Composite material for tobacco raw material warehouse as well as preparation method and application of composite material
By modifying the composite material of polyurea resin and epoxy resin, the corrosion problem caused by phosphine in tobacco raw material warehouses is solved, the corrosion resistance of warehouse walls and security systems is improved, and the structural integrity and normal equipment of the warehouse are ensured. run.
Patent Information
- Application Number
- CN202411409434.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-10
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-10-10
AI Technical Summary
The wall corrosion and security system corrosion problems caused by tobacco raw material warehouses cannot be effectively solved by the existing technology, resulting in damage to the warehouse structure and equipment failure, affecting the quality and production safety of tobacco.
Using a composite material, including polyurea resin, modified epoxy resin, hydroxyapatite and silicon micropowder, the chemical resistance of the material is improved by the modification treatment and used for corrosion protection coatings for warehouse walls and security systems. .
It significantly improves the density and chemical corrosion resistance of warehouse walls, prevents phosphine penetration and circuit board corrosion, extends the service life of the equipment, and reduces maintenance costs and environmental pollution risks.
Smart Images

Figure BDA0005077588630000071 
Figure BDA0005077588630000081 
Figure BDA0005077588630000091
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of corrosion-resistant materials, and in particular to a composite material for a tobacco raw material warehouse and a preparation method and application thereof. Background Art
[0002] Tobacco raw material warehouses are special warehouses used by tobacco production enterprises to store tobacco raw materials. Each warehouse has a large storage volume of raw tobacco leaves and high tobacco value, which puts extremely high demands on the fire alarm system in the raw material warehouse. Since tobacco raw materials usually contain some microorganisms and pests and diseases, tobacco companies often carry out centralized disinfection and killing of microorganisms and pests and diseases left on tobacco raw materials in tobacco raw material warehouses.
[0003] As a broad-spectrum fumigant insecticide, aluminum phosphide is widely used in the tobacco industry to treat tobacco raw materials for insecticide treatment. Specifically, during the insecticide treatment process, aluminum phosphide absorbs moisture in the air after being fumigated and meets water, thereby producing highly toxic phosphine gas. The walls and related facilities in the warehouse that have been in a phosphine environment for a long time will have the following problems:
[0004] 1) The surface of the masonry brick wall will peel due to corrosion, and the brick wall will have penetrating corrosion and cracks over a long period of time, affecting the integrity of the wall structure;
[0005] 2) Penetrating corrosion cracks in the wall destroy the sealing of the wall, which may lead to leakage of pesticides and reduce the concentration of pesticides in the warehouse. The reduction of pesticide concentration will prolong the insecticide cycle, affect the quality of tobacco raw materials, and increase the cost of insecticide control;
[0006] 3) Due to the highly toxic nature of pesticides, their leakage may cause serious environmental problems such as groundwater pollution and impact on nearby humans and animals;
[0007] 4) The combined influence of factors such as wall corrosion and geological settlement causes cracks in the warehouse roof and water leakage. Water leakage can directly lead to complete failure of the warehouse function;
[0008] 5) The electronic equipment of the embedded heat and smoke detection system of the warehouse security system may be broken or short-circuited due to long-term exposure to the phosphine environment, which poses a great threat to the normal alarm and fire protection of the security system.
[0009] The above-mentioned problems caused by phosphine produced by the use of aluminum phosphide for insecticide in tobacco raw material warehouses have always been a pain point in the industry.
[0010] In response to the problem of equipment corrosion in the warehouse caused by phosphine, the prior art has disclosed a "protection device for precision electronic alarm equipment in a phosphine disinfection environment" in the publication number CN105636388A. The "protection device" described in the public document refers to the protection of optical video monitoring alarm equipment installed in a phosphine environment, while for the embedded circuit board of the linear beam type temperature and smoke fire detection system, the circuit of the circuit board is directly exposed to the phosphine environment, and the above-mentioned protection device using the sealing isolation method cannot provide protection for the system; the publication number CN202637795U discloses a "fire-fighting device for preventing corrosion by corrosive gases", but this device is limited to installing a tung oil protective film on the surface of the protected device or installing a sealing box with a bottom plate similar to the protective film. The key point is that the tung oil protective film and the "glass glue" used for sealing between the sealing box and the protected device are prone to aging and failure, so the "fire-fighting device" has no relevance or reference significance for the protection of the temperature and smoke fire detector circuit board described in the present invention.
