Water-based sound insulation and noise reduction coating and preparation method thereof
By using a combination of acrylic IPN emulsion and a variety of fillers in noise reduction coatings, the problems of poor wear resistance and VOC pollution of existing coatings are solved, and high-efficiency sound insulation and low-pollution water-based sound insulation and noise reduction coatings are achieved.
Patent Information
- Application Number
- CN202411586477.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-08
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing noise reduction coatings have poor wear resistance after long-term use, resulting in a reduced noise isolation effect and contain high VOC substances, polluting the environment.
Based on the IPN acrylic emulsion, combined with damping fillers, flame retardants, additives, acrylic resins, vinyl chloride copolymer resins, tributyl phosphate, dioctyl phthalate, ethylene glycol, carboxymethyl cellulose , sodium hexametaphosphate, silica fine sand and sodium nitrite, water-based sound insulation and noise reduction coatings are prepared by stirring, pressurization, sterilization and drying, thereby improving the density and wear resistance of the coating.
It significantly improves the sound insulation effect and wear resistance of the paint, reduces VOC content, reduces environmental pollution, and enhances the adhesion and durability of the paint.
Smart Images

Figure CN119081490A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of water-based coatings, and in particular to a water-based sound insulation and noise reduction coating and a preparation method thereof. Background Art
[0002] Paint plays a protective role, and the addition of additives can impart different properties to the paint. Noise-reducing paint is a special type of paint designed to reduce the transmission of vibration and sound, thereby lowering noise levels. It effectively reduces noise caused by impact, vibration, or mechanical movement by absorbing and dissipating mechanical energy. This paint contains materials with high damping properties that convert sound energy into heat, thereby reducing the transmission of noise. The principle of noise-reducing paint is mainly based on its special physical and chemical properties. Some noise-reducing paints use nano-multilayered structural materials to sandwich the coating molecules in the middle, forming diaphragms with sound-insulating effects. These diaphragms can be evenly distributed, reducing the transmission of sound waves, thereby achieving the effect of sound absorption and sound insulation. Common noise-reducing paints, while improving the noise reduction effect, have poor wear resistance. After long-term use, the thickness of the paint often decreases, and the noise reduction effect becomes increasingly poor. To this end, we provide a water-based sound-insulating and noise-reducing paint and a preparation method thereof. Summary of the Invention
[0003] The purpose of the present invention is to solve the above technical problems and provide a water-based sound insulation and noise reduction coating and a preparation method thereof, which has the advantages of sound insulation and noise reduction effect, reduces VOC content, and increases coating thickness.
[0004] To achieve this purpose, the present invention provides a water-based sound insulation and noise reduction coating and a preparation method thereof, which adopts the following technical embodiments: A water-based sound insulation and noise reduction coating, which is mainly composed of acrylic IPN emulsion: the ingredients of the water-based sound insulation and noise reduction coating mainly include: 20-40 parts of acrylic IPN emulsion, 20-30 parts of damping pigments and fillers, 5-8 parts of flame retardants, 5-15 parts of additives, 15-25 parts of acrylic resin and vinyl chloride copolymer resin, 5-15 parts of tributyl phosphate and dioctyl phthalate, 10-25 parts of ethylene glycol, 5-15 parts of carboxymethyl cellulose and sodium hexametaphosphate, 10-20 parts of silica sand and sodium nitrite, and 30-40 parts of water; The damping pigments and fillers include epoxy resin, silicone resin and mica powder; The flame retardant is at least one of carbamate, phosphate and rigid chlorinated polystyrene; The auxiliary agent is at least one of N-methyl pyrrolidone and modified polyphenyl sulfide.
[0005] Preferably, the damping pigment and filler include the following components in parts by mass: 30-40 parts of epoxy resin, 20-30 parts of silicone resin, and 40-50 parts of mica powder.
[0006] Preferably, the preparation method of the damping pigment and filler comprises the following specific steps: S1: First, prepare weighed epoxy resin, silicone resin, and mica powder as synthetic materials; S2: Pour the epoxy resin and the silicone resin into a blender, and stir and mix them to ensure they are fully mixed; S3: Add mica powder to the thoroughly stirred mixture and stir again to ensure that it is thoroughly stirred; S4: After stirring evenly, a colloid is formed to obtain a damping pigment filler, and the filler is collected.
