Ultralow-density organic silicon sponge as well as preparation method and application thereof

Through the combination of modified silicone resin and graphene, the problem of excessive density of silicone sponges is solved, the mechanical properties and bactericidal ability are improved, and the preparation of ultra-low density sponges is realized, which is suitable for a variety of application scenarios.

CN119081423APending Publication Date: 2024-12-06WUHAN INSTITUTES OF ADVANCED TECHNOLOGY CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411446756.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-16
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The density of pure silicone sponges is too high, resulting in poor mechanical properties and cannot be used at low density.

Method used

Modified silicone resin, thiolated graphene, active hydrogen-capped polysiloxane and catalyst are used to enhance the molecular chain interaction force, improve the mechanical properties of the sponge, and achieve ultra-low density sponge through foaming agents. preparation.

Benefits of technology

The silicone sponge with a density of 50-100kg/m3 was successfully prepared, which has satisfactory mechanical properties, and the sterilization effect and compression permanent deformation ability are improved through the addition of graphene. It is suitable for clothing and furniture and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081423A_ABST
    Figure CN119081423A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of polymer foaming materials, in particular to ultralow-density organic silicon sponge and a preparation method thereof.The ultralow-density organic silicon sponge is prepared from modified organic silicon resin and thiolated graphene, the modified organic silicon resin is obtained by reaction of reactive hydrogen-terminated polysiloxane II, polybutadiene containing epoxy groups and hydroxyl acrylate. The organic silicon resin is modified, so that the intermolecular force of the organic silicon resin is enhanced, and the density of the organic silicon sponge can reach 50 kg / m < 3 > to the minimum and is far lower than that of common organic silicon sponge. In addition, thiolated graphene and organic silicon resin are compounded, so that the strength of the sponge can be further enhanced, the antibacterial capability of the sponge can be improved by utilizing the antibacterial and bactericidal capabilities of graphene, and the sponge can be applicable to the fields of clothing, furniture and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of polymer foaming materials, and in particular to an ultra-low density silicone sponge and a preparation method and application thereof. Background Art

[0002] Silicone foam materials have excellent heat resistance, weather resistance and biocompatibility. They will not change color, powder or yellow during long-term use. No solvents need to be added during the preparation of silicone foam materials, so there is no solvent residue and the VOC is almost zero. They are particularly suitable for use in clothing and home environments that are closely related to the human body.

[0003] Since the molecular polarity of silicone materials is weak, the interaction force between their molecular chains is low, and their molecular chains are highly flexible, and basically no crystalline phase is formed between the molecular chains. The above reasons lead to the poor mechanical properties of pure silicone materials, which cannot be compared with traditional resins. Since the mechanical properties of silicone foam materials are often poor, if the foaming ratio is too large and the sponge density is low, its mechanical properties will further decrease, making the prepared sponge unusable. Therefore, the density of pure silicone sponge is often greater than 100kg / m 3 , the density cannot be reduced any further. Summary of the invention

[0004] In order to solve the problem of too high density of silicone sponge in the prior art, the present application provides an ultra-low density silicone sponge, the raw materials of the silicone sponge include: modified silicone resin, thiol-modified graphene, active hydrogen-terminated polysiloxane I, inhibitor, catalyst I and foaming agent, wherein the modified silicone resin is obtained by reacting active hydrogen-terminated polysiloxane II, epoxy group-containing polybutadiene and hydroxy acrylate.

[0005] The density of the ultra-low density silicone sponge described in this application is 50-100 kg / m 3 , preferably 50-80kg / m 3 .

[0006] The present application uses polybutadiene and hydroxy acrylate containing epoxy groups to modify the silicone resin, thereby enhancing the polarity of the silicone resin, enhancing the interaction force between the molecular chains, and effectively improving the mechanical strength of the resin, so that the sponge prepared therefrom can still have satisfactory mechanical properties at a lower density, thus overcoming the problem of poor mechanical properties of silicone sponge at low density.

[0007] In a specific embodiment of the present application, the structural formula of the active hydrogen-terminated polysiloxane II is:

[0008] The range of n is 10-100.

[0009] In a specific embodiment of the present application, the polymerization degree of the active hydrogen-terminated polysiloxane II is 10-100, for example, 10, 20, 30, 40, 50, 60, 70, 80, 90, 100, etc.

