Flexible acrylic polyurethane finish paint and preparation method thereof

By using elastically expanded microsphere modified hydroxyacrylic resin and hyperbranched silicon modified saturated polyester resin in acrylic polyurethane topcoat, combined with a modified isocyanate mixture, the slow drying speed and short application period in the prior art are solved. The problem of this paper is to achieve high strength, high flexibility and environmentally friendly topcoat, suitable for baking assembly line operations.

CN119081531APending Publication Date: 2024-12-06LUOYANG SUNRUI ANTI-CORROSION ENG TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411349337.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-26
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing acrylic polyurethane topcoat has slow drying speed and long drying time on the baking assembly line, and the paint film has low hardness and short application period, which cannot meet the needs of long-term assembly line spraying operations.

Method used

The combination of component A and component B, including elastically expanded microsphere modified hydroxyacrylic resin, hyperbranched silicon modified saturated polyester resin, modified isocyanate mixture, etc., can improve the drying speed through specific preparation methods and formulas. and paints for suitable periods, enhancing the interlayer bonding and chemical resistance of the paint film.

Benefits of technology

It has achieved fast drying speed, long application period of coating, fast hardness increase, and no retardation phenomenon. The paint film has high strength, high flexibility and excellent chemical resistance. It is suitable for assembly line spraying operations, low production energy consumption and construction emissions Less, low VOC content, good environmental protection performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to the technical field of coatings, in particular to a flexible acrylic polyurethane finish paint. The finish paint comprises a component A and a component B. The component A comprises elastic expansion microsphere modified hydroxy acrylic resin, hyperbranched silicon modified saturated polyester resin, body filler, an anti-aging agent, other auxiliaries and a first solvent. And the component B comprises a modified isocyanate mixed solution and a second solvent. The flexible acrylic polyurethane finish paint provided by the invention has the characteristics of high drying speed, long working life of the paint, good interlayer binding force in a matched coating and the like, and has the characteristics of high hardness rise and no after-tack phenomenon due to the drying speed, and a cured paint film has the properties of high strength, good flexibility, excellent chemical resistance and the like; the production process and the construction process of the finishing coat are relatively simple, the finishing coat can be suitable for assembly line spraying operation, the production energy consumption is low, and the construction emission is less; in addition, the finish paint is low in VOC content and environment-friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of coatings, and in particular to a flexible acrylic polyurethane topcoat and a preparation method thereof. Background Art

[0002] The steel structure of railway bridges needs the protective and decorative function of coatings during production and use. The steel structure and component materials of bridges are generally corroded by the environment or electrochemical effects during use. The metal corrosion of the steel structure and components of bridges has caused huge safety hazards and economic losses. Therefore, the corrosion protection of the steel structure and components of bridges has always received much attention.

[0003] According to the provisions of the Q / CR749-2020 "Protective Coatings and Paints for Railway Bridge Steel Structures and Components" standard, the main components of the anti-corrosion coatings are epoxy zinc-rich primer + epoxy intermediate paint + polyurethane or fluorocarbon topcoat. Among the common corrosion protection methods, the use of anti-corrosion coatings for protection has the excellent characteristics of easy operation and outstanding anti-corrosion performance. It is widely used in bridges, bearings, and ancillary steel structures.

[0004] Acrylic polyurethane topcoat has good decorative properties, chemical resistance, good weather resistance and corrosion resistance. It has now been successfully applied to furniture, vehicles, ships, aircraft and other fields, becoming a hot spot in the field of coating decoration. At present, there are many studies on room temperature self-drying polyurethane paint in China. The best construction temperature of this paint is 15-35℃, and the paint film is completely cross-linked and cured. However, it is baked and dried for 1 hour in a heated drying oven (50-60℃) on the coating line. The drying (actual drying) effect varies, resulting in poor interlayer bonding.

[0005] Production line operations can realize surface treatment, welding, painting, assembly and other process flows of steel structures and components. The painting process uses a catenary automatic conveyor spray line. The entire catenary conveyor is a closed-loop S-shaped route, and the primer, midcoat and topcoat are sprayed in sequence. The baking line operation meets the production efficiency of the company's spraying, but it puts forward higher requirements on the drying and other properties of the topcoat. For example, in order to adapt to the baking line, the topcoat must dry quickly, and because the baking line requires a long period of line operation, the topcoat needs to have good stability and a long application period.

[0006] CN113045979A discloses a high elasticity, high strength, weather-resistant acrylic polyurethane coating and its preparation method. Through the interaction between modified hydroxy acrylic resin, polyester resin, modified polyol, elastic powder, pigment, organic drier, HDI trimer curing agent and modified isocyanate elastomer curing agent, the coating has the characteristics of high elasticity, high strength, high weather resistance, excellent chemical corrosion resistance, etc. However, this system is mainly used for concrete protection, the paint film has low hardness and slow drying, and is not suitable for operation on a baking line.

[0007] CN118271943A discloses a low-temperature quick-drying acrylic polyurethane and its preparation method, which uses hydroxyl acrylic resin and polyaspartic acid ester as main raw materials, and the amino active groups on the main chain of polyaspartic acid ester react with isocyanate to form a urea bond with strong polarity, and the ester bonds on the side chains provide flexibility and adhesion. However, the coating has a violent reaction and a short application period, and cannot meet the requirements of long-cycle assembly line spraying operations. Summary of the invention

[0008] In order to solve the problems of the prior art mentioned in the above background technology, the present application provides a flexible acrylic polyurethane topcoat, and its technical solution is as follows: The flexible acrylic polyurethane topcoat provided by the present application comprises component A and component B, wherein the component A comprises elastically expanded microsphere modified hydroxyl acrylic resin, hyperbranched silicon modified saturated polyester resin, physical filler, anti-aging agent, other additives, and a first solvent; the component B comprises a modified isocyanate mixed liquid and a second solvent; wherein the weight ratio of the elastically expanded microsphere modified hydroxyl acrylic resin, hyperbranched silicon modified saturated polyester resin, physical filler, anti-aging agent to the first solvent is (45.0-55.0): (5-7): (15.0-32.0): (0.8-2.0): (4.0-9.0); the weight ratio of the modified isocyanate mixed liquid to the second solvent is (5.0-18.0): (2.0-5.0); and the weight ratio of the component A to the component B is (5-10): 1.