[0007] Preferably, in step S2, the stirring time of the epoxy resin and the silicone resin is 20 minutes, and the rotation speed of the stirring blade needs to be maintained at 1000 to 1200 revolutions per minute when the materials are stirred.
[0008] Preferably, in step S3, mica powder is added, the stirring time is 40 minutes, and the rotation speed of the stirring blade needs to be maintained at 1000 to 1200 revolutions per minute when the material is stirred.
[0009] A method for preparing a water-based sound insulation and noise reduction coating comprises the following steps: Step 1: Raw materials preparation includes: acrylic IPN emulsion, damping pigments and fillers, flame retardants, additives, acrylic resin and vinyl chloride copolymer resin, tributyl phosphate and dioctyl phthalate, ethylene glycol, carboxymethyl cellulose and sodium hexametaphosphate, silica sand and sodium nitrite, and water; Step 2: Mixing and emulsifying: Mix the acrylic IPN emulsion, damping pigments and fillers, additives, and water and stir until uniformly mixed to obtain a first mixture; Step 3: Pressurizing the first mixture obtained in step 2 to increase the roughness of the surface of the solid material; Step 4: After pressurizing in step 3, flame retardant, acrylic resin and vinyl chloride copolymer resin, tributyl phosphate and dioctyl phthalate, ethylene glycol, carboxymethyl cellulose and sodium hexametaphosphate, silica fine sand and sodium nitrite are added and stirred to obtain a second mixture; Step 5: sterilize the second mixture at high temperature, dry it, and then cool it to obtain a water-based sound insulation and noise reduction coating.
[0010] Preferably, in step 2 and step 4, the stirring temperature is 15-35° C., the stirring time is 1.5 h, and the stirring speed is 1500-2000 rpm.
[0011] Preferably, in step 3, the pressure of the pressurization treatment is 0.3-0.5 MPa, and the holding time is 120 minutes.
[0012] Preferably, in step 5, the high temperature sterilization temperature is 100-120° C. and the time is 10 minutes.
[0013] Preferably, in step 5, the drying temperature is 120-160° C., and the drying time is 2 hours.
[0014] The present invention has at least the following beneficial effects: The water-based sound insulation and noise reduction coating of the present invention adopts acrylic IPN emulsion as the main component and is mixed with damping pigments and fillers to improve sound insulation ability, reduce VOC content, reduce VOC emissions, reduce indoor air pollution, protect the atmospheric environment, prevent greenhouse gas emissions, and reduce the total emission of toxic substances in the production process; Damping pigments and fillers are made by mixing a variety of fillers to increase the thickness of water-based paint, increase the density between paints, reduce the sound transmission rate, and improve the overall sound insulation effect; Adding acrylic resin and vinyl chloride copolymer resin provides strength and durability to the coating, while also helping to improve the adhesion of the coating; Tributyl phosphate and dioctyl phthalate are added as plasticizers to improve the flexibility and impact resistance of the coating; Adding ethylene glycol helps improve the moisture retention and durability of the coating; While providing good sound insulation, silica fine sand and sodium nitrite are added to further enhance the wear resistance and corrosion resistance of the coating.
[0015] Other advantages, objectives and features of the present invention will be reflected in part from the following description and will be understood by those skilled in the art through study and practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 This is a comparison diagram of the noise reduction test of the water-based sound insulation and noise reduction coating prepared in Example 1 of the present invention; Figure 2 This is a comparative relationship diagram of the wear resistance of the water-based sound insulation and noise reduction coating prepared in Example 1 of the present invention; Figure 3 This is a comparison diagram of the noise reduction test of the water-based sound insulation and noise reduction coating prepared in Example 2 of the present invention; Figure 4 This is a comparative diagram of the wear resistance of the water-based sound insulation and noise reduction coating prepared in Example 2 of the present invention. DETAILED DESCRIPTION
[0017] In order to make the purpose, technical embodiments and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0018] The application principle of the present invention is described in detail below with reference to the accompanying drawings.
