Environment-friendly halogen-free modified expanded polystyrene as well as preparation method and application thereof

By coating bio-based charcoal-forming agents and flame retardants on the surface of foamed polystyrene particles, using materials such as polydopamine and calcium alginate, the problems of flammability and poor hydrophobicity of foamed polystyrene are solved, and environmentally friendly and halogen-free are prepared Modified foamed polystyrene improves its flame retardant properties and hydrophilicity, and is suitable for lightweight building materials.

CN119081304AInactive Publication Date: 2024-12-06LANZHOU JIAOTONG UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411219229.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing foamed polystyrene is flammable and has poor hydrophobicity in building insulation materials, and commonly used adhesives are harmful to human health, with large particle size limits of flame retardant, unpolymerized monomer residues and low impregnation efficiency.

Method used

Using polydopamine as the binder, the surface of foamed polystyrene particles is coated with bio-based charcoal and flame retardant through the coating method to prepare environmentally friendly halogen-free modified foamed polystyrene, using calcium alginate and hydrogen Environmentally friendly materials such as magnesium oxide improve their flame retardant and hydrophilicity.

Benefits of technology

Realize non-toxic, environmentally friendly, flame-retardant and hydrophilic modified foamed polystyrene particles, improve their application performance in lightweight building materials, enhance flame-retardant and hydrophilic properties, and reduce adhesives toxicity risk.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081304A_ABST
    Figure CN119081304A_ABST
Patent Text Reader

Abstract

The invention discloses environment-friendly halogen-free modified expanded polystyrene as well as a preparation method and application thereof. The modified expanded polystyrene is polydopamine modified expanded polystyrene of which the surface is coated with a bio-based carbon-forming agent and a flame retardant. Wherein the bio-based carbon forming agent is calcium alginate; the flame retardant is magnesium hydroxide. According to the invention, a polydopamine coating is used as an adhesive, and the surface of a polydopamine modified expanded polystyrene particle is coated with a bio-based charring agent and a flame retardant through a coating method, so that the environment-friendly halogen-free modified expanded polystyrene particle is synthesized, and the particle has the advantages of no toxicity, environment friendliness, flame retardance, hydrophilicity and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to modified expanded polystyrene, and in particular to environmentally friendly halogen-free modified expanded polystyrene and a preparation method and application thereof. Background Art

[0002] Building energy conservation is one of the effective ways to solve the problem of energy shortage in the future. A large part of building energy consumption is the heat energy consumption of the building's exterior walls. Building exterior wall insulation technology is to strengthen the insulation and heat insulation measures of the wall structure and carry out insulation treatment to reduce the heat energy consumption of the building. This technology is widely used in the fields of construction and roads and bridges.

[0003] There are many types of building insulation materials, among which expanded polystyrene (EPS) has a small volume density, low thermal conductivity, low price and low production cost, and is widely used in building insulation.

[0004] However, expanded polystyrene is a porous polyolefin foam material. Since its main chain is rich in hydrocarbons, there are many aromatic rings in the side chain, and the foam material itself has high porosity, large specific surface area and high air circulation, it is very easy to burn. In addition, due to its hydrophobicity, the low-density expanded polystyrene particles float in the slurry and are unevenly dispersed, making it difficult for the hydration products of the inorganic gelling material to penetrate. This poor combination between the expanded polystyrene particles and the matrix gelling material often makes the expanded polystyrene particles a weak point in the entire system, affecting the comprehensive performance of lightweight building materials. Therefore, when preparing lightweight building materials, it is necessary to take effective modification measures to improve the hydrophobicity and flame retardancy of the expanded polystyrene particles.

[0005] Adding flame retardants during the polymerization or impregnation process of expanded polystyrene is an effective method for obtaining flame-retardant expanded polystyrene. For example, in Chinese patent CN202310351196.8, a polymerized phosphatic nitrogen silicon flame retardant and a halogen-free polystyrene flame retardant masterbatch are disclosed in the application document, which uses a polymerized phosphatic nitrogen silicon flame retardant and a certain formula to obtain a halogen-free polystyrene flame retardant masterbatch through a twin-screw extruder; another example is Chinese patent CN201010018136.7, which discloses a flame-retardant polymer foam material and a preparation method thereof, which heats an organic flame retardant or an organic flame retardant mixture until the organic flame retardant melts and then attaches it to the surface of the polymer foam plastic by spraying, coating or impregnation to form an organic flame retardant layer, and finally obtains a flame-retardant polymer foam material. However, these methods have large restrictions on the particle size of the flame retardant, and there are problems such as residual unpolymerized monomers and low impregnation efficiency.