[0010] In a specific embodiment of the present application, the content of active hydrogen in the active hydrogen-terminated polysiloxane II is 0.05-0.2 wt %.

[0011] In a specific embodiment of the present application, the number of epoxy groups in the epoxy group-containing polybutadiene is two or more, preferably, the number of epoxy groups is two, and further, the molecular weight of the epoxy group-containing polybutadiene is 500-2000, and its structural formula is:

[0012] The range of m is 5-35.

[0013] In a specific embodiment of the present application, the epoxy value of the epoxy group-containing polybutadiene is 0.1-0.5, such as 0.1, 0.2, 0.3, 0.4, 0.5, etc.

[0014] In a specific embodiment of the present application, the structural formula of the hydroxy acrylate is:

[0015]

[0016] R 1 CH 3 or -H,R 2 It is ethyl or propyl.

[0017] That is to say, in a specific embodiment of the present application, the hydroxy acrylate is selected from at least one of hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate and hydroxypropyl methacrylate.

[0018] In the present application, the structural formula of the modified silicone resin is:

[0019]

[0020] , where n ranges from 10 to 100, m ranges from 5 to 35, and R 1 CH 3 or -H,R 2 It is ethyl or propyl.

[0021] In the present application, the groups at both ends of the main chain of the modified silicone resin are active hydrogen and vinyl, respectively, and the molecular chain also contains carbon-carbon chain segments with relatively high regularity. The vinyl in the modified silicone resin reacts with the active hydrogen in the active hydrogen-terminated polysiloxane I and the hydroxyl group in the foaming agent to generate hydrogen to achieve foaming.

[0022] In the present application, the reaction process for synthesizing the modified silicone resin is:

[0023]

[0024] In a specific embodiment of the present application, the thickness of the thiol-modified graphene is 1-10 nm, for example, 1 nm, 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, etc.

[0025] In a specific embodiment of the present application, the sheet diameter of the thiol-modified graphene is 0.5-10 μm, for example, 0.5 μm, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, etc.

[0026] In a specific embodiment of the present application, the thiol content of the thiol-modified graphene is 0.1-1wt%, for example, 0.1wt%, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt%, 1wt%, etc.

[0027] In a specific embodiment of the present application, the raw materials of the silicone sponge include, by weight: 70-180 parts of modified silicone resin, 0.2-10 parts of thiol-modified graphene, 2-20 parts of active hydrogen-terminated polysiloxane I, 0.01-0.1 parts of inhibitor, 0.1-1 parts of catalyst I and 1-10 parts of foaming agent.

[0028] In a specific embodiment of the present application, the foaming agent is selected from at least one of monohydric alcohol, polyhydric alcohol, hydroxyl-terminated polysiloxane, and deionized water; preferably, the foaming agent is selected from at least one of hydroxy silicone oil, isopropyl alcohol, and glycerol.

[0029] On the other hand, the present application also provides a method for preparing the ultra-low density silicone foam, comprising the following steps:

[0030] 1) uniformly mixing the modified silicone resin, catalyst I, blowing agent and thiol-modified graphene to obtain material A;

[0031] 2) uniformly mixing the modified silicone resin, the active hydrogen-terminated polysiloxane I and the inhibitor to obtain material B;

[0032] 3) After material A and material B are uniformly mixed, the mixture is allowed to stand for foaming to obtain the ultra-low density silicone sponge.

[0033] In a specific embodiment of the present application, the catalyst I is a platinum catalyst.

[0034] In a specific embodiment of the present application, the inhibitor is an alkynol inhibitor.

[0035] In a specific embodiment of the present application, the material A further comprises 0.5 parts by weight of color paste.

[0036] In a specific embodiment of the present application, the content of active hydrogen in the active hydrogen-terminated polysiloxane I is 1-1.6 wt %.

[0037] In a specific embodiment of the present application, the method for preparing the ultra-low density silicone foam comprises the following steps:

[0038] 1) By weight, 50-100 parts of modified silicone resin, 0.1-1 parts of platinum catalyst I, 0.5 parts of color paste, 1-10 parts of foaming agent, and 0.2-10 parts of thiol graphene are uniformly mixed to obtain material A;

[0039] 2) uniformly mixing 20-80 parts of modified silicone resin, 2-20 parts of active hydrogen-terminated polysiloxane I, and 0.01-0.1 parts of acetylene alcohol inhibitor by weight to obtain material B;

[0040] 3) After material A and material B are uniformly mixed, the mixture is allowed to stand for foaming to obtain the ultra-low density silicone sponge.