[0011] Looking at the above technical solutions, on the one hand, they all adopt the method of adding additional protective devices to the equipment in the phosphine environment for corrosion protection. The method of adding additional protective devices not only makes the installation and fixation of the original equipment to be protected time-consuming and labor-intensive, but also the method of adding additional protective devices is not suitable for embedded smoke and temperature sensing systems; on the other hand, the above technical solutions only protect the optical video monitoring equipment in the phosphine environment, but are powerless to protect the wall surface of the raw material warehouse that is in contact with phosphine and requires a complete seal. It should be noted that no reports have been found in the prior art on the problem of leakage caused by corrosion of the inner wall of the tobacco raw material warehouse caused by phosphine, and the search results show that it is completely blank.
[0012] In summary, at present, there is no effective solution to the problems of surface corrosion and wall leaks in raw material warehouses caused by phosphine in the tobacco industry. The roof of the raw material warehouse has to face shutdowns due to frequent maintenance due to roof leaks caused by phosphine corrosion, warehouse structure changes and geological subsidence. At the same time, there are no effective protective measures to prevent corrosion of the many existing embedded temperature and smoke detection systems in the raw material warehouses of most tobacco production enterprises. Summary of the invention
[0013] In view of this, the object of the present invention is to provide a composite material for a tobacco raw material warehouse, which has good density and chemical corrosion resistance, and can effectively resist the wall corrosion of the tobacco raw material warehouse caused by phosphine and the corrosion of the security system used in the tobacco raw material warehouse.
[0014] The composite material for tobacco raw material warehouse of the present invention comprises the following raw materials in parts by weight: 80-150 parts of polyurea resin, 100-150 parts of solvent, 3-10 parts of modifier and 5-15 parts of modified epoxy resin.
[0015] Preferably, the polyurea resin is at least one of polycaprolactam, polyurethaneimide, polyacrylurea, polyureaamide and aspartame polyurea resin.
[0016] Preferably, the preparation method of the modified epoxy resin comprises the following steps:
[0017] (1) 80-95 parts by weight of epoxy resin, 5-15 parts by weight of curing agent and 5-10 parts by weight of modifier are mixed in water, stirred, and then 2-10 parts by weight of surfactant are added to the water to emulsify to form a water-in-oil emulsion;
[0018] (2) adding 0.5-1.5 wt% urea to the water-in-oil emulsion, then dropping 1-3 wt% formaldehyde, adjusting the pH to 6, heating to 60-70° C., and reacting for 1-2 hours;
[0019] (3) Cooling, centrifuging, washing and drying.
[0020] Preferably, the epoxy resin in step (1) is bisphenol A epoxy resin; the curing agent is di-sec-butylamine; and the surfactant is Tween 80.
[0021] Preferably, the solvent consists of acetone and ethyl acetate in a mass ratio of 2-10:5-10.
[0022] Preferably, the modifier is composed of hydroxyapatite and silicon powder in a mass ratio of 1-5:1-5.
[0023] More preferably, the particle size of the silicon powder is 10-70 nm; the particle size of the hydroxyapatite is 80-200 nm.
[0024] Another object of the present invention is to provide a method for preparing the composite material for tobacco raw material warehouse, comprising the following steps:
[0025] S1, weigh the raw materials according to the proportion;
[0026] S2, pouring the polyurea resin into the solvent and continuously stirring until it is completely dissolved to form a uniform solution;
[0027] S3, adding the modifier to the solution obtained in step S2, and continuously stirring to obtain a mixed solution;
[0028] S4, adding the modified epoxy resin to the mixed solution obtained in step S3, and continuously stirring until the mixture is uniform;
[0029] S5, degassing the uniformly mixed solution in step S4 to obtain a composite material for tobacco raw material warehouses.