[0006] Due to the hydrophobicity of expanded polystyrene particles, flame retardant coating requires the use of adhesives on the surface of each pre-expanded polystyrene particle, and the flame retardant is coated on the pre-expanded polystyrene particles through physical bonding or chemical bonding, and flame retardant expanded polystyrene is prepared by secondary foaming. Usually, the coating of flame retardants has no effect on the foaming process. For example, Chinese patent CN201210550942.8 discloses a method for preparing a coated halogen-free flame retardant expanded polystyrene, which uses a phenolic resin or melamine resin containing a small amount of alkali metal silicate and a smoke suppressant as an adhesive, and prepares a coated halogen-free flame retardant expanded polystyrene by a coating method. However, the most commonly used adhesives for the coating method are thermosetting resins, such as phenolic resins and melamine formaldehyde resins, which usually contain formaldehyde and are harmful to human health. Therefore, it is crucial to choose an environmentally friendly, non-toxic, and flame-retardant adhesive. Summary of the invention

[0007] The purpose of the present invention is to provide an environmentally friendly halogen-free modified expanded polystyrene and a preparation method and application thereof, which solves the problem that the adhesive used in the existing coating method is harmful. A polydopamine coating is used as an adhesive, and a bio-based carbon-forming agent and a flame retardant are coated on the surface of polydopamine-modified expanded polystyrene particles through a coating method to synthesize environmentally friendly halogen-free modified expanded polystyrene particles. The particles have the advantages of being non-toxic, environmentally friendly, flame-retardant, hydrophilic, etc.

[0008] In order to achieve the above object, the present invention provides an environmentally friendly halogen-free modified foamed polystyrene, wherein the modified foamed polystyrene is a polydopamine-modified foamed polystyrene whose surface is coated with a bio-based carbon-forming agent and a flame retardant.

[0009] Preferably, the bio-based carbon former is calcium alginate; or / and the flame retardant is magnesium hydroxide.

[0010] Preferably, the magnesium hydroxide is hexagonal flaky magnesium hydroxide, and the flaky layers are stacked on each other to form a "card room" structure.

[0011] Preferably, the mass of the flame retardant is 20-40wt% of the mass of the bio-based carbon-forming agent matrix; and the bio-based carbon-forming agent matrix is ​​sodium alginate.

[0012] Another object of the present invention is to provide a method for preparing the environmentally friendly halogen-free modified foamed polystyrene, which comprises: adding a flame retardant metal oxide precursor whose mass after hydration is 20 to 40 wt% of the mass of the bio-based carbon-forming agent matrix to a bio-based carbon-forming agent matrix with a concentration of 1 to 3 wt%, uniformly dispersing, heating, and obtaining a flame retardant / bio-based carbon-forming agent mixed solution; uniformly dispersing polydopamine-modified foamed polystyrene in the flame retardant / bio-based carbon-forming agent mixed solution, coating, removing the solution, and drying to obtain flame retardant / bio-based carbon-forming agent modified foamed polystyrene particles; soaking the flame retardant / bio-based carbon-forming agent modified foamed polystyrene particles in a CaCl2 solution with a concentration of 1 to 3 wt%, removing the solution, and drying to obtain an environmentally friendly halogen-free modified foamed polystyrene.

[0013] Preferably, the mass ratio of the bio-based carbon-forming agent to the polydopamine-modified expanded polystyrene is (20-60):8.

[0014] Preferably, the heating temperature is 95°C.

[0015] More preferably, the heating time is 4 hours.

[0016] Preferably, the bio-based carbon former matrix is ​​sodium alginate.

[0017] Preferably, the flame retardant metal oxide precursor is magnesium oxide.

[0018] More preferably, the magnesium oxide is prepared by crushing magnesite, passing it through a 200 mesh sieve, and calcining it at 750° C. for 1 hour at a heating rate of 5° C. / min in a muffle furnace.

[0019] Preferably, after the coating is completed, the modified expanded polystyrene is fished out and placed on a filter screen, and allowed to stand at room temperature to filter out the solution.

[0020] Preferably, the preparation of the polydopamine-modified expanded polystyrene comprises: adding tris(hydroxymethyl)aminomethane to water, stirring evenly and adjusting the pH value of the solution to 8.5±0.5 to provide an alkaline environment for the self-polymerization of dopamine, then adding dopamine, mixing evenly, and obtaining a mixed solution containing dopamine; stirring expanded polystyrene in the mixed solution containing dopamine, then removing the reaction material, washing, and drying to obtain polydopamine-modified expanded polystyrene particles; wherein the mass ratio of tris(hydroxymethyl)aminomethane, dopamine, expanded polystyrene, and water is 1.21:4:8:1000.