[0041] Preferably, the amount of the modified silicone resin in step 1) is 50-70 parts.

[0042] Preferably, the amount of thiol-synthesized graphene in step 1) is 1-10 parts.

[0043] Preferably, the amount of the modified silicone resin in step 2) is 20-50 parts.

[0044] In a specific embodiment of the present application, the preparation method of the modified silicone resin includes: mixing active hydrogen-terminated polysiloxane II, epoxy-group-containing polybutadiene, hydroxy acrylate, organic solvent and catalyst II and heating them for reaction; after the reaction is completed, vacuum distillation, separation and purification are performed to obtain the modified silicone resin.

[0045] In a specific embodiment of the present application, the polymerization degree of the active hydrogen-terminated polysiloxane II is 10-100.

[0046] In a specific embodiment of the present application, the content of active hydrogen in the active hydrogen-terminated polysiloxane II is 0.05-0.2 wt %.

[0047] In a specific embodiment of the present application, the epoxy value of the epoxy group-containing polybutadiene is 0.1-0.5.

[0048] In a specific embodiment of the present application, the hydroxy acrylate is selected from at least one of hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate and hydroxypropyl methacrylate.

[0049] In a specific embodiment of the present application, the organic solvent is selected from at least one of toluene, ethyl acetate and butyl acetate.

[0050] In a specific embodiment of the present application, the catalyst II is selected from at least one of dibutyltin dilaurate, tetrabutyl titanate, and lead isooctanoate.

[0051] In a specific embodiment of the present application, the inhibitor is at least one of ethynyl cyclohexanol and 3,7,11-trimethyldodecyn-3-ol.

[0052] In a specific embodiment of the present application, the raw material dosage of the modified silicone resin is, by weight: 10-50 parts of active hydrogen-terminated polysiloxane II, 5-20 parts of epoxy group-containing polybutadiene, 1-20 parts of hydroxy acrylate, 100-500 parts of organic solvent, and 0.01-0.1 parts of catalyst.

[0053] Preferably, the epoxy group-containing polybutadiene accounts for 5-10 parts.

[0054] In a specific embodiment of the present application, the heating reaction specifically includes: reflux reaction at 80-120° C. for 3-6 hours.

[0055] In a third aspect, the present application provides the application of the above-mentioned ultra-low density silicone sponge in the fields of clothing and furniture.

[0056] The present application adopts modified silicone resin to overcome the defect of insufficient mechanical strength of silicone resin. At the same time, the addition of thiol-modified graphene can not only further improve the mechanical properties of the sponge, but also give the sponge excellent bactericidal effect. The thiol group on the surface of graphene can effectively avoid the degradation of polysiloxane molecular chains and reduce the compression permanent deformation ability of the foam, so that it can be better used in clothing, furniture and other fields.

[0057] Beneficial effects:

[0058] 1. The present application adopts polybutadiene and hydroxy acrylate containing epoxy groups to modify silicone resin, thereby enhancing the polarity of silicone resin, enhancing the interaction force between molecular chains, and effectively improving the mechanical strength of the resin, so that the sponge prepared therefrom can still have satisfactory mechanical properties at a lower density, thus overcoming the problem of poor mechanical properties of silicone sponge at low density.

[0059] 2. The ultra-low density silicone sponge provided in the present application organically combines thiol-modified graphene and modified silicone resin, which can simultaneously exert the excellent reinforcement effect and bactericidal properties of graphene, so that the prepared silicone sponge has a strong bactericidal ability, and the thiol groups on the surface of graphene can effectively avoid the degradation of polysiloxane molecular chains, so that the compression permanent deformation ability of the foam is greatly reduced, and the foam maintains good elasticity for a long time, and can be widely used in clothing, furniture and other fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0060] Figure 1 This is a physical picture of the organosilicon sponge prepared in Example 1 of the present application;

[0061] Figure 2 This is a physical picture of the silicone sponge prepared in Comparative Example 1 of the present application. DETAILED DESCRIPTION

[0062] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0063] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0064] In this article, the terms "comprises", "comprising" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device that includes a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of more restrictions, an element defined by the sentence "comprising a ..." does not exclude the presence of other identical elements in the process, method, article or device that includes the element.