[0030] In the specific preparation process of the present invention, the modifier hydroxyapatite and silicon powder need to be pre-dispersed and mixed using an ultrasonic disperser.
[0031] The present invention also provides an application of a composite material for a tobacco raw material warehouse for corrosion prevention in a tobacco raw material warehouse. The composite material can be used for corrosion prevention of warehouse wall surfaces or circuit boards of security systems.
[0032] Preferably, the application of the composite material for tobacco raw material warehouse for corrosion prevention in a tobacco raw material warehouse comprises the following steps:
[0033] i) First, clean the surface of the warehouse wall or the surface of the security system circuit board to remove dust and oil;
[0034] ii) heating the composite material to 70-75°C and coating it on the surface of the warehouse wall or the surface of the security system circuit board;
[0035] iii) After coating, maintain at room temperature for more than 48 hours.
[0036] Preferably, during the coating in step ii), the ambient temperature is above 10° C. and the relative humidity is below 85%.
[0037] Preferably, the coating in step ii) is carried out by spraying or brushing, and the coating thickness on the surface of the warehouse wall is 1.5-2.0 mm; the coating thickness on the surface of the security system circuit board is 200-300 μm.
[0038] The composite material in the present invention has the property of being resistant to chemical corrosion, and the specific principle is as follows:
[0039] The key point of preparing the composite material of the present invention is to modify the polyurea resin on the one hand and the epoxy resin on the other hand.
[0040] Specifically, when modifying the epoxy resin, a modifier composed of powdered hydroxyapatite and silicon micropowder is added. During the mixing process with the hydroxyapatite, the silicon micropowder partially enters into the void structure of the hydroxyapatite to fill it. By modifying the epoxy resin using the above treatment method, the chemical corrosion resistance of the epoxy resin can be improved.
[0041] Specifically, when modifying the polyurea resin as the main substrate, the substrate polyurea resin is first dissolved using solvents acetone and ethyl acetate, and then the modifier and modified epoxy resin are added to the dissolved solution, and the polyurea resin is modified in this process.
[0042] In the modification process of polyurea resin, the modifier hydroxyapatite and silicon powder are first dispersed and mixed, wherein the dispersion and mixing, on the one hand, partially disperses the powdered hydroxyapatite and silicon powder, and on the other hand, allows the partially dispersed silicon powder to enter the void structure in the hydroxyapatite to achieve the mixing of the two. The dispersion and mixing operation not only disperses the hydroxyapatite and silicon powder as much as possible, but also fills the void structure in the hydroxyapatite with silicon powder as much as possible during the dispersion process. The composite material prepared by using modified epoxy resin and modified polyurea resin significantly improves the chemical corrosion resistance of the composite material.
[0043] Compared with the prior art, the present invention has the following beneficial effects:
[0044] 1. In addition to having strong adhesion to masonry walls, as well as excellent tensile strength, tear strength and elongation, the composite material of the present invention also has a lower permeability coefficient. The lower permeability coefficient value reflects the strong compactness of the composite material, which can effectively prevent phosphine gas from penetrating into the wall surface and causing the wall to be corroded and peeled.
[0045] 2. The composite material of the present invention also has strong chemical corrosion resistance. In the hydrochloric acid resistance test, under the conditions of 15% concentration and 60°C, the color remained stable after more than 72 hours of corrosion resistance; and under the conditions of phosphoric acid as the immersion medium, 30% concentration and 40°C, the color remained stable after 90 days of testing, showing strong chemical corrosion resistance.