[0019] A water-based sound insulation and noise reduction coating, which is mainly composed of acrylic IPN emulsion: the ingredients of the water-based sound insulation and noise reduction coating mainly include: 20-40 parts of acrylic IPN emulsion, 20-30 parts of damping pigments and fillers, 5-8 parts of flame retardants, 5-15 parts of additives, 15-25 parts of acrylic resin and vinyl chloride copolymer resin, 5-15 parts of tributyl phosphate and dioctyl phthalate, 10-25 parts of ethylene glycol, 5-15 parts of carboxymethyl cellulose and sodium hexametaphosphate, 10-20 parts of silica sand and sodium nitrite, and 30-40 parts of water; Damping pigments and fillers include epoxy resin, silicone resin and mica powder; The flame retardant is at least one of carbamate, phosphate ester and rigid chlorinated polystyrene; The auxiliary agent is at least one of N-methyl pyrrolidone and modified polyphenyl sulfide.
[0020] The damping pigment and filler mentioned above include the following components in parts by mass: 30-40 parts of epoxy resin, 20-30 parts of silicone resin, and 40-50 parts of mica powder.
[0021] The preparation method of the damping pigment and filler comprises the following specific steps: S1: First, prepare weighed epoxy resin, silicone resin, and mica powder as synthetic materials; S2: Pour the epoxy resin and the silicone resin into a blender, and stir and mix them to ensure they are fully mixed; S3: Add mica powder to the thoroughly stirred mixture and stir again to ensure that it is thoroughly stirred; S4: After stirring evenly, a colloid is formed to obtain a damping pigment filler, and the filler is collected.
[0022] In step S2, the stirring time of the epoxy resin and the silicone resin is 20 minutes, and the rotation speed of the stirring blade needs to be maintained at 1000 to 1200 revolutions per minute when the materials are stirred.
[0023] In step S3, mica powder is added, the stirring time is 40 minutes, and the rotation speed of the stirring blade needs to be maintained at 1000 to 1200 revolutions per minute when the material is stirred.
[0024] A method for preparing a water-based sound insulation and noise reduction coating comprises the following steps: Step 1: Raw materials preparation includes: acrylic IPN emulsion, damping pigments and fillers, flame retardants, additives, acrylic resin and vinyl chloride copolymer resin, tributyl phosphate and dioctyl phthalate, ethylene glycol, carboxymethyl cellulose and sodium hexametaphosphate, silica sand and sodium nitrite, and water; Step 2: Mixing and emulsifying: Mix the acrylic IPN emulsion, damping pigments and fillers, additives, and water and stir until uniformly mixed to obtain a first mixture; Step 3: Pressurizing the first mixture obtained in step 2 to increase the roughness of the surface of the solid material; Step 4: After pressurizing in step 3, flame retardant, acrylic resin and vinyl chloride copolymer resin, tributyl phosphate and dioctyl phthalate, ethylene glycol, carboxymethyl cellulose and sodium hexametaphosphate, silica fine sand and sodium nitrite are added and stirred to obtain a second mixture; Step 5: sterilize the second mixture at high temperature, dry it, and then cool it to obtain a water-based sound insulation and noise reduction coating.
[0025] Wherein, in step 2 and step 4, the stirring temperature is 15-35° C., the stirring time is 1.5 h, and the stirring speed is 1500-2000 rpm.
[0026] Wherein, in step 3, the pressure of the pressurization treatment is 0.3-0.5 MPa, and the holding time is 120 minutes.
[0027] Wherein, in step 5, the high temperature sterilization temperature is 100-120°C and the time is 10 minutes.
[0028] Wherein, in step 5, the drying temperature is 120-160° C., and the drying time is 2 hours. Example 1
[0029] Water-based sound insulation and noise reduction coatings are mainly based on acrylic IPN emulsion: the main ingredients of water-based sound insulation and noise reduction coatings include: 30 parts of acrylic IPN emulsion, 25 parts of damping pigments and fillers, 6 parts of flame retardants, 5 parts of additives, 15 parts of acrylic resin and vinyl chloride copolymer resin, 10 parts of tributyl phosphate and dioctyl phthalate, 10 parts of ethylene glycol, 8 parts of carboxymethyl cellulose and sodium hexametaphosphate, 15 parts of silica sand and sodium nitrite, and 35 parts of water; Damping pigments and fillers include epoxy resin, silicone resin and mica powder; The flame retardant is at least one of carbamate, phosphate ester and rigid chlorinated polystyrene; The auxiliary agent is at least one of N-methyl pyrrolidone and modified polyphenyl sulfide.