[0065] The present invention provides an ultra-low density silicone sponge to solve the problem that the density of the silicone sponge in the related art is lower than 100 kg / m 3 The problem of low strength and inability to inhibit bacteria.

[0066] The present invention provides a method for preparing an ultra-low density silicone sponge, comprising the following steps:

[0067] Step S101, in a four-necked flask equipped with a stirrer, a reflux condenser, a thermometer and a dropping funnel and filled with nitrogen, 10-50 parts of active hydrogen-terminated polysiloxane II with a degree of polymerization of 10-100, 5-20 parts of polybutadiene resin containing epoxy groups, 1-20 parts of hydroxy acrylate, 100-500 parts of organic solvent, and 0.01-0.1 parts of catalyst II are added respectively, and reflux reaction is carried out at 80-120° C. for 3-6 hours. After the reaction is completed, the organic solvent is removed by vacuum distillation, and the by-products are removed by column chromatography to obtain a modified silicone resin;

[0068] Step S102, preparing material A, uniformly mixing 50-100 parts of modified silicone resin, 0.1-1 parts of platinum catalyst, 0.5 parts of color paste, 1-10 parts of foaming agent, and 0.2-10 parts of thiol-modified graphene to obtain material A;

[0069] Step S103, preparing material B, uniformly mixing 30-80 parts of modified silicone resin, 2-20 parts of active hydrogen-terminated polysiloxane I, and 0.01-0.1 parts of acetylene alcohol inhibitor to form material B;

[0070] Step S104, foaming, after material A and material B are uniformly mixed, they are allowed to stand for foaming to obtain the ultra-low density silicone sponge.

[0071] In a specific embodiment of the present invention, thiol-modified graphene was purchased from Xi'an Qiyue Biotechnology Co., Ltd., active hydrogen-terminated polysiloxane II and active hydrogen-terminated polysiloxane I were both purchased from Ningbo Runhe High-tech Materials Technology Co., Ltd., and epoxy-group-containing polybutadiene resin was purchased from Wuhan Kemik Biomedicine Technology Co., Ltd.

[0072] The present invention is further described in detail below through specific examples.

[0073] Example 1

[0074] This embodiment provides a method for preparing an ultra-low density silicone sponge, comprising the following steps:

[0075] Step S101, in a four-necked flask equipped with a stirrer, a reflux condenser, a thermometer and a dropping funnel and filled with nitrogen, 10 parts of active hydrogen-terminated polysiloxane II with a degree of polymerization of 10, 5 parts of polybutadiene resin with an epoxy value of 0.5, 2 parts of hydroxyethyl acrylate, 100 parts of toluene solvent, and 0.02 parts of dibutyltin dilaurate are added respectively, and reflux reaction is carried out at 80° C. for 5 hours. After the reaction is completed, toluene is removed by reduced pressure distillation, and by-products are removed by column chromatography to obtain a modified silicone resin.

[0076] Step S102, preparing material A, uniformly mixing 70 parts of the modified silicone resin obtained in S101, 0.2 parts of a platinum catalyst, 0.5 parts of a color paste, 10 parts of hydroxyl silicone oil, and 1 part of a thiol-modified graphene having a thiol content of 1 wt%, as material A.

[0077] Step S103, preparing material B, uniformly mixing 30 parts of the modified silicone resin obtained in S101, 4 parts of active hydrogen-terminated polysiloxane I with an active hydrogen content of 1.6 wt%, and 0.02 parts of ethynyl cyclohexanol inhibitor to obtain material B.

[0078] Step S104, foaming, after material A and material B are uniformly mixed, they are allowed to stand for foaming to obtain the ultra-low density silicone sponge.

[0079] Comparative Example 1

[0080] The difference between this comparative example and Example 1 is that the modified silicone resin is replaced with an unmodified hydroxyl-terminated polysiloxane with a degree of polymerization of 50 of equal mass (purchased from Ningbo Runhe High-tech Materials Technology Co., Ltd.), and the rest of the process is the same as Example 1 to obtain a silicone sponge.