[0046] 3. The final product of the composite material is tested according to ISO11890-1 / ASTM D-1259 standards, and the volatile organic compound content is 0%, so it is environmentally friendly, and no odor or harmful substances will penetrate into the tobacco raw materials to affect the quality of tobacco. DETAILED DESCRIPTION
[0047] The present invention will be further described below in conjunction with the embodiments.
[0048] Example 1
[0049] A method for preparing a composite material for a tobacco raw material warehouse, comprising the following steps:
[0050] Step 1: Preparation of modified epoxy resin, the steps are as follows:
[0051] (1) 90 parts by weight of bisphenol A epoxy resin (DGEBA), 10 parts by weight of curing agent di-sec-butylamine (DMDA) and 10 parts by weight of modifier are mixed in water and stirred, and then 5 parts by weight of surfactant Tween 80 is added to the water to emulsify to form an oil-in-water emulsion; the modifier is composed of hydroxyapatite and silica powder in a mass ratio of 1:1;
[0052] (2) adding 1.0 wt% urea to the water-in-oil emulsion, then dropping 2 wt% formaldehyde, dropping hydrochloric acid solution to adjust the pH to 6, heating to 60° C., and reacting for 1.5 hours;
[0053] (3) Cooling, centrifuging, washing and drying.
[0054] Step 2: Preparation of composite materials for tobacco raw material warehouses, the steps are as follows:
[0055] S1, 40g acetone and 60g ethyl acetate were mixed to obtain a solvent; 3g powdered hydroxyapatite and 5g silicon powder were pre-dispersed and mixed using an ultrasonic disperser to obtain a modifier; then 120g polyurea resin (polycaprolactam) and 15g modified epoxy resin prepared in step 1 were weighed and set aside;
[0056] S2, pouring the polyurea resin into the solvent and continuously stirring until it is completely dissolved to form a uniform solution;
[0057] S3, adding the modifier to the solution obtained in step S2, and continuously stirring to obtain a mixed solution;
[0058] S4, adding the modified epoxy resin to the mixed solution obtained in step S3, and continuously stirring until the mixture is uniform;
[0059] S5, degassing the uniformly mixed solution in step S4 (degassing adopts a conventional method in the art) to obtain a composite material for tobacco raw material warehouse.
[0060] Example 2
[0061] A method for preparing a composite material for a tobacco raw material warehouse, comprising the following steps:
[0062] Step 1: Preparation of modified epoxy resin, the steps are as follows:
[0063] (1) 85 parts by weight of bisphenol A epoxy resin (DGEBA), 15 parts by weight of curing agent di-sec-butylamine (DMDA) and 8 parts by weight of modifier are mixed in water and stirred, and then 4 parts by weight of surfactant Tween 80 is added to the water to emulsify to form an oil-in-water emulsion; the modifier is composed of hydroxyapatite and silica powder in a mass ratio of 2:1;
[0064] (2) adding 1.0 wt % urea to the water-in-oil emulsion, then dropping 2 wt % formaldehyde, dropping hydrochloric acid solution to adjust the pH to 6, heating to 65° C., and reacting for 2 hours;
[0065] (3) Cooling, centrifuging, washing and drying.
[0066] Step 2: Preparation of composite materials for tobacco raw material warehouses, the steps are as follows:
[0067] S1, 50g of acetone and 50g of ethyl acetate are mixed uniformly to obtain a solvent; 5g of powdered hydroxyapatite and 5g of silicon powder are pre-dispersed and mixed using an ultrasonic disperser to obtain a modifier; then 80g of polyurea resin (polycaprolactam) and 10g of the modified epoxy resin prepared in step 1 are weighed and set aside;
[0068] S2~S6 are the same as in Example 1.