[0009] In some embodiments, the other additives include a defoamer, a first dispersant, a leveling agent, a pigment, and a thixotropic agent; in terms of weight, component A includes: 45.0 to 55.0 parts of elastic expanded microsphere modified hydroxy acrylic resin, 5 to 7 parts of hyperbranched silicon modified saturated polyester resin, 0.5 to 1.5 parts of a defoamer, 0.2 to 0.9 parts of a first dispersant, 0.5 to 1.5 parts of a leveling agent, 12.0 to 25.0 parts of a pigment, 15.0 to 32.0 parts of a physical filler, 0.8 to 2.0 parts of an anti-aging agent, 0.2 to 1.0 parts of a thixotropic agent, and 4.0 to 9.0 parts of a first solvent.

[0010] In some embodiments, the preparation process of the elastic expanded microsphere modified hydroxy acrylic resin is as follows: Preparation of elastic expanded microsphere particles: The expanded microspheres and elastic rubber nanoparticles are mixed evenly and added to a mixed solvent; then the second dispersant and the first silane coupling agent are added, and after being evenly dispersed, the mixture is heated under reflux at (110-130)°C for (20-40) min, cooled and filtered, dried and ground to obtain the mixture; Preparation of elastic expanded microspheres modified hydroxy acrylic resin: The elastic expanded microsphere particles, the second silane coupling agent, the hydroxy acrylic resin and the polyamide wax powder are dispersed uniformly to obtain a mixture; the mixture is added into butyl acetate, and then a polysiloxane compound containing hydrophobic particles is added, and after being dispersed uniformly, the mixture is heated under reflux at (120-160)° C. for (5-15) minutes to maintain the solid content of the obtained mixed substance between 68% and 72%; and finally the mixed substance is filtered to obtain the obtained mixture.

[0011] In some embodiments, the ratio of the expanded microspheres, elastic rubber nanoparticles, mixed solvent, second dispersant, and first silane coupling agent is 100g: (170-230)g: (300-700)ml: (1.2-1.8)g: (0.1-0.9)g; wherein the expanded microspheres are one or more of MH-60W15, MH-80W, MS205D, and F80DE in any proportion, and the particle size is 40-90μm; the elastic rubber nanoparticles are elastic nano-vulcanized rubber elastic powder, which is one or more of nitrile rubber, acrylic rubber, halogenated butyl rubber, chloroprene rubber, and EPDM rubber in any proportion; the second dispersant is polyvinyl alcohol, polypropylene ether, polyacrylamide, triethylhexyl phosphoric acid, Euka 710S, BYK-220s, B YK-AT203 or a combination of any proportion; the mixed solvent is a mixture of propylene glycol methyl ether acetate and butyl acetate in a mass ratio of (3-7): (1-3); the ratio of the elastic expanded microsphere particles, the second silane coupling agent, hydroxy acrylic resin, polyamide wax powder, butyl acetate, and polysiloxane compound containing hydrophobic particles is 50g: (0.8-1.5)g: (400-500)g: (0.1-0.5)g: (80-130)ml: (0.9-2.3)g; wherein the solid content of the hydroxy acrylic resin is 60-70%; the first silane coupling agent and the second silane coupling agent are a combination of any proportion of one or more of γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, KH-560, and KH-550.

[0012] In some embodiments, the preparation process of the hyperbranched silicon-modified saturated polyester resin is as follows: Adding the organic silicon resin intermediate and the amino resin into toluene, stirring and heating until completely dissolved; then adding the catalyst, stirring and heating to (130-180)°C and keeping the temperature for (7-9) hours, after the solution is transparent and uniform, completely draining the water generated by the reaction, cooling to (40-60)°C, and obtaining the first polymer; The hyperbranched saturated polyester resin, the third silane coupling agent and the first polymer are mixed, and heated to (120-160)°C with stirring and kept warm for (3-5) hours. After the toluene solvent is refluxed to completely discharge the water generated by the reaction, the reaction product is filtered and collected to obtain a hyperbranched silicon-modified saturated polyester resin.

[0013] In some embodiments, the mass ratio of the silicone resin intermediate, amino resin, toluene, catalyst, hyperbranched saturated polyester resin, and the third silane coupling agent is 150: (20-30): (110-130): (0.3-0.7): (30-40): (1.2-1.8); the silicone resin intermediate is one or a combination of any proportion of triethylsilane, dimethylsiloxane, Cheersil8537, and RSN-6018; the amino resin is urea-formaldehyde resin, benzoguanamine formaldehyde The resin is ETERMINO9411-75, aniline formaldehyde resin, one or more combinations in any proportion; the hyperbranched saturated polyester resin is one or more combinations in any proportion of terminal hydroxyl hyperbranched polyester HyPerH20, terminal hydroxyl hyperbranched polyester HyPerH40, terminal hydroxyl hyperbranched polyester H202; the third silane coupling agent is one or more combinations in any proportion of γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, KH-560, KH-550.