[0081] Comparative Example 2

[0082] The difference between this comparative example and Example 1 is that no thiolated graphene is added to the formula of this comparative example, and other substances and amounts are the same as those in Example 1, to obtain an organosilicon sponge.

[0083] Comparative Example 3

[0084] The difference between this comparative example and Example 1 is that graphene (not thiolated) is added to the formula of this comparative example, and other substances and amounts are the same as those in Example 1, to obtain an organosilicon sponge.

[0085] Example 2

[0086] This embodiment provides a method for preparing an ultra-low density silicone sponge, comprising the following steps:

[0087] Step S101, in a four-necked flask equipped with a stirrer, a reflux condenser, a thermometer and a dropping funnel and filled with nitrogen, 50 parts of active hydrogen-terminated polysiloxane II with a degree of polymerization of 50, 9 parts of polybutadiene resin with an epoxy value of 0.1, 10 parts of hydroxypropyl acrylate, 300 parts of ethyl acetate solvent, and 0.1 part of tetrabutyl titanate are added respectively, and reflux reaction is carried out at 120° C. for 3 hours. After the reaction is completed, ethyl acetate is removed by reduced pressure distillation, and by-products are removed by column chromatography to obtain a modified silicone resin.

[0088] Step S102, preparing material A, uniformly mixing 50 parts of the modified silicone resin obtained in S101, 0.1 parts of a platinum catalyst, 0.5 parts of a color paste, 1 part of an isopropyl alcohol foaming agent, and 3 parts of thiol-modified graphene having a thiol content of 0.6 wt%, as material A.

[0089] Step S103, preparing material B, uniformly mixing 50 parts of the modified silicone resin obtained in S101, 20 parts of active hydrogen-terminated polysiloxane I with an active hydrogen content of 1 wt%, and 0.01 parts of 3,7,11-trimethyldodecyne-3-ol inhibitor as material B.

[0090] Step S104, foaming, after material A and material B are uniformly mixed, they are allowed to stand for foaming to obtain the ultra-low density silicone sponge.

[0091] Example 3

[0092] This embodiment provides a method for preparing an ultra-low density silicone sponge, comprising the following steps:

[0093] Step S101, in a four-necked flask equipped with a stirrer, a reflux condenser, a thermometer and a dropping funnel and filled with nitrogen, 30 parts of active hydrogen-terminated polysiloxane II with a degree of polymerization of 80, 10 parts of polybutadiene resin with an epoxy value of 0.2, 20 parts of hydroxyethyl methacrylate, 500 parts of butyl acetate solvent, and 0.01 parts of lead isooctanoate are added respectively, and reflux reaction is carried out at 100° C. for 5 hours. After the reaction is completed, butyl acetate is removed by reduced pressure distillation, and by-products are removed by column chromatography to obtain a modified silicone resin.

[0094] Step S102, preparing material A, uniformly mixing 60 parts of the modified silicone resin obtained in S101, 1 part of a platinum catalyst, 0.5 parts of a color paste, 6 parts of propylene glycol, and 10 parts of thiol-modified graphene with a thiol content of 0.15 wt%, as material A.

[0095] Step S103, preparing material B, uniformly mixing 20 parts of the modified silicone resin obtained in S101, 20 parts of active hydrogen-terminated polysiloxane I with an active hydrogen content of 1.2 wt%, and 0.1 parts of ethynyl cyclohexanol inhibitor as material B.

[0096] Step S104, foaming, after material A and material B are uniformly mixed, they are allowed to stand for foaming to obtain the ultra-low density silicone sponge.

[0097] The sponges prepared in the above embodiments and comparative examples were tested for performance:

[0098] (1) Apparent density test: Tested according to the method specified in ASTM D1056;

[0099] (2) Tensile property test: According to the method specified in standard ASTM D412, the specimen was cut into a dumbbell shape with a thickness of 5 mm and its tensile strength was tested.

[0100] (3) Compression set test: Tested according to the method specified in ASTM D1056;

[0101] (4) Antibacterial effect test: The five groups of samples were sterilized by ultraviolet radiation and then inoculated with Escherichia coli and Staphylococcus aureus at a concentration of 8.0*104 CFU / piece. The number of bacteria was tested after 30 minutes.

[0102] The performance test results are shown in Table 1.