[0021] Another object of the present invention is to provide application of the environmentally friendly halogen-free modified expanded polystyrene in lightweight building materials.

[0022] Another object of the present invention is to provide a lightweight building material, which comprises the following raw materials in parts by weight: 50 to 100 parts of a cementitious material and 10 to 50 parts of the environmentally friendly halogen-free modified expanded polystyrene.

[0023] Preferably, the cementitious material is selected from any one or more of geopolymer, gypsum, cement mortar and concrete.

[0024] Another object of the present invention is to provide a method for preparing the lightweight building material, which comprises: stirring and mixing the raw materials of the cementitious material and water, then adding the environmentally friendly halogen-free modified expanded polystyrene to the mixture, and increasing the stirring speed and continuing stirring to obtain a uniform slurry; then pouring the slurry into a mold, lightly vibrating the mold, curing, demolding and curing to obtain the lightweight building material.

[0025] Preferably, when the gelling material is a geopolymer, the raw materials are selected from metakaolin and an alkali activator.

[0026] Preferably, the raw materials of the gelling material and water are stirred and mixed for 1 minute.

[0027] Preferably, the stirring speed is increased and stirring is continued for 3 minutes.

[0028] Preferably, the stirring speed of the raw materials of the gelling material and water is 140±5 rpm / min.

[0029] Preferably, the rotation speed after adding the expanded polystyrene particles is 285±10 rpm / min.

[0030] The environmentally friendly halogen-free modified expanded polystyrene and the preparation method and application thereof of the present invention solve the problem that the adhesive used in the existing coating method is harmful and has the following advantages:

[0031] (1) The environmentally friendly halogen-free modified expanded polystyrene particles of the present invention have the advantages of being non-toxic, environmentally friendly, flame retardant, and hydrophilic. While modifying the expanded polystyrene particles to be flame retardant, improving their hydrophilicity is an important part of expanding the application of expanded polystyrene particles in the field of lightweight building materials;

[0032] (2) The adhesive used in the modified expanded polystyrene particles of the present invention is very different from the adhesive used in the past to coat the flame-retardant expandable polystyrene. In the past, most of the adhesives used were thermosetting resins, such as phenolic resins and melamine formaldehyde resins. The adhesive in the present invention is polydopamine, which has the advantages of being renewable, non-toxic, environmentally friendly, flame-retardant and hydrophilic. The prepared polydopamine-modified expanded polystyrene particles have good hydrophilicity and certain flame retardancy. At the same time, the polydopamine coating can be used as a fixing platform, and the flame retardant is fixed on the polydopamine-modified expanded polystyrene particles by a coating method.

[0033] (3) The environmentally friendly halogen-free modified expanded polystyrene particles of the present invention use environmentally friendly halogen-free bio-based charring agents and metal hydroxide flame retardants, which are environmentally friendly and non-toxic. At the same time, the hydrophilic groups (hydroxyl, carboxyl) in the bio-based charring agents and metal hydroxide flame retardants provide good hydrophilicity. Therefore, the bio-based charring agents and metal hydroxide flame retardants are fixed on the polydopamine modified expanded polystyrene particles by a coating method, which can improve the flame retardant properties and improve their hydrophilicity. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 The water contact angles of the unmodified expanded polystyrene of the present invention and the modified expanded polystyrene particles prepared in Examples 1 to 7.

[0035] Figure 2 This is a water resistance test of the modified expanded polystyrene particles prepared in Examples 1 to 7 of the present invention.

[0036] Figure 3 The thermogravimetric curves of the unmodified expanded polystyrene of the present invention and the modified expanded polystyrene particles prepared in Examples 1 to 7.

[0037] Figure 4 These are optical photographs of the unmodified expanded polystyrene of the present invention and the modified expanded polystyrene particles prepared in Examples 1 to 7 burning for 10 seconds under a butane torch.

[0038] Figure 5 It is a cross-sectional view of the lightweight geopolymer building material of the present invention.

[0039] Figure 6 It is the total heat release in the cone calorimetry test (CCT) of the lightweight geopolymer building material of the present invention.

[0040] Figure 7 It is the total smoke production in the cone calorimetry test (CCT) of the lightweight geopolymer building material of the present invention. DETAILED DESCRIPTION

[0041] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0042] The expanded polystyrene (EPS) used in the following examples and comparative examples is a commercially available product, wherein the particle size of the expanded polystyrene particles is 3 to 5 mm and the density is 11 kg / m 3; The density of expanded polystyrene foam board is 13kg / m 3 .