[0014] In some embodiments, the preparation process of the modified isocyanate mixture is as follows: In a nitrogen protection environment, aliphatic polyisocyanate and modified elastic isocyanate are mixed; then, in a nitrogen protection environment, a mixture of xylene and butyl acetate is added and mixed evenly to obtain a modified isocyanate mixed solution; Among them, the mass ratio of aliphatic polyisocyanate, modified elastic isocyanate, xylene and butyl acetate is 70: (28-32): (7-13): (7-13).

[0015] In some embodiments, the aliphatic polyisocyanate is one or a combination of any proportion of Covestro N3390, Covestro N75, and Wanhua HT100; the modified elastic isocyanate is one or a combination of any proportion of Covestro N3800, Asahi Kasei E40580T, and Feiyang GB963B100.

[0016] In some embodiments, the defoamer is one or more of polyether-modified silicone oil, polyoxypropanolamine ether, polyoxypropylene glycerol ether, polydimethylsiloxane, Defom6800, BYK-038, and Euka 272S in any proportion; the first dispersant is one or more of polyvinyl alcohol, polypropylene ether, polyacrylamide, triethylhexyl phosphoric acid, Euka 710S, BYK-220s, and BYK-AT203 in any proportion; the leveling agent is one or more of polyether-modified polysiloxane, fluorocarbon polymer leveling agent, polydimethylsiloxane, BYK-306, Tego415, and Efka3777 in any proportion; the pigment is one or more of titanium dioxide R996, phthalocyanine blue, lemon yellow, carbon black H-315, and medium chrome yellow in any proportion; The physical filler is one or a combination of any proportion of 800 mesh precipitated barium sulfate, 325 mesh talc powder, 800 mesh feldspar powder, and 800 mesh wollastonite powder; the anti-aging agent is one or a combination of any proportion of benzotriazole, 2-hydroxy-4-octyloxybenzophenone, pentaerythritol tetra(2-cyano-3,3-diphenylacrylate), bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate, Feiyang GA392, and Feiyang GA1230; the thixotropic agent is one or a combination of any proportion of polyamide wax MT-PLUS, polyolefin wax, organic bentonite 140#, modified hydrogenated castor oil, and BYK~410; the first solvent and the second solvent are one or a combination of any proportion of xylene, butyl acetate, toluene, propylene glycol methyl ether acetate, and ethyl ester.

[0017] The present application also provides a method for preparing the flexible acrylic polyurethane topcoat as described above, wherein the preparation process of component A is as follows: According to the formula, elastic expansion microsphere modified hydroxy acrylic resin, hyperbranched silicon modified saturated polyester resin, defoamer, first dispersant, leveling agent and part of first solvent are mixed uniformly to obtain mixture I; pigment, physical filler and thixotropic agent are gradually added to mixture I and dispersed uniformly, and when the material fineness is ≤30 μm, an anti-aging agent is added, and the remaining first solvent is used to adjust the viscosity of the product, and finally the product is filtered through a sieve to obtain the component A; The preparation process of component B is: According to the formula, the modified isocyanate mixed liquid and the second solvent are evenly dispersed, and the product is filtered through a sieve to obtain the component B; The preparation process of the flexible acrylic polyurethane topcoat is as follows: component A and component B are mixed in a certain weight ratio and stirred evenly to obtain the topcoat.

[0018] Compared with the prior art, the flexible acrylic polyurethane topcoat provided in this application has the following beneficial effects: The flexible acrylic polyurethane topcoat provided in the present application has the characteristics of fast drying speed, long coating application period, good interlayer bonding in the matching coating, etc., and due to its drying speed, it has the characteristics of fast hardness increase and no back-sticking phenomenon, and the cured paint film has the properties of high strength, good flexibility, excellent chemical resistance, etc., and the production process and construction process of the topcoat are relatively simple, and it can be applied to assembly line spraying operations. Its production energy consumption is low and the construction emissions are small. In addition, the topcoat itself has a low VOC (volatile organic compound) content and is environmentally friendly. DETAILED DESCRIPTION

[0019] In order to make the purpose, technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0020] The present application provides an operational example of a method for preparing a flexible acrylic polyurethane topcoat, comprising the following steps: (1) The preparation process of component A is as follows: According to the formula, elastic expansion microsphere modified hydroxy acrylic resin and hyperbranched silicon modified saturated polyester resin are added to a dispersion tank, and a defoamer, a dispersant, and a first solvent of a leveling agent are added thereto, and dispersed at a medium speed of 600 to 900 r / min for 10 to 20 minutes to obtain a mixture I; Under low speed (speed 200-400r / min) stirring, gradually add raw materials such as pigment, body filler and thixotropic agent into mixture I, disperse at high speed (1200-1500r / min) for 30-40 minutes, add anti-aging agent until the fineness of the mixed material is ≤30μm, adjust the viscosity with the remaining first solvent, filter with 80 mesh screen, and package to obtain component A; (2) The preparation process of component B is as follows: According to the formula, take the modified isocyanate mixed liquid and add it into the dispersion tank, add the second solvent into it, disperse it at medium speed (600-900r / min) for 5-10 minutes, disperse it evenly, filter it with an 80-mesh screen, and package it to obtain component B.

[0021] (3) The preparation process of the flexible acrylic polyurethane topcoat is as follows: Component A and Component B are mixed in a certain weight ratio for paint preparation, and stirred evenly to obtain the topcoat.

[0022] Among them, the coating formula is: Measured in parts by weight, component A includes: 45.0-55.0 parts of elastic expanded microsphere modified hydroxy acrylic resin, 5-7 parts of hyperbranched silicon modified saturated polyester resin, 0.5-1.5 parts of defoaming agent, 0.2-0.9 parts of first dispersant, 0.5-1.5 parts of leveling agent, 12.0-25.0 parts of pigment, 15.0-32.0 parts of physical filler, 0.8-2.0 parts of anti-aging agent, 0.2-1.0 parts of thixotropic agent and 4.0-9.0 parts of first solvent.