[0103] Table 1

[0104]

[0105] It can be seen from Table 1 that the density of the sponges prepared in Comparative Example 1 and Examples 1-3 is similar, both less than 100 kg / m 3 , but the tensile strength of the sponge prepared by Examples 1-3 is significantly higher than that of Comparative Example 1, reflecting that the modified silicone resin used in this application can significantly improve the mechanical strength of the ultra-low density silicone sponge, avoiding the problem that the sponge cannot be used due to too low strength. From the comparison between Comparative Examples 2-3 and Examples 1-3, it can be seen that the number of bacteria in the sponge sample with the addition of thiol-treated graphene is significantly reduced, and the compression permanent deformation is significantly less than that of Comparative Example 2. In addition, the amount of graphene added in Example 3 is the largest, and the number of bacteria is the smallest, reflecting that the antibacterial ability of the sponge is significantly improved after adding graphene. From Comparative Example 3, it can be seen that the graphene is not thiolated, which increases the compression permanent deformation of the sponge and cannot maintain good elasticity, because the presence of thiol groups can effectively avoid the degradation of polysiloxane molecular chains, thereby reducing the compression permanent deformation ability of the sponge.

[0106] The specific embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0107] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0108] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. An ultra-low density silicone sponge, characterized in that: The raw materials of the organic silicone sponge include: modified organic silicone resin, mercaptolated graphene, active hydrogen-terminated polysiloxane I, inhibitor, catalyst I and foaming agent, wherein the modified organic silicone resin is obtained by reacting active hydrogen-terminated polysiloxane II, epoxy group-containing polybutadiene and hydroxy acrylate.

2. The ultra-low density silicone sponge according to claim 1, characterized in that: The structural formula of the active hydrogen-terminated polysiloxane II is: The range of n is 10-100; Preferably, the molecular weight of the epoxy group-containing polybutadiene is 500-2000, and its structural formula is: m ranges from 5 to 35; Preferably, the structural formula of the hydroxy acrylate is: R1 is CH3 or H, and R2 is ethyl or propyl.

3. The ultra-low density silicone sponge according to claim 1, characterized in that: The thickness of the thiol-modified graphene is 1-10 nm; Preferably, the sheet diameter of the thiol-synthesized graphene is 0.5-10 μm; Preferably, the thiol content of the thiol-modified graphene is 0.1-1 wt %.

4. The ultra-low density silicone sponge according to claim 1, characterized in that: The polymerization degree of the active hydrogen-terminated polysiloxane II is 10-100; Preferably, the active hydrogen content in the active hydrogen-terminated polysiloxane II is 0.05-0.2 wt %.

5. The ultra-low density silicone sponge according to claim 1, characterized in that: The epoxy value of the epoxy group-containing polybutadiene is 0.1-0.

5.

6. The ultra-low density silicone sponge according to claim 1, characterized in that: The foaming agent is selected from at least one of monohydric alcohol, polyhydric alcohol, hydroxyl-terminated polysiloxane and deionized water.

7. The ultra-low density silicone sponge according to claim 1, characterized in that: The raw materials of the organic silicone sponge include, by weight: 70-180 parts of modified organic silicone resin, 0.2-10 parts of thiol graphene, 2-20 parts of active hydrogen-terminated polysiloxane I, 0.01-0.1 parts of inhibitor, 0.1-1 parts of catalyst I and 1-10 parts of foaming agent.

8. The method for preparing the ultra-low density silicone sponge according to any one of claims 1 to 7, characterized in that: The following steps are involved: 1) uniformly mixing the modified silicone resin, catalyst I, blowing agent and thiol-modified graphene to obtain material A; 2) uniformly mixing the modified organic silicone resin, the active hydrogen-terminated polysiloxane I and the inhibitor to obtain material B; 3) After material A and material B are uniformly mixed, the mixture is allowed to stand for foaming to obtain the ultra-low density silicone sponge.

9. The preparation method according to claim 8, characterized in that: The preparation method of the modified silicone resin comprises: mixing active hydrogen-terminated polysiloxane II, epoxy-containing polybutadiene, hydroxy acrylate, organic solvent and catalyst II, and heating the mixture for reaction; after the reaction is completed, performing reduced pressure distillation, separation and purification to obtain the modified silicone resin.

10. Application of the ultra-low density silicone sponge according to any one of claims 1 to 7 in the fields of clothing and furniture.