[0030] The damping pigment and filler mentioned above include the following components in parts by mass: 30 parts of epoxy resin, 20 parts of silicone resin, and 50 parts of mica powder.
[0031] The preparation method of the damping pigment and filler comprises the following specific steps: S1: First, prepare weighed epoxy resin, silicone resin, and mica powder as synthetic materials; S2: Pour the epoxy resin and silicone resin into the blender and stir and mix them until they are fully and evenly mixed. The stirring time is 20 minutes, and the speed of the stirring blade needs to be maintained at 1000 to 1200 revolutions per minute. S3: Add mica powder to the thoroughly stirred mixture and stir again to ensure thorough mixing. The stirring time is 40 minutes. The speed of the stirring blade should be maintained at 1000 to 1200 revolutions per minute. S4: After stirring evenly, a colloid is formed to obtain a damping pigment filler, and the filler is collected.
[0032] A method for preparing a water-based sound insulation and noise reduction coating comprises the following steps: Step 1: Raw materials preparation includes: acrylic IPN emulsion, damping pigments and fillers, flame retardants, additives, acrylic resin and vinyl chloride copolymer resin, tributyl phosphate and dioctyl phthalate, ethylene glycol, carboxymethyl cellulose and sodium hexametaphosphate, silica sand and sodium nitrite, and water; Step 2: Mixing and emulsifying: Mix the acrylic IPN emulsion, damping pigments and fillers, additives, and water and stir at a temperature of 15-35°C for 1.5 hours at a speed of 1500-2000 rpm until uniformly mixed to obtain a first mixture. Step 3: The first mixture obtained in step 2 is subjected to a pressure treatment at a pressure of 0.3-0.5 MPa for 120 minutes to increase the roughness of the surface of the solid material; Step 4: After pressurizing in step 3, flame retardant, acrylic resin and vinyl chloride copolymer resin, tributyl phosphate and dioctyl phthalate, ethylene glycol, carboxymethyl cellulose and sodium hexametaphosphate, silica fine sand and sodium nitrite are added and stirred and mixed at a temperature of 15-35° C. for 1.5 hours at a stirring speed of 1500-2000 rpm, and the mixture is stirred to obtain a second mixture. Step 5: sterilize the second mixture at high temperature, and then dry it at a temperature of 120-160° C. for 2 hours. After cooling, a water-based sound insulation and noise reduction coating is obtained.
[0033] Experimental analysis shows that: Example 1 prepares a water-based sound insulation and noise reduction coating, which has good sound insulation and noise reduction effects and reduces the sound transmission intensity. In addition, Example 1 maintains high wear resistance at room temperature. The experiment uses different coatings on the same wall, conducts an impact test on the outside of the wall, and detects the decibel value on the inside of the wall. The specific noise reduction degree is compared. Figure 1 The wear resistance of the water-based sound insulation and noise reduction coating prepared in Example 1 has also been greatly improved. In the experiment, different coatings were applied to the same bricks, and the temperature was gradually increased. The specific wear resistance was compared with that of acrylic paint and polyurethane paint. Figure 2 shown.
[0034] The experimental data of Example 1 is compared with that of latex paint, see Table 1.
[0035] Table 1. Parameter analysis data for unpainted bricks, latex paint bricks, and paint bricks from Example 1. Experimental comparison Example 1 Bricks Unpainted bricks Latex paint bricks Noise reduction level high Low Low wear resistance high Low middle Example 2
[0036] Water-based sound insulation and noise reduction coatings are mainly based on acrylic IPN emulsion: the main ingredients of water-based sound insulation and noise reduction coatings include: 30 parts of acrylic IPN emulsion, 25 parts of damping pigments and fillers, 5 parts of flame retardants, 5 parts of additives, 15 parts of tributyl phosphate and dioctyl phthalate, 15 parts of ethylene glycol, 8 parts of carboxymethyl cellulose and sodium hexametaphosphate, and 35 parts of water; Damping pigments and fillers include epoxy resin, silicone resin and mica powder; The flame retardant is at least one of carbamate, phosphate ester and rigid chlorinated polystyrene; The auxiliary agent is at least one of N-methyl pyrrolidone and modified polyphenyl sulfide.