[0069] Example 3
[0070] A method for preparing a composite material for a tobacco raw material warehouse, comprising the following steps:
[0071] Step 1: Preparation of modified epoxy resin, the steps are as follows:
[0072] (1) 88 parts by weight of bisphenol A epoxy resin (DGEBA), 12 parts by weight of curing agent di-sec-butylamine (DMDA) and 6 parts by weight of accelerator are mixed in water and stirred, and then 5 parts by weight of surfactant Tween 80 is added to the water to emulsify to form an oil-in-water emulsion; the modifier is composed of hydroxyapatite and silica powder in a mass ratio of 1:1;
[0073] (2) adding 1.0 wt% urea to the water-in-oil emulsion, then dropping 2 wt% formaldehyde, dropping hydrochloric acid solution to adjust the pH to 6, heating to 60° C., and reacting for 1.5 hours;
[0074] (3) Cooling, centrifuging, washing and drying.
[0075] Step 2: Preparation of composite materials for tobacco raw material warehouses, the steps are as follows:
[0076] S1, 60g of acetone and 90g of ethyl acetate are mixed uniformly to obtain a solvent; 1g of powdered hydroxyapatite and 2g of silicon powder are pre-dispersed and mixed using an ultrasonic disperser to obtain a modifier; then 150g of polyurea resin and 12g of the modified epoxy resin prepared in step 1 are weighed and set aside;
[0077] S2~S6 are the same as in Example 1.
[0078] Comparative Example 1
[0079] The difference between Comparative Example 1 and Example 1 is that in the preparation process of the modified epoxy resin in step 1, no modifier consisting of hydroxyapatite and silica powder is added, and the rest are the same.
[0080] Comparative Example 2
[0081] The difference between Comparative Example 2 and Example 1 is that no modifier consisting of hydroxyapatite and silicon powder is added during the preparation of the composite material in step 2, and the rest is the same (a modifier consisting of hydroxyapatite and silicon powder is added during the preparation of the modified epoxy resin).
[0082] Comparative Example 3
[0083] The difference between Comparative Example 3 and Example 1 is that in step 1, in the process of modifying the epoxy resin, and in step 2, in the process of preparing the composite material, only a modifier (10 parts by weight) consisting of a single hydroxyapatite is added, and the rest are the same.
[0084] Comparative Example 4
[0085] The difference between Comparative Example 4 and Example 1 is that in step 1, only a modifier consisting of a single silicon powder (10 parts by weight) is added during the preparation of the epoxy resin and the composite material in step 2, and the rest are the same.
[0086] Comparative Example 5
[0087] The difference between Comparative Example 5 and Example 1 is that in the process of modifying the epoxy resin in step 1 and preparing the composite material in step 2, no modifier is added.
[0088] Comparative Example 6
[0089] The difference between Comparative Example 6 and Example 1 is that in step 1, in the process of modifying the epoxy resin and in step 2, in the process of preparing the composite material, the silicon powder is replaced by nano zinc oxide, and the rest are the same.
[0090] The composite materials for tobacco raw material warehouses prepared in Examples 1-3 and Comparative Examples 1-6 were subjected to performance tests, wherein the testing standards were: hardness in accordance with ISO868-2003 / ASTM D-2240; tensile strength and elongation in accordance with ISO37-2005 / ASTM D-638; adhesion in accordance with DIN EN ISO 4624 / ASTM D-4541; and permeability coefficient in accordance with ISO 15106-3:2003.
[0091] The results are shown in Table 1 below:
[0092] Table 1 Performance comparison of different embodiments and comparative examples
[0093]
[0094] The hydrochloric acid corrosion resistance of the composite materials prepared in Examples 1-3 and Comparative Examples 1-5 was tested according to the standard of DIN ISO 1817-2016. The results are shown in Table 2:
[0095] Table 2 Hydrochloric acid resistance test of different embodiments and comparative examples
[0096]
[0097] According to the standard of DIN ISO 1817-2016, the composite materials prepared in Examples 1-3 and Comparative Examples 1-6 were immersed in a phosphoric acid solution. The results are shown in Table 3:
[0098] Table 3 Phosphoric acid immersion resistance test of different embodiments and comparative examples
[0099]
[0100] As can be seen from Table 1, the composite material prepared by the present invention has relatively strong adhesion, tensile strength, tear strength and elongation in basic properties, and has relatively low permeability coefficient and water vapor permeability. The water vapor permeability and permeability reflect the performance of the medium penetrating through the test material. The larger the value, the easier it is to penetrate. For corrosion resistance, the easier it is for the medium to penetrate through the composite material protective coating, the worse the protective performance of the coating for the protected object. This can also be verified from the tests in Tables 2 and 3.