[0023] In component B, the weight ratio of the modified isocyanate mixture to the second solvent is (5.0-18.0): (2.0-5.0); The weight ratio of component A to component B is (5-10):1.

[0024] The operation example of the preparation method of elastic expanded microsphere modified hydroxy acrylic resin is as follows: (1) Preparation of elastic expanded microsphere particles: The expanded microspheres (particle size distribution is 40-90 μm) and elastic rubber nanoparticles are evenly mixed, added into a round-bottom flask containing a mixed solvent, and a dispersant and a first silane coupling agent are added dropwise, and ultrasonic dispersion is performed. Thereafter, the mixture is heated to reflux for (20-40) min at (110-130) ° C, cooled and filtered, and the filtrate is placed in an oven at 80 ° C and baked for 5 h. After the product is dried, it is ground into particles of 800-1250 meshes to obtain elastic expanded microsphere particles.

[0025] Wherein, the ratio of the expanded microspheres, elastic rubber nanoparticles, mixed solvent, second dispersant, and first silane coupling agent is 100g: (170-230) g: (300-700) ml: (1.2-1.8) g: (0.1-0.9) g; The expanded microspheres are one or a combination of any proportion of MH-60W15, MH-80W, MS205D, and F80DE, and the particle size is 40 to 90 μm; the elastic rubber nanoparticles are elastic nano-vulcanized rubber elastic powders, which are one or a combination of any proportion of nitrile rubber, acrylic rubber, halogenated butyl rubber, chloroprene rubber, and EPDM rubber; the mixed solvent is a mixture of propylene glycol methyl ether acetate and butyl acetate in a mass ratio of (3 to 7): (1 to 3); (2) Preparation of elastic expanded microspheres modified hydroxy acrylic resin: 1) Weigh the elastic expanded microsphere particles, the second silane coupling agent, the hydroxy acrylic resin (solid content 75-80%), and the polyamide wax powder, and use a high-speed disperser to disperse at a speed of 1000-1500 r / min for 40 minutes; 2) Add the above mixture into a round-bottom flask containing butyl acetate, dropwise add the polysiloxane compound containing hydrophobic particles, ultrasonically disperse for 40 minutes, heat under reflux at (120-160)°C for (5-15) minutes, and maintain the solid content of the mixture between 68% and 72%.

[0026] 3) Filter the mixed substance in step 2) with a 100-mesh filter to obtain elastic expanded microsphere-modified hydroxy acrylic resin.

[0027] The ratio of the elastic expanded microsphere particles, the second silane coupling agent, the hydroxy acrylic resin, the polyamide wax powder, butyl acetate, and the polysiloxane compound containing hydrophobic particles is 50g: (0.8-1.5)g: (400-500)g: (0.1-0.5)g: (80-130)ml: (0.9-2.3)g; The solid content of the hydroxy acrylic resin is 75-80%; the first silane coupling agent and the second silane coupling agent are one or a combination of any proportion of γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, KH-560, and KH-550.

[0028] The operation example of the preparation method of the hyperbranched silicon-modified saturated polyester resin is as follows: (1) Weigh the organic silicone resin intermediate, amino resin and toluene in sequence and add them to the reaction kettle. Stir and heat until completely dissolved, then add the catalyst and keep the temperature at (130-180)°C for (7-9) hours. After the solvent becomes transparent and uniform, completely drain the water generated by the reaction and cool to (40-60)°C to obtain the first polymer.

[0029] (2) Take another three-necked flask, add the hyperbranched saturated polyester resin, the third silane coupling agent and the first polymer obtained in step 1, stir and heat to (120-160)°C and keep warm for (3-5) hours. After the solvent refluxes to completely discharge the water generated by the reaction, filter and collect the reaction product. The hyperbranched silicon-modified saturated polyester resin is obtained.

[0030] Among them, the mass ratio of the silicone resin intermediate, the amino resin, toluene, the catalyst, the hyperbranched saturated polyester resin, and the third silane coupling agent is 150: (20-30): (110-130): (0.3-0.7): (30-40): (1.2-1.8); The silicone resin intermediate is one or a combination of any proportion of triethylsilane, dimethylsiloxane, Cheersil8537, and RSN-6018; the amino resin is one or a combination of any proportion of urea-formaldehyde resin, melamine formaldehyde resin, and aniline formaldehyde resin; the hyperbranched saturated polyester resin is one or a combination of any proportion of terminal hydroxyl hyperbranched polyester HyPerH20, terminal hydroxyl hyperbranched polyester HyPerH40, and terminal hydroxyl hyperbranched polyester H202; the third silane coupling agent is one or a combination of any proportion of γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, KH-560, and KH-550.

[0031] The operation example of the preparation method of the modified isocyanate mixed solution is as follows: Seal a clean and dry dispersion tank with nitrogen in advance, and make the internal oxygen content ≤5%. Weigh and put aliphatic polyisocyanate and modified elastic isocyanate into the dispersion tank and mix them. Add xylene and butyl acetate under nitrogen protection, and stir at 800r / min for 10 minutes to obtain a mixture with uniform mixing, good capacity and stable storage.

[0032] Among them, the mass ratio of aliphatic polyisocyanate, modified elastic isocyanate, xylene and butyl acetate is 70: (28-32): (7-13): (7-13); the aliphatic polyisocyanate is one or a combination of several of Covestro N3390, Covestro N75, Wanhua HT100 in any proportion; the modified elastic isocyanate is one or a combination of several of Covestro N3800, Asahi Kasei E40580T, Feiyang GB963B100 in any proportion.