[0037] A method for preparing a water-based sound insulation and noise reduction coating comprises the following steps: Step 1: Raw materials preparation includes: acrylic IPN emulsion, damping pigments and fillers, flame retardants, additives, tributyl phosphate and dioctyl phthalate, ethylene glycol, carboxymethyl cellulose and sodium hexametaphosphate, and water; Step 2: Mixing and emulsifying: Mix the acrylic IPN emulsion, damping pigments and fillers, additives, and water and stir at a temperature of 15-35°C for 1.5 hours at a speed of 1500-2000 rpm until uniformly mixed to obtain a first mixture. Step 3: The first mixture obtained in step 2 is subjected to a pressure treatment at a pressure of 0.3-0.5 MPa for 120 minutes to increase the roughness of the surface of the solid material; Step 4: After pressurizing in step 3, flame retardant, tributyl phosphate, dioctyl phthalate, ethylene glycol, carboxymethyl cellulose, and sodium hexametaphosphate are added and stirred at a temperature of 15-35° C. for 1.5 hours at a speed of 1500-2000 rpm to obtain a second mixture. Step 5: sterilize the second mixture at high temperature, and then dry it at a temperature of 120-160° C. for 2 hours. After cooling, a water-based sound insulation and noise reduction coating is obtained.
[0038] Experimental analysis shows that: Example 2: Prepare water-based sound insulation and noise reduction coatings, which have good sound insulation and noise reduction effects and reduce the sound intensity on the other side of the coating. Use different coatings on the same wall to carry out impact tests on the outside of the wall and detect the decibel value on the inside of the wall. The specific noise reduction degree is compared. Figure 3 The wear resistance of the water-based sound insulation and noise reduction coating prepared in Example 2 was not improved. The experiment used the same bricks to apply different coatings and gradually increased the temperature. The specific wear resistance was compared with acrylic paint and polyurethane paint. Figure 4 shown.
[0039] The experimental data of Example 2 is compared with that of latex paint, see Table 2.
[0040] Table 2. Parameter analysis data for unpainted bricks, latex paint bricks, and paint bricks from Example 2. Experimental comparison Example 2 Bricks Unpainted bricks Latex paint bricks Noise reduction level high Low Low wear resistance middle Low middle The present invention discloses a water-based sound insulation and noise reduction coating and a preparation method thereof. The prepared water-based sound insulation and noise reduction coating has high sound insulation and noise reduction effect, high wear resistance, and durability. The coating mainly adopts an acrylic IPN emulsion and is mixed with damping pigments and fillers to improve sound insulation capability, reduce VOC content, reduce VOC emissions, reduce indoor air pollution, protect the atmospheric environment, prevent greenhouse gas emissions, and reduce the total emission of toxic substances in the production process. The coating is prepared by mixing multiple fillers to increase the thickness of the water-based coating, increase the density between coatings, reduce sound transmission rate, and improve the overall sound insulation effect. Acrylic resin and vinyl chloride copolymer resin are added to increase the strength and durability of the coating and also help improve the adhesion of the coating. Tributyl phosphate and dioctyl phthalate are added as plasticizers to improve the flexibility and impact resistance of the coating. Ethylene glycol is added to help improve the moisture retention and durability of the coating. Silica fine sand and sodium nitrite are added to further enhance the wear resistance and corrosion resistance of the coating while achieving good sound insulation effect. The above embodiments are only used to illustrate rather than limit the technical embodiments of the present invention. Relevant technicians in this field can make reasonable modifications or equivalent substitutions to the present invention, but any modifications and partial substitutions that do not depart from the spirit and scope of the present invention should be included in the scope of the claims of the present invention.
[0041] The contents not described in detail in this specification belong to the prior art known to professional and technical personnel in this field.
Claims
1. A water-based sound insulation and noise reduction coating, characterized in that: Water-based sound insulation and noise reduction coatings are mainly based on acrylic IPN emulsion: the ingredients of water-based sound insulation and noise reduction coatings mainly include: 20-40 parts of acrylic IPN emulsion, 20-30 parts of damping pigments and fillers, 5-8 parts of flame retardants, 5-15 parts of additives, 15-25 parts of acrylic resin and vinyl chloride copolymer resin, 5-15 parts of tributyl phosphate and dioctyl phthalate, 10-25 parts of ethylene glycol, 5-15 parts of carboxymethyl cellulose and sodium hexametaphosphate, 10-20 parts of silica fine sand and sodium nitrite, and 30-40 parts of water; The damping pigments and fillers include epoxy resin, silicone resin and mica powder; The flame retardant is at least one of carbamate, phosphate and hard chlorinated polystyrene; The auxiliary agent is at least one of N-methyl pyrrolidone and modified polyphenyl sulfide.