[0043] The main reagents used in the following examples and comparative examples include, but are not limited to, related products of the following companies, such as: dopamine hydrochloride (98%) from Aladdin Chemical Reagent Co., Ltd., tris(hydroxymethyl)aminomethane from Shanghai Zhongqin Chemical Reagent Co., Ltd., sodium alginate and anhydrous calcium chloride from Sinopharm Chemical Reagent Co., Ltd.

[0044] The magnesium oxide used in the following examples is made of magnesite provided by Yaodong Mining Import & Export (Dalian) Co., Ltd., which is crushed and passed through a 200-mesh sieve and calcined at 750°C for 1 hour in a muffle furnace at a heating rate of 5°C / min. The prepared magnesium oxide has an activity rate of 76.53%, and after hydration, it presents a typical hexagonal flake shape of magnesium hydroxide, and the flakes are stacked on each other to form a "card room" structure.

[0045] The metakaolin used in the following examples was purchased from Gongyi Chenyi Refractory Abrasive Co., Ltd., with a bulk density of 589.3 kg / m 3 , Al2O3 and SiO2 account for 91.97% of its composition.

[0046] The alkaline activator used in the following examples is prepared from water glass and 14 mol / L NaOH solution, and the modulus is 1.5. The water glass is provided by Gansu Yiyuan Industry and Trade Co., Ltd., and the modulus is 3.17.

[0047] Example 1

[0048] A polydopamine-modified expanded polystyrene particle, the preparation method of which comprises:

[0049] 1.21 g of tris(hydroxymethyl)aminomethane) was added to 1000 g of deionized water, and the mixture was stirred evenly. Hydrochloric acid was added to adjust the pH value of the solution to 8.5±0.5, and then 4 g of dopamine was added. The mixture was mixed evenly to obtain a mixed solution containing dopamine.

[0050] Then, 8 g of expanded polystyrene particles were stirred in the mixed solution containing dopamine for 24 hours, and then the reaction material was fished out, washed and dried to obtain polydopamine-modified expanded polystyrene particles.

[0051] Example 2

[0052] An environmentally friendly halogen-free modified expanded polystyrene, the preparation method of which comprises:

[0053] 20 g of sodium alginate was added to 2000 g of deionized water to prepare a sodium alginate solution with a concentration of 1 wt %, and 8 g of the polydopamine-modified expanded polystyrene particles prepared in Example 1 were added and uniformly dispersed, and mechanically stirred for 3 hours for coating. After being fished out, the modified expanded polystyrene particles were placed on a 60-mesh filter screen and allowed to stand at room temperature for 1 hour to filter out excess solution, and the sodium alginate-modified expanded polystyrene particles were obtained after drying;

[0054] 60 g of anhydrous calcium chloride was added to 2000 g of deionized water to prepare a 3 wt% CaCl2 solution, and the sodium alginate modified expanded polystyrene particles were immersed in the 3 wt% CaCl2 solution for 3 hours, and then dispersed and fished out. The particles were dried in an oven at 40°C to obtain environmentally friendly halogen-free modified expanded polystyrene particles modified with calcium alginate.

[0055] Example 3

[0056] The method is basically the same as Example 2, except that 40 g of sodium alginate is added to 2000 g of deionized water to prepare a 2 wt % sodium alginate solution, and the 2 wt % sodium alginate solution is used to prepare the environmentally friendly halogen-free modified expanded polystyrene particles modified with calcium alginate.

[0057] Example 4

[0058] The method is basically the same as Example 2, except that 60 g of sodium alginate is added to 2000 g of deionized water to prepare a 3 wt % sodium alginate solution, and the 3 wt % sodium alginate solution is used to prepare calcium alginate-modified environmentally friendly halogen-free modified expanded polystyrene particles.

[0059] Example 5

[0060] An environmentally friendly halogen-free modified expanded polystyrene, the preparation method of which comprises:

[0061] Prepare 2000g of 3wt% sodium alginate solution, add 8.28g of magnesium oxide and evenly disperse (8.28g of magnesium oxide is hydrated to generate 12g of magnesium hydroxide), heat the mixed solution in a 95°C water bath for 4 hours to obtain a magnesium hydroxide / sodium alginate solution in which the magnesium hydroxide content is 20% of the mass of the sodium alginate matrix;

[0062] 8 g of the polydopamine modified expanded polystyrene prepared in Example 1 was added to the above magnesium hydroxide / sodium alginate solution and uniformly dispersed, and mechanically stirred for 3 hours for coating. After being fished out, the modified expanded polystyrene particles were placed on a 60-mesh filter and allowed to stand at room temperature for 1 hour to filter out excess solution, and the magnesium hydroxide / sodium alginate modified expanded polystyrene particles were obtained after drying;

[0063] The magnesium hydroxide / sodium alginate modified expanded polystyrene particles were immersed in a 1wt% CaCl2 solution for 3 hours, dispersed and then fished out, and dried in an oven at 40°C to obtain magnesium hydroxide / calcium alginate modified environmentally friendly halogen-free expanded polystyrene particles.