[0033] The present application also provides the following embodiments and comparative examples: Embodiment 1: The formula of the flexible acrylic polyurethane topcoat provided is shown in Table 1: Table 1 Acrylic polyurethane topcoat formula

[0034] The preparation method of the coating of this application is as follows 1. Preparation of Component A: (1) Add elastic expandable microsphere modified hydroxy acrylic resin and hyperbranched silicon modified saturated polyester resin into a dispersion tank, add defoamer, dispersant, leveling agent and part of solvent in order according to the formula amount, and disperse at a medium speed of 600 r / min for 15 minutes to obtain a mixture I; (2) While stirring at a low speed of 200 r / min, gradually add the pigment, filler and thixotropic agent in the formula to the mixture I, and disperse at a high speed of 1500 r / min for 40 min. When the fineness is ≤30 μm, add the anti-aging agent, adjust the viscosity with the remaining solvent, filter with an 80-mesh screen, and package by weight; 2. Preparation of Component B: Add the modified isocyanate mixed liquid into the dispersion tank according to the above formula, add butyl acetate, disperse at a medium speed of 600 r / min for 10 minutes, filter with an 80-mesh sieve, and package.

[0035] 3. Preparation of a flexible acrylic polyurethane topcoat: Prepare the paint in a mass ratio of 8:1 between component A and component B, and then stir evenly.

[0036] Example 2 The formula of the flexible acrylic polyurethane topcoat provided is shown in Table 2: Table 2 Acrylic polyurethane topcoat formula

[0037] The preparation method of the coating of this application is as follows 1. Preparation of Component A: (1) Add elastic expandable microsphere modified hydroxy acrylic resin and hyperbranched silicon modified saturated polyester resin into a dispersion tank, add defoamer, dispersant, leveling agent and part of solvent in order according to the formula amount, and disperse at a medium speed of 900 r / min for 10 min to obtain a mixture I; (2) Gradually add the pigment, filler and thixotropic agent in the formula to the mixture I under low speed stirring at 400 r / min, disperse at high speed at 1200 r / min for 30 min, add anti-aging agent when the fineness is ≤30 μm, adjust the viscosity with the remaining solvent, filter with 80 mesh sieve, and package by weight; 2. Preparation of Component B: Add the modified isocyanate mixture according to the above formula into the dispersion tank, add butyl acetate thereto, disperse at a medium speed of 700 r / min for 12 minutes, filter with an 80-mesh sieve, and package.

[0038] 3. Preparation of a flexible acrylic polyurethane topcoat: Prepare the paint in a mass ratio of 6:1 between component A and component B, and then stir evenly.

[0039] Example 3 The formula of the flexible acrylic polyurethane topcoat provided is shown in Table 3: Table 3 Acrylic polyurethane topcoat formula

[0040] The preparation method of the coating of this application is as follows 1. Preparation of Component A: (1) Add elastic expandable microsphere modified hydroxy acrylic resin and hyperbranched silicon modified saturated polyester resin into a dispersion tank, add defoamer, dispersant, leveling agent and part of solvent in order according to the formula amount, and disperse at a medium speed of 800 r / min for 17 minutes to obtain a mixture I; (2) While stirring at a low speed of 200 r / min, gradually add the pigment, filler and thixotropic agent in the formula to the mixture I, and disperse at a high speed of 1300 r / min for 35 min. When the fineness of the mixed material is ≤30 μm, add an anti-aging agent, adjust the viscosity with the remaining solvent, filter with an 80-mesh screen, and package by weight; 2. Preparation of Component B: Add the modified isocyanate mixed liquid into the dispersion tank according to the above formula, add butyl acetate, disperse at a medium speed of 600 r / min for 15 minutes, filter with an 80-mesh sieve, and package.

[0041] 3. Preparation of a flexible acrylic polyurethane topcoat: Prepare the paint in a mass ratio of 5:1 between component A and component B, and then stir evenly.

[0042] In addition, the preparation process of the elastic expanded microsphere modified hydroxy acrylic resin, hyperbranched silicon modified saturated polyester resin, and modified isocyanate mixed solution in Examples 1-3 is as follows: 1. The preparation method of elastic expanded microsphere modified hydroxy acrylic resin is as follows: (1) Preparation of elastic expanded microsphere particles: The expanded microspheres and elastic rubber nanoparticles are mixed evenly, added into a round-bottom flask containing a mixed solvent, the second dispersant and the first silane coupling agent are added dropwise, ultrasonic dispersion is performed, and then heating and reflux are performed at 120° C. for 30 minutes, cooling and filtering, and the filtrate is placed in an oven at 80° C. for 5 hours. After the product is dried, it is ground into particles of 800 to 1250 meshes to obtain elastic expanded microsphere particles.

[0043] Wherein, the ratio of the expanded microspheres, elastic rubber nanoparticles, mixed solvent, second dispersant, first silane coupling agent is 100g: 200g: 500ml: 1.5g: 0.5g; Among them, the expanded microspheres are MH-60W15, and the particle size is 60 μm; the elastic rubber nanoparticles are elastic nano-vulcanized nitrile rubber; the mixed solvent is a mixture of propylene glycol methyl ether acetate and butyl acetate in a mass ratio of 3:1; the second dispersant is polyvinyl alcohol; and the first silane coupling agent is KH560.

[0044] (2) Preparation of elastic expanded microspheres modified hydroxy acrylic resin: 1) Weigh the elastic expanded microsphere particles, the second silane coupling agent, the hydroxy acrylic resin, and the polyamide wax powder, and use a high-speed disperser to disperse at a speed of 1300 r / min for 40 minutes; 2) The above mixture was added into a round-bottom flask containing butyl acetate, and the polysiloxane compound containing hydrophobic particles was added dropwise. The mixture was dispersed by ultrasonic for 40 minutes and heated under reflux at 130° C. for 10 minutes to maintain the solid content of the mixture between 68% and 72%.