[0101] The hydrochloric acid corrosion resistance test and phosphoric acid immersion test in Table 2 and Table 3 fully illustrate that the composite material prepared by the method of the present invention has significantly improved chemical corrosion resistance compared with the composite material prepared without modification. Further, it can be seen from the comparative values that the use of a single hydroxyapatite or a single silicon powder as a modifier does not have the ability to improve the chemical corrosion resistance of the composite material; at the same time, it can also be seen that the chemical corrosion resistance of the composite material prepared by only modifying the epoxy resin or only modifying the polyurea resin is far inferior to that of the composite material prepared by modifying both the epoxy resin and the polyurea resin.
[0102] In addition, it can be seen from Table 1, Table 2 and Table 3 that when the silicon powder in the modifier is replaced by nano zinc oxide and the rest of the modification processes are carried out normally, the composite material obtained in Comparative Example 6 is improved in some properties compared with Comparative Examples 1-5, for example, the water vapor permeability and permeability coefficient indicators are better than those of Comparative Examples 1-5, but it is still far behind Example 1, which may be due to the agglomeration of nano zinc oxide and the inability to fully intervene in the voids of hydroxyapatite for filling; further, the composite material obtained in Comparative Example 6 has good chemical corrosion resistance in the hydrochloric acid and phosphoric acid corrosion resistance test, but in the 90-day hydrochloric acid and phosphoric acid corrosion resistance test, the color showed a slight change and the weight showed a large change, so it is not recommended for use in tobacco raw material warehouses.
[0103] Example 5
[0104] The composite material prepared in Example 1 was applied to the circuit board of a linear optical beam smoke detector to prevent phosphine corrosion. At the same time, a blank control group and two additional groups coated with the composite material in Comparative Example 1 were set as control groups.
[0105] Specifically, the above-mentioned circuit board is first coated with the composite material prepared in Example 1 according to the following steps:
[0106] i) Fix the circuit board horizontally on the fixture and clean the surface of the circuit board with a brush or hair dryer to remove dust and oil stains;
[0107] ii) Temporarily isolate components and circuits that do not require corrosion protection with oil paper;
[0108] iii) Use a brush to evenly apply the composite material to the circuits on the circuit board that need to be protected, with a coating thickness of 200-300 μm;
[0109] iv) When applying by brush, the paint should be applied indoors at a temperature between 10 and 35°C and a relative humidity between 50 and 85%;
[0110] v) After the brush coating is completed, the circuit board is cured at room temperature for 72 hours.
[0111] The circuit board of the linear beam smoke detector coated with the composite material was placed in a warehouse in a phosphine environment for fumigation. The fumigation test period was 1 month. During the fumigation period, the maximum concentration of phosphine was 1000ppm. After one month, the warehouse was opened to take out the circuit board for appearance inspection, and the circuit board was installed for functional testing. The test results showed that the circuit board coated with the composite material in Example 1 functioned completely normally, while the blank control group and the circuit board coated with the composite material in Comparative Example 1 both had functional failures to varying degrees.
[0112] The above is only a preferred embodiment of the present invention. It should be pointed out that, for those skilled in the art, without departing from the principle of the present invention, it is also possible to use common polyurea materials purchased on the market, or materials with similar properties that have been modified and retouched to achieve the same effect. These implementations using common polyurea materials or modified and retouched polyurea materials should also be considered as the protection scope of the present invention.