[0064] Example 6

[0065] The method is basically the same as Example 5, except that the content of magnesium hydroxide is 30% of the mass of the sodium alginate matrix.

[0066] Example 7

[0067] The method is basically the same as Example 5, except that the content of magnesium hydroxide is 40% of the mass of the sodium alginate matrix.

[0068] The physical properties of the environmentally friendly halogen-free modified expanded polystyrene particles prepared in Examples 1 to 7 are shown in Table 1. By comparing the data of the coating efficiency and bulk density of Examples 1 to 7, it is shown that as the concentration of sodium alginate increases, the coating efficiency of the embodiments increases, and the high-concentration sodium alginate solution has a higher viscosity, which is conducive to adhesion on the surface of expanded polystyrene. However, if the concentration of sodium alginate is greater than 3wt%, the viscosity of the solution will be too high, and the modified expanded polystyrene particles after drying will adhere to each other and be difficult to separate. In addition, the introduction of magnesium hydroxide can improve the coating efficiency, but a high addition amount will affect the dispersibility of magnesium hydroxide and cause partial agglomeration.

[0069] Table 1 Physical properties of environmentally friendly halogen-free modified expanded polystyrene particles in the examples

[0070]

[0071]

[0072] Example 8

[0073] A lightweight building material, the preparation method of which comprises:

[0074] The metakaolin and the alkali activator were mixed at a low speed (140±5 r / min) for 1 min, and then the modified expanded polystyrene particles or unmodified expanded polystyrene of the above embodiments or comparative examples in different proportions were added to the mixture. The proportion of the lightweight building materials was shown in Table 2, and stirred at a high speed (285±10 r / min) for 3 min to obtain a uniform slurry;

[0075] Then, the slurry was poured into molds with dimensions of 40 mm × 40 mm × 40 mm and 100 mm × 100 mm × 20 mm, and placed on a vibration table for slight vibration molding. The specimen and the mold were sealed and left to stand in a standard curing box for 24 hours, then demolded and subjected to standard curing (humidity ≥ 95%, temperature (20 ± 0.5) ° C) until 28 days of age to obtain a lightweight geopolymer building material.

[0076] Table 2 Proportions of lightweight building materials

[0077]

[0078] Experimental Example 1 Contact Angle Test

[0079] According to the same method as in Examples 1 to 7, a 4 cm×4 cm×2 cm expanded polystyrene foam board was modified, and the water contact angle of the prepared modified expanded polystyrene foam board was tested by a contact angle meter (OCA25).

[0080] like Figure 1 As shown in FIG. 1 , the water contact angle test results of the modified expanded polystyrene board and the unmodified expanded polystyrene board prepared in Examples 1 to 7 of the present invention are shown in FIG. Figure 1 It can be seen that the water contact angle of unmodified expanded polystyrene is 105.8°, which has obvious hydrophobicity. After polydopamine is introduced on the surface of expanded polystyrene particles, the water contact angle of Example 1 is 22.2°, which has good hydrophilicity, indicating that the polydopamine coating containing hydrophilic groups (hydroxyl and amino groups) is successfully coated on the surface of expanded polystyrene. When modified with 1wt% sodium alginate solution, the water contact angle of Example 2 is 20.6°, which is attributed to the hydrophilic groups (hydroxyl and carboxyl groups) in calcium alginate, which can increase the hydrophilicity of the coating. As the concentration of sodium alginate increases, a dense calcium alginate film will form on the surface, resulting in an increase in the degree of cross-linking and a decrease in hydrophilic groups, which makes it difficult for water molecules to penetrate, resulting in an increase in the water contact angle. As the proportion of magnesium hydroxide in the sodium alginate matrix increases, the water contact angle of the embodiment gradually decreases, and the water contact angles of the samples of Example 5 and Example 6 are reduced to 36.2° and 22.8°, respectively, which indicates that magnesium hydroxide containing a large amount of hydroxyl groups (-OH, Mg-OH) can increase the hydrophilicity of the embodiment. However, when the proportion of magnesium hydroxide in the sodium alginate matrix is ​​40wt%, the water contact angle of the modified expanded polystyrene sample is increased to 26.4°. This is attributed to the partial agglomeration of magnesium hydroxide when the addition amount is too large, resulting in a decrease in the hydroxyl groups contained on the surface of the expanded polystyrene, and the water contact angle is reduced.