[0045] 3) Filter the mixed substance in step 2) with a 100-mesh filter to obtain elastic expanded microsphere-modified hydroxy acrylic resin.

[0046] The ratio of the elastic expanded microsphere particles, the second silane coupling agent, the hydroxy acrylic resin, the polyamide wax powder, butyl acetate, and the polysiloxane compound containing hydrophobic particles is 50g:1.2g:450g:0.1g:100ml:1.5g; Among them, the second silane coupling agent is KH550; the hydroxy acrylic resin is Deqian FS-4365A, and the solid content of the hydroxy acrylic resin is 75-80%; the polysiloxane compound containing hydrophobic particles is Efka3033.

[0047] 2. The preparation method of hyperbranched silicon modified saturated polyester resin is as follows: (1) Weigh the silicone resin intermediate, amino resin and toluene in sequence and add them into a reactor. Stir and heat until completely dissolved, then add the catalyst and keep the temperature at 150°C for 8 hours. After the solvent becomes transparent and uniform, completely discharge the water generated by the reaction and cool it to about 50°C to obtain the first polymer.

[0048] (2) Take another three-necked flask, add the hyperbranched saturated polyester resin, the third silane coupling agent and the first polymer obtained in step 1, stir and heat to 140°C for 4 hours, and after the solvent refluxes to completely discharge the water generated by the reaction, filter and collect the reaction product. The hyperbranched silicon-modified saturated polyester resin is obtained.

[0049] The mass ratio of the silicone resin intermediate, the amino resin, the toluene, the catalyst, the hyperbranched saturated polyester resin, and the third silane coupling agent is 150 g: 25 g: 120 g: 0.5 g: 35 g: 1.5 g; Among them, the organic silicone resin intermediate is RSN-6018; the amino resin is ETERMINO9411-75 benzoguanamine formaldehyde resin; the hyperbranched saturated polyester resin is HyPerH20; and the third silane coupling agent is KH-560.

[0050] 3. The preparation method of the modified isocyanate mixed solution is as follows: Seal a clean and dry dispersion tank with nitrogen in advance, and make the internal oxygen content ≤5%. Weigh and put aliphatic polyisocyanate and modified elastic isocyanate into the dispersion tank and mix them. Add xylene and butyl acetate under nitrogen protection, and stir at 800r / min for 10 minutes to obtain a mixture with uniform mixing, good capacity and stable storage.

[0051] Among them, the mass ratio of aliphatic polyisocyanate, modified elastic isocyanate, xylene and butyl acetate is 70:30:10:10; the aliphatic polyisocyanate is Wanhua HT100; and the modified elastic isocyanate is Covestro N3800.

[0052] Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that the resin used in component A in this comparative example is not the elastic expanded microsphere modified hydroxy acrylic resin and the hyperbranched silicon modified saturated polyester resin, but the unmodified resin FS-4365A directly replaces the elastic expanded microsphere modified hydroxy acrylic resin and the hyperbranched silicon modified saturated polyester resin in Example 1 with equal mass, and other formulas and preparation methods are consistent with Example 1.

[0053] Comparative Example 2 The only difference between Comparative Example 2 and Example 1 is that only one of the resins used in component A in this comparative example is that no hyperbranched silicon-modified saturated polyester resin is added, and only elastic expanded microsphere-modified hydroxy acrylic resin is added, and the mass of the elastic expanded microsphere-modified hydroxy acrylic resin in this comparative example is equal to the sum of the masses of the elastic expanded microsphere-modified hydroxy acrylic resin and the hyperbranched silicon-modified saturated polyester resin in Example 1. Other formulas and preparation methods are consistent with Example 1.

[0054] Comparative Example 3 The difference between Comparative Example 1 and Example 1 is that the resin of component B in this comparative example is not a modified isocyanate mixed liquid, but ordinary isocyanate resin N75 or the like is used to replace the aliphatic polyisocyanate and modified elastic isocyanate in Example 1, so that the ordinary isocyanate resin N75 is directly mixed with xylene and butyl acetate to prepare an isocyanate resin solution, and other formulas and preparation methods are consistent with Example 1.

[0055] Comparative Example 4 The difference between this comparative example 1 and Example 1 is that the resin of component B in this comparative example is not a modified isocyanate mixed solution (the modified isocyanate mixed solution is a mixed solution formed by mixing aliphatic polyisocyanate and modified elastic isocyanate), but one of the aliphatic polyisocyanate and the modified elastic isocyanate, Covestro N3800, which is directly mixed with xylene and butyl acetate to prepare an isocyanate resin solution, and the mass of Covestro N3800 in this comparative example is equal to the sum of the masses of the aliphatic polyisocyanate and the modified elastic isocyanate in Example 1. Other formulas and preparation methods are consistent with Example 1.

[0056] The products obtained in the above examples and comparative examples were subjected to the following performance tests, and the test results were obtained, as shown in Table 4 below: Table 4 Performance data of examples and comparative examples

[0057] Analysis of the above comparative examples and embodiment data shows that: 1. The resin used in component A is not the elastic expanded microsphere modified hydroxy acrylic resin and the hyperbranched silicon modified saturated polyester resin. In the two cases where only one of the resins used in component A (no hyperbranched silicon modified saturated polyester resin paint film is added), the elongation at break of the obtained topcoat coating cannot meet the requirement of elongation at break ≥ 50, and the alkali resistance and resistance to artificial accelerated aging and other properties cannot meet the requirements.