Claims
1. A composite material for tobacco raw material warehouse, characterized in that: The invention comprises the following raw materials in parts by weight: 80-150 parts of polyurea resin, 100-150 parts of solvent, 3-10 parts of modifier and 5-15 parts of modified epoxy resin.
2. The composite material for tobacco raw material warehouse according to claim 1, characterized in that: The polyurea resin is at least one of polycaprolactam, polyurethaneimide, polyacrylurea, polyureaamide and aspartame polyurea resin.
3. The composite material for tobacco raw material warehouse according to claim 1, characterized in that: The preparation method of the modified epoxy resin comprises the following steps: (1) 80-95 parts by weight of epoxy resin, 5-15 parts by weight of curing agent and 5-10 parts by weight of modifier are mixed in water, stirred, and then 2-10 parts by weight of surfactant are added to the water to emulsify to form a water-in-oil emulsion; (2) adding 0.5-1.5 wt% urea to the water-in-oil emulsion, then dropping 1-3 wt% formaldehyde, adjusting the pH to 6, heating to 60-70° C., and reacting for 1-2 hours; (3) Cooling, centrifuging, washing and drying.
4. The composite material for tobacco raw material warehouse according to claim 3, characterized in that: The epoxy resin in step (1) is bisphenol A epoxy resin; the curing agent is di-sec-butylamine; the surfactant is Tween 80; and the modifier is composed of hydroxyapatite and silicon powder in a mass ratio of 1-5:1-5.
5. The composite material for tobacco raw material warehouse according to claim 1, characterized in that: The solvent consists of acetone and ethyl acetate in a mass ratio of 2-10:5-10.
6. The composite material for tobacco raw material warehouse according to claim 1, characterized in that: The modifier is composed of hydroxyapatite and silicon powder in a mass ratio of 1-5:1-5.
7. The composite material for tobacco raw material warehouse according to claim 6, characterized in that: The particle size of the silicon micropowder is 10-70nm; the particle size of the hydroxyapatite is 80-200nm.
8. A method for preparing the composite material for tobacco raw material warehouse according to claim 1, characterized in that The following steps are involved: S1, weigh the raw materials according to the proportion; S2, pouring the polyurea resin into the solvent and continuously stirring until it is completely dissolved to form a uniform solution; S3, adding the modifier to the solution obtained in step S2, and continuously stirring to obtain a mixed solution; S4, adding the modified epoxy resin to the mixed solution obtained in step S3, and continuously stirring until the mixture is uniform; S5, degassing the uniformly mixed solution in step S4 to obtain a composite material for tobacco raw material warehouses.
9. An application of the composite material for tobacco raw material warehouse according to claim 1 for corrosion prevention in tobacco raw material warehouse, characterized in that: The composite material can be used for corrosion protection of warehouse wall surfaces or circuit boards of security systems; The application of the composite material for tobacco raw material warehouse to prevent corrosion in a tobacco raw material warehouse comprises the following steps: i) First, clean the surface of the warehouse wall or the surface of the security system circuit board to remove dust and oil; ii) heating the composite material to 70-75°C and coating it on the surface of the warehouse wall or the surface of the security system circuit board; iii) After coating, maintain at room temperature for more than 48 hours.
10. Application of the composite material for tobacco raw material warehouse for corrosion prevention in tobacco raw material warehouse according to claim 9, characterized in that: During the coating in step ii), the ambient temperature is above 10° C. and the relative humidity is below 85%; The coating is applied by spraying or brushing, and the coating thickness on the surface of the warehouse wall is 1.5-2.0 mm; the coating thickness on the surface of the security system circuit board is 200-300 μm.
Citation Information
Patent Citations
Protection apparatus for precise electronic alarm device in hydrogen phosphide elimination environment
CN105636388A
Wall damage self-repairing decorative paint and preparation method thereof
CN110172300A
Method for preventing breakage and leakage of tank car storage tank
CN117212699A
High-performance moisture-curing polyurea resin and preparation method thereof
CN117986524A
Continuous production of emulsion type aqueous coating compound
JP1989292068A