[0081] Experimental Example 2 Water resistance test

[0082] The modified expanded polystyrene particles prepared in Examples 1 to 7 were stirred and washed in tap water for several times, and the mass changes before and after were recorded to evaluate their water resistance.

[0083] like Figure 2 As shown in FIG. 1 , the water resistance test results of the modified expanded polystyrene particles prepared in Examples 1 to 7 of the present invention are shown in FIG. Figure 2 It can be seen that all modified expanded polystyrenes showed a relatively obvious mass loss after the initial water washing. The mass of Example 1 decreased by 34.40% after multiple water washings, which was attributed to the higher content of hydrophilic groups in the polydopamine coating. However, the polydopamine coating deposited on the surface of the expanded polystyrene had good adhesion, which avoided greater mass loss. The mass loss of Example 2 was as high as 38.89% after the initial water washing, and a greater mass loss (58.85%) was caused after multiple water washings. This was attributed to the large number of hydrophilic groups (hydroxyl and carboxyl groups) contained in calcium alginate, and the hydrophilicity of the modified coating increased, resulting in a decrease in its water resistance. With the increase of calcium alginate content, the mass changes of Examples 3 and 4 were small after multiple water washings, and the mass loss was reduced to 23.28% and 18.82%, which was attributed to the increase in the degree of cross-linking of the modified coating, the formation of a dense calcium alginate film, and the reduction of surface hydrophilic groups, which made it difficult for water molecules to penetrate and the water resistance of the modified coating increased. Example 7 has the smallest mass loss (9.98%) and exhibits good water resistance, which indicates that the in-situ generated magnesium hydroxide is embedded and fixed in the calcium alginate coating, thereby improving the durability of the modified expanded polystyrene. With the increase of magnesium hydroxide content, the mass loss rate of the modified expanded polystyrene decreases after multiple washings, which is attributed to the decrease in the relative proportion of the calcium alginate matrix and the increase in the durability of the modified expanded polystyrene. Therefore, by using polydopamine as a binder, environmentally friendly halogen-free modified expanded polystyrene particles with good durability can be prepared.

[0084] Experimental Example 3 Thermogravimetric Analysis

[0085] The modified expanded polystyrene particles obtained in Examples 1 to 7 were subjected to thermogravimetric analysis by a thermogravimetric analyzer (TA TGA55). The test results are shown in Tables 3 and Figure 3 shown.

[0086] Table 3 Thermogravimetric results of modified expanded polystyrene particles in the examples

[0087]

[0088] From Table 3 and Figure 3 The thermogravimetric results and thermogravimetric curves of the unmodified expanded polystyrene and the modified expanded polystyrene prepared in Examples 1 to 7 show that the maximum thermal decomposition temperature (T max ) is 404℃, the maximum thermal decomposition rate (DTGmax ) is -1.88% / ℃, and there is almost no residual carbon (0.17wt%) until 800℃, which shows that the unmodified expanded polystyrene has almost no carbon-forming ability. After the polydopamine coating is introduced on the surface of the expanded polystyrene, the thermal stability of Example 1 is improved, and the temperature (T 10% ) and T max The temperature of DTG increased to 368℃ and 414℃ respectively. max The final carbon residue yield was -1.68% / ℃, and the final carbon residue yield was 1.11wt%. The presence of the polydopamine coating helps to capture the free carbon released by the expanded polystyrene during the combustion process, thereby promoting carbonization and preventing the expanded polystyrene from further pyrolysis. However, the thin polydopamine coating on the surface of the expanded polystyrene limits the improvement of thermal stability. DTG of Examples 2, 3 and 4 max The carbon residue yields were respectively reduced to -1.54% / ℃, -0.92% / ℃ and -0.77% / ℃, and the carbon residue yields were respectively increased to 7.09wt%, 10.1wt% and 12.15wt%. The calcium alginate that was thermally decomposed first formed carbon on the surface of the expanded polystyrene particles, forming a protective layer to inhibit the thermal decomposition of the expanded polystyrene. Example 4 has the highest calcium alginate coating efficiency, the strongest carbonization ability, the highest carbon residue yield, and DTG max Lower, better thermal stability. DTG of Examples 5, 6 and 7 max They dropped to -1.15% / ℃, -1.08% / ℃ and -0.94% / ℃ respectively, while T max The temperature of the magnesium hydroxide was reduced to 372 ℃, 363 ℃ and 351 ℃ respectively, which was attributed to the dehydration of magnesium hydroxide during thermal decomposition, absorption of a large amount of heat, generation of a large amount of water vapor to dilute the oxygen concentration around the expanded polystyrene, and inhibition of thermal decomposition of the expanded polystyrene. In addition, the residual carbon yield of Examples 5, 6 and 7 was reduced from 12.15wt% to 6.87wt%, 7.35wt% and 6.96wt% respectively, which was because the water vapor released by magnesium hydroxide during pyrolysis caused a greater mass loss.