[0058] 2. In the two cases where the resin of component B is not a modified isocyanate mixture but a common isocyanate resin and component B is not a mixture formed by aliphatic polyisocyanate and modified elastic isocyanate, the application period of the formulated coating is less than 2 hours and cannot meet the requirements of the on-site automated coating line.

[0059] 3. The flexible acrylic polyurethane topcoat prepared in the embodiment of the present application has the characteristics of fast drying speed, long coating application period, good interlayer bonding in the matching coating, etc., and due to its drying speed, it has the characteristics of fast hardness increase and no back-sticking phenomenon, and the cured paint film has the properties of high strength, good flexibility, excellent chemical resistance, etc., and the production process and construction process of the topcoat are relatively simple, and it can be applied to assembly line spraying operations. Its production energy consumption is low and the construction emissions are small. In addition, the topcoat itself has a low VOC (volatile organic compound) content and is environmentally friendly.

[0060] In summary, the flexible acrylic polyurethane topcoat provided in this application has at least the following design concepts and beneficial effects: The flexible acrylic polyurethane topcoat provided in the present application uses elastic expanded microsphere modified hydroxyl acrylic resin as the main film-forming substance, adds low-viscosity, high-hydroxyl value hyperbranched silicon modified saturated polyester resin and pigment additives, and uses modified isocyanate mixed liquid as a curing agent. The obtained topcoat has the characteristics of fast drying speed, long coating application period, good interlayer bonding in the matching coating, and the like. In addition, due to its drying speed, it has the characteristics of fast hardness increase and no back-sticking phenomenon. The cured paint film has the properties of high strength, good flexibility, excellent chemical resistance, etc., and the production process and construction process of the topcoat are relatively simple, which can be applied to assembly line spraying operations. Its production energy consumption is low and construction emissions are low. In addition, the topcoat itself has a low VOC (volatile organic compound) content and is environmentally friendly.

[0061] Therefore, the flexible acrylic polyurethane topcoat is suitable for line spraying operation on the coating line. The polyurethane topcoat is applied by airless spraying on the coating line. The coated workpiece is then baked and dried to complete the coating line coating. The specific topcoat coating process is: substrate cooling - spraying topcoat - leveling, baking - lowering). In summary, the flexible acrylic polyurethane topcoat provided by the present application can be used as a topcoat for bridge steel structures and components in baking line operations.

[0062] This application has the following beneficial effects: 1. The flexible acrylic polyurethane topcoat of the present application uses elastic expanded microsphere modified hydroxy acrylic resin as the main film-forming substance, and adds hyperbranched silicon modified saturated polyester resin to improve the flexibility of the hydroxy acrylic topcoat (elongation at break ≥ 50%), and the topcoat meets the requirements of the film temperature resistance and drying (actual drying) performance under the baking line operation conditions. The modified isocyanate mixture is compounded to improve the compatibility between isocyanates and the application period of the coating.

[0063] 2. The flexible acrylic polyurethane topcoat of this application has excellent construction and anti-corrosion properties, and its specific features are: (1) Fast drying speed (50℃, actual drying (no fingerprints after finger pressure) ≤ 60min); (2) The coating has a long working life, which is ≥3h at 35℃; (3) The matching coating (epoxy zinc-rich primer + epoxy intermediate paint + polyurethane topcoat) has good interlayer bonding strength (adhesion ≥ 10MPa), and the hardness increases quickly, without back-sticking phenomenon, which is convenient for palletizing; (5) The topcoat itself has low VOC (volatile organic compound) content and good environmental performance; (6) The cured paint film has high strength, good flexibility (bending ≤1mm), elongation at break ≥50%, and excellent chemical resistance; 3. The coating production process and construction process of the present application are relatively simple, and assembly line spraying can be adopted, with low production energy consumption and low construction emissions. In addition, the topcoat itself has a low VOC content and good environmental performance.

[0064] It should be noted that: In this article, “~” is used to indicate a numerical range, and the range indicated by this expression includes two endpoint values.

[0065] In addition to the actual selections embodied in the above specific embodiments, the above formulation ranges may be used in the specific implementation of the present application, including but not limited to the above embodiment schemes.

[0066] The specific parameters or some commonly used reagents or raw materials in the above embodiments are specific embodiments or preferred embodiments of the present application, but are not intended to limit the present application. Those skilled in the art may make adaptive adjustments within the scope of the present application.

[0067] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.

Claims

1. A flexible acrylic polyurethane topcoat, comprising component A and component B, characterized in that: The component A comprises elastic expansion microsphere modified hydroxy acrylic resin, hyperbranched silicon modified saturated polyester resin, physical filler, anti-aging agent, other additives, and a first solvent; The component B includes a modified isocyanate mixed solution and a second solvent; The weight ratio of the elastic expanded microsphere modified hydroxy acrylic resin, the hyperbranched silicon modified saturated polyester resin, the physical filler, the anti-aging agent and the first solvent is (45.0-55.0): (5-7): (15.0-32.0): (0.8-2.0): (4.0-9.0); the weight ratio of the modified isocyanate mixed solution and the second solvent is (5.0-18.0): (2.0-5.0); The weight ratio of the component A to the component B is (5-10):

1.

2. The flexible acrylic polyurethane topcoat according to claim 1, characterized in that: The other additives include defoamer, first dispersant, leveling agent, pigment, thixotropic agent; Measured in parts by weight, component A includes: 45.0-55.0 parts of elastic expanded microsphere modified hydroxy acrylic resin, 5-7 parts of hyperbranched silicon modified saturated polyester resin, 0.5-1.5 parts of defoaming agent, 0.2-0.9 parts of first dispersant, 0.5-1.5 parts of leveling agent, 12.0-25.0 parts of pigment, 15.0-32.0 parts of physical filler, 0.8-2.0 parts of anti-aging agent, 0.2-1.0 parts of thixotropic agent and 4.0-9.0 parts of first solvent.