2. The water-based sound insulation and noise reduction coating according to claim 1, characterized in that: The damping pigment and filler mentioned above include the following components in parts by mass: 30-40 parts of epoxy resin, 20-30 parts of silicone resin, and 40-50 parts of mica powder.
3. The water-based sound insulation and noise reduction coating according to claim 2, characterized in that: The preparation method of the damping pigment filler comprises the following specific steps: S1: First, prepare weighed epoxy resin, silicone resin, and mica powder as synthetic materials; S2: introducing the epoxy resin and the silicone resin into a stirrer, and stirring and mixing them to make them fully and evenly stirred; S3: adding mica powder to the mixed liquid which is stirred evenly, and stirring again to make it evenly stirred; S4: After stirring evenly, a colloid is formed to obtain a damping color filler, and the filler is collected.
4. The water-based sound insulation and noise reduction coating according to claim 3, characterized in that: In step S2, the stirring time of the epoxy resin and the silicone resin is 20 minutes, and the rotation speed of the stirring blade needs to be maintained at 1000 to 1200 revolutions per minute when the materials are stirred.
5. The water-based sound insulation and noise reduction coating according to claim 3, characterized in that: In step S3, mica powder is added and the stirring time is 40 minutes. When the material is stirred, the rotation speed of the stirring blade needs to be maintained at 1000 to 1200 revolutions per minute.
6. The method for preparing a water-based sound insulation and noise reduction coating according to any one of claims 1 to 5, characterized in that: The method comprises the following preparation steps: Step 1: Raw materials preparation includes: acrylic IPN emulsion, damping pigment filler, flame retardant, additive, acrylic resin and vinyl chloride copolymer resin, tributyl phosphate and dioctyl phthalate, ethylene glycol, carboxymethyl cellulose and sodium hexametaphosphate, silica fine sand and sodium nitrite, water; Step 2: Mixing and emulsifying: Mix the acrylic IPN emulsion, damping pigment and filler, additives and water and stir until the mixture is uniformly mixed to obtain a first mixture; Step 3: subjecting the first mixture obtained in step 2 to a pressure treatment to increase the roughness of the surface of the solid material; Step 4: after the pressurization in step 3, flame retardant, acrylic resin and vinyl chloride copolymer resin, tributyl phosphate and dioctyl phthalate, ethylene glycol, carboxymethyl cellulose and sodium hexametaphosphate, silica fine sand and sodium nitrite are added and stirred and mixed, and the second mixture is obtained after stirring evenly; Step 5: sterilize the second mixture at high temperature, dry it, and obtain a water-based sound insulation and noise reduction coating after cooling.
7. The method for preparing a water-based sound insulation and noise reduction coating according to claim 6, characterized in that: In step 2 and step 4, the stirring temperature is 15-35° C., the stirring time is 1.5 h, and the stirring speed is 1500-2000 rpm.
8. The method for preparing a water-based sound insulation and noise reduction coating according to claim 6, characterized in that: In step 3, the pressure of the pressurization treatment is 0.3-0.5 MPa, and the holding time is 120 minutes.
9. The method for preparing a water-based sound insulation and noise reduction coating according to claim 6, characterized in that: In step 5, the high temperature sterilization temperature is 100-120°C and the time is 10 minutes.
10. The method for preparing a water-based sound insulation and noise reduction coating according to claim 6, characterized in that: In step 5, the drying temperature is 120-160° C., and the drying time is 2 h.
Citation Information
Patent Citations
Aquosity damping paint
CN1048224A
Water-based noise-reducing coating
CN105255284A
Sound-insulation heat-preservation fireproof plate as well as preparation method and application thereof
CN117602908A
Improvements in or relating to synthetic resin emulsions and their production and to surface coatings and vibration damping compositions derived therefrom
GB893816A
Damping water-borne coating composition
JP2005187514A