[0089] Experimental Example 4 Flame retardant performance test

[0090] The flame retardant properties of the environmentally friendly halogen-free modified expanded polystyrene prepared in Examples 1 to 7 were tested by a butane spray gun. The test results are as follows: Figure 4 shown.

[0091] Depend on Figure 4From the optical photographs of the unmodified expanded polystyrene and the modified expanded polystyrene prepared in Examples 1 to 7 burning under a butane torch for 10 seconds, it can be seen that the honeycomb structure of the expanded polystyrene will shrink rapidly in the flame, causing the particles to melt and leave sticky residues, and burn rapidly at high temperatures. After the flame retardant modification, the flame spread speed of the examples during the combustion process is significantly slowed down, and with the increase of the flame retardant content, the improvement of the flame retardant performance is very obvious, especially in Examples 4 and 7, which were exposed to the flame of the butane torch for 10 seconds, and the flame basically did not spread. In summary, the environmentally friendly halogen-free modified expanded polystyrene particles prepared have good flame retardant properties.

[0092] Experimental Example 5 Uniformity Evaluation

[0093] The 40 mm×40 mm×40 mm lightweight building material prepared in Example 8 was cut into a cross section to evaluate the uniformity of the expanded polystyrene in the matrix cementitious material. The test results are as follows: Figure 5 shown.

[0094] Depend on Figure 5 From the cross-sectional diagram of the lightweight geopolymer building material, it can be seen that due to the hydrophobicity and low density of the expanded polystyrene particles, the unmodified expanded polystyrene particles will float severely, and the distribution in the geopolymer matrix is ​​obviously uneven and mainly concentrated in the upper part of the sample; while the hydrophilically modified expanded polystyrene particles are evenly distributed in the geopolymer matrix, which shows that the hydrophilic modification of the expanded polystyrene particles is effective.

[0095] Experimental Example 6 Cone Calorimetry Test

[0096] The 100 mm×100 mm×20 mm lightweight building material prepared in Example 8 was subjected to a cone calorimeter test (CCT) at 50 kW / m 2 The test was carried out under external heat flow, and the test results are shown in Table 4 and Figures 6-7 shown.

[0097] Table 4 Cone calorimetry test results of lightweight building materials in Example 8

[0098]

[0099] From Table 4 and Figure 6 The heat release of lightweight building materials shows that the maximum heat release (pHRR) of C1 containing Example 4 is 11.41 kW / m 2 , the total heat release (THR) is 7.19MJ / m 2 When the magnesium hydroxide content is 20% of the mass of the sodium alginate matrix, the pHRR and THR of M1 containing Example 5 are increased to 14.1 kW / m 2and 8.42MJ / m 2 , and there was a violent exotherm in the later stage of the test. This may be because the magnesium oxide layer formed fell off at high temperature, causing the expanded polystyrene at the bottom layer to be further pyrolyzed. Since the thermal decomposition of calcium alginate (above 210°C) occurred before magnesium hydroxide (above 320°C), the presence of magnesium hydroxide destroyed the integrity of the carbon layer, causing the expanded polystyrene to burn rapidly in the early stage, which was also confirmed by the TGA results. As the magnesium hydroxide content increased, the pHRR and THR of P5 containing Example 7 decreased to 6.06kW / m 2 and 1.94MJ / m 2 , which is only 53.11% and 26.98% of C1, and no large exothermic peak appeared in the later stage of the test. This is attributed to the higher magnesium hydroxide content, which increases the heat absorbed by magnesium hydroxide during thermal decomposition and the release of water vapor; while reducing the oxygen concentration around the expanded polystyrene and playing a gas phase flame retardant role, the magnesium oxide fire-resistant protective layer covering the surface of the expanded polystyrene also plays a condensed phase flame retardant role, inhibiting the thermal decomposition process of the expanded polystyrene.

