / g to 500m 2 / g; The molecular sieve powder includes at least one of unmodified molecular sieve powder, acid-modified molecular sieve powder, alkali-modified molecular sieve powder and salt-modified molecular sieve powder, and is optionally subjected to high temperature combined modification.

3. A method for preparing the adsorption-type masterbatch according to claim 1 or 2, characterized in that: The following steps are involved: S1, melt extrusion: After the raw materials are stirred and mixed, they are melt extruded through a twin-screw extruder to obtain masterbatch strips, which are transported by a conveying mechanism; S2, controlled cooling: using the first cooling mechanism to perform controlled cooling and pre-forming on the masterbatch strips on the conveying mechanism; S3, compaction and exhaust: use the extrusion mechanism to extrude the predetermined masterbatch strips to expel air bubbles and obtain solid masterbatch strips; S4, cooling and cutting: using the second cooling mechanism to cool the solid masterbatch strips, and then cutting them into pellets to obtain adsorption-type masterbatch.

4. The preparation method according to claim 3, characterized in that: The conveying mechanism includes a conveyor belt with a length greater than 10m. Along the running direction of the conveyor belt, the first cooling mechanism and the second cooling mechanism are respectively arranged upstream and downstream of the extrusion mechanism. The first cooling mechanism includes several fans and a first temperature monitor, and the second cooling mechanism includes several fans and a second temperature monitor.

5. The preparation method according to claim 4, characterized in that: The first cooling mechanism includes 4-8 cooling fans and 1-2 spare fans, which cool the masterbatch strips to 70-80℃; Among them, the first temperature monitor measures the temperature of the masterbatch strips cooled by each cooling fan and the standby fan: (1) When it is detected that the temperature of the masterbatch strip after passing through a cooling fan is lower than or equal to 75-80°C, the subsequent cooling fan and / or standby fan is not started; (2) When the temperature of the masterbatch bar is higher than 80°C after passing through the last cooling fan, start the standby fan.

6. The preparation method according to claim 4, characterized in that: The second cooling mechanism includes 1-5 cooling fans and a second temperature monitor to cool the masterbatch strips to below 40°C.

7. The preparation method according to any one of claims 3 to 6, characterized in that: The extrusion mechanism includes n groups of extrusion units, where 1≤n≤6, and each group of extrusion units has a pressure roller group and an adjusting spring. The pressure roller group includes a pressure roller An and a pressure roller Bn. The adjusting spring adjusts the distance between the pressure roller An and the pressure roller Bn, so that the pressure roller An and the pressure roller Bn exert an extrusion effect on the masterbatch strip perpendicular to the length direction of the pressure roller, thereby squeezing and discharging bubbles in the masterbatch strip.

8. The preparation method according to claim 7, characterized in that: The n groups of pressing rollers An and Bn of the pressing units are arranged in the horizontal direction; or The extrusion mechanism comprises at least two groups of extrusion units, and the pressure roller groups of each extrusion unit are evenly arranged at an angle of 180° / n.

9. The preparation method according to claim 8, characterized in that: The regulating spring is directly or indirectly arranged at least one end of the pressing roller group, so that the deformation amount of the masterbatch strip passing through the pressing roller group in the extrusion direction is 1-10%.

10. An adsorption-type biofilm modified filler, comprising the adsorption-type masterbatch according to claim 1 or 2, or the adsorption-type masterbatch prepared by the preparation method according to any one of claims 3 to 9, wherein the raw materials thereof include, by weight: Polyolefin 60-80 parts Adsorption masterbatch 20-40 parts Wherein, the weight percentage of ammonia nitrogen adsorption material is 5-12%; The adsorption type biofilm modified filler is prepared by melt extrusion of the raw materials.