[0100] From Table 4 and Figure 7 The total smoke production of lightweight building materials shows that the total smoke production (TSP) of C1 is 0.64m 2 The introduction of magnesium hydroxide as a flame retardant can effectively reduce the TSP value of modified lightweight building materials. The TSP of P5 is reduced to 0.51m 2 Compared with C1, its TSP value decreased by 17.74%. This is mainly because magnesium hydroxide, as a flame retardant, inhibits the thermal decomposition of expanded polystyrene. At the same time, the large amount of water vapor released by magnesium hydroxide during the thermal decomposition process dilutes the smoke generated by the combustion of expanded polystyrene; the formed magnesium oxide protective layer also reduces the generation and overflow of smoke.

[0101] These results indicate that the modification of expanded polystyrene particles with a magnesium hydroxide / calcium alginate composite flame retardant system can effectively improve the fire safety of lightweight geopolymer composites compared to calcium alginate alone.

[0102] Although the content of the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as a limitation of the present invention. After reading the above content, it will be apparent to those skilled in the art that various modifications and substitutions of the present invention will occur. Therefore, the protection scope of the present invention should be limited by the appended claims.

Claims

1. An environmentally friendly halogen-free modified expanded polystyrene, It is characterized in that The modified expanded polystyrene is polydopamine-modified expanded polystyrene whose surface is coated with a bio-based carbon-forming agent and a flame retardant.

2. The environmentally friendly halogen-free modified expanded polystyrene according to claim 1, It is characterized in that The bio-based carbon-forming agent is calcium alginate; or / and the flame retardant is magnesium hydroxide.

3. A method for preparing the environmentally friendly halogen-free modified expanded polystyrene as claimed in claim 1 or 2, It is characterized in that The method includes: Adding a flame retardant metal oxide precursor in a concentration of 20 to 40 wt % of the mass of the bio-based carbon former matrix after hydration to a bio-based carbon former matrix with a concentration of 1 to 3 wt %, uniformly dispersing, and heating to obtain a flame retardant / bio-based carbon former mixed solution; The polydopamine modified expanded polystyrene particles are uniformly dispersed in the flame retardant / bio-based carbon forming agent mixed solution, coated, the solution is removed, and dried to obtain flame retardant / bio-based carbon forming agent modified expanded polystyrene particles; The flame retardant / bio-based carbon forming agent modified expanded polystyrene particles are added to a CaCl 2 The product is immersed in a solution, the solution is removed, and the product is dried to obtain environmentally friendly halogen-free modified expanded polystyrene.

4. The preparation method according to claim 3, It is characterized in that The heating temperature is 95°C.

5. The preparation method according to claim 3, It is characterized in that The flame retardant metal oxide precursor is magnesium oxide.

6. The preparation method according to claim 3, It is characterized in that The preparation of the polydopamine-modified expanded polystyrene comprises: Tris(hydroxymethyl)aminomethane) is mixed in water, stirred evenly and the pH value of the solution is adjusted to 8.5±0.5 to provide an alkaline environment for the self-polymerization of dopamine, and then dopamine is added and mixed evenly to obtain a mixed solution containing dopamine; Stirring the expanded polystyrene in the mixed solution containing dopamine, then taking out the reaction material, washing it, and drying it to obtain polydopamine-modified expanded polystyrene particles; Wherein, the mass ratio of tris(hydroxymethyl)aminomethane, dopamine, expanded polystyrene and water is 1.21:4:8:1000.

7. Use of the environmentally friendly halogen-free modified expanded polystyrene as claimed in claim 1 or 2 in lightweight building materials.

8. A lightweight building material, It is characterized in that The lightweight building material comprises the following raw materials in parts by weight: 50 to 100 parts of cementitious material, 10 to 50 parts of The environmentally friendly halogen-free modified expanded polystyrene as described in claim 1 or 2.

9. The lightweight building material according to claim 8, It is characterized in that The cementitious material is selected from any one or more of geopolymer, gypsum, cement mortar and concrete.

10. A method for preparing the lightweight building material according to claim 8 or 9, It is characterized in that The method includes: The raw materials of the gelling material and water are stirred and mixed, and then the environmentally friendly halogen-free modified expanded polystyrene is added to the mixture, and the stirring speed is increased and continued to be stirred to obtain a uniform slurry; The slurry is then poured into a mold, slightly vibrated to form, solidify, demould and cure to obtain a lightweight building material.

Citation Information

Patent Citations

  • Flame-retarding polymer foam material and preparation method thereof

    CN102127269B

  • Preparation method of coated halogen-free flame-retardant foamable polystyrene

    CN102977402A

  • Polymeric phosphorus-nitrogen-silicon flame retardant and halogen-free polystyrene flame-retardant master batch

    CN116376031A