3. The flexible acrylic polyurethane topcoat according to claim 1, characterized in that: The preparation process of the elastic expanded microsphere modified hydroxy acrylic resin is as follows: Preparation of elastic expanded microsphere particles: The expanded microspheres and elastic rubber nanoparticles are mixed evenly and added to a mixed solvent; then the second dispersant and the first silane coupling agent are added, and after being evenly dispersed, the mixture is heated under reflux at (110-130)°C for (20-40) min, cooled and filtered, dried and ground to obtain the mixture; Preparation of elastic expanded microspheres modified hydroxy acrylic resin: The elastic expanded microsphere particles, the second silane coupling agent, the hydroxy acrylic resin and the polyamide wax powder are dispersed uniformly to obtain a mixture; the mixture is added into butyl acetate, and then a polysiloxane compound containing hydrophobic particles is added, and after being dispersed uniformly, the mixture is heated under reflux at (120-160)° C. for (5-15) minutes to maintain the solid content of the obtained mixed substance between 68% and 72%; and finally the mixed substance is filtered to obtain the obtained mixture.

4. The flexible acrylic polyurethane topcoat according to claim 3, characterized in that: The ratio of the expanded microspheres, elastic rubber nanoparticles, mixed solvent, second dispersant, first silane coupling agent is 100g: (170 ~ 230) g: (300 ~ 700) ml: (1.2 ~ 1.8) g: (0.1 ~ 0.9) g; The expanded microspheres are one or a combination of any proportion of MH-60W15, MH-80W, MS205D, and F80DE, and the particle size is 40 to 90 μm; The elastic rubber nanoparticles are elastic nano-vulcanized rubber elastic powder, which is one or a combination of any proportion of nitrile rubber, acrylic rubber, halogenated butyl rubber, chloroprene rubber, and EPDM rubber; The second dispersant is one or a combination of any proportion of polyvinyl alcohol, polypropylene ether, polyacrylamide, triethylhexyl phosphoric acid, Euka 710S, BYK-220s, and BYK-AT203; The mixed solvent is prepared by mixing propylene glycol methyl ether acetate and butyl acetate in a mass ratio of (3-7):(1-3); The ratio of the elastic expanded microsphere particles, the second silane coupling agent, the hydroxy acrylic resin, the polyamide wax powder, butyl acetate, and the polysiloxane compound containing hydrophobic particles is 50g: (0.8-1.5)g: (400-500)g: (0.1-0.5)g: (80-130)ml: (0.9-2.3)g; Wherein, the solid content of the hydroxy acrylic resin is 60-70%; The first silane coupling agent and the second silane coupling agent are one or a combination of any proportion of γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, KH-560, and KH-550.

5. The flexible acrylic polyurethane topcoat according to claim 1, characterized in that: The preparation process of the hyperbranched silicon-modified saturated polyester resin is as follows: Adding the organic silicon resin intermediate and the amino resin into toluene, stirring and heating until completely dissolved; then adding the catalyst, stirring and heating to (130-180)°C and keeping the temperature for (7-9) hours, after the solution is transparent and uniform, completely draining the water generated by the reaction, cooling to (40-60)°C, and obtaining the first polymer; The hyperbranched saturated polyester resin, the third silane coupling agent and the first polymer are mixed, and heated to (120-160)°C with stirring and kept warm for (3-5) hours. After the toluene solvent is refluxed to completely discharge the water generated by the reaction, the reaction product is filtered and collected to obtain a hyperbranched silicon-modified saturated polyester resin.

6. The flexible acrylic polyurethane topcoat according to claim 5, characterized in that: The mass ratio of the organic silicone resin intermediate, amino resin, toluene, catalyst, hyperbranched saturated polyester resin, and the third silane coupling agent is 150: (20-30): (110-130): (0.3-0.7): (30-40): (1.2-1.8); The organic silicon resin intermediate is one or a combination of any proportion of triethylsilane, dimethylsiloxane, Cheersil8537, and RSN-6018; The amino resin is one or a combination of any proportion of urea-formaldehyde resin, benzoguanamine formaldehyde resin ETERMINO9411-75, and aniline formaldehyde resin; The hyperbranched saturated polyester resin is one or a combination of any proportions of terminal hydroxyl hyperbranched polyester HyPerH20, terminal hydroxyl hyperbranched polyester HyPerH40, and terminal hydroxyl hyperbranched polyester H202; The third silane coupling agent is one of γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, KH-560, and KH-550, or a combination of several of them in any proportion.

7. The flexible acrylic polyurethane topcoat according to claim 1, characterized in that: The preparation process of the modified isocyanate mixed solution is as follows: In a nitrogen protection environment, aliphatic polyisocyanate and modified elastic isocyanate are mixed; then, in a nitrogen protection environment, a mixture of xylene and butyl acetate is added and mixed evenly to obtain a modified isocyanate mixed solution; Among them, the mass ratio of aliphatic polyisocyanate, modified elastic isocyanate, xylene and butyl acetate is 70: (28-32): (7-13): (7-13).

8. The flexible acrylic polyurethane topcoat according to claim 7, characterized in that: The aliphatic polyisocyanate is one or a combination of any proportion of Covestro N3390, Covestro N75, and Wanhua HT100; The modified elastic isocyanate is one or a combination of any proportion of Covestro N3800, Asahi Kasei E40580T, and Feiyang GB963B100.

9. The flexible acrylic polyurethane topcoat according to claim 2, characterized in that : The defoaming agent is one or a combination of any proportion of polyether modified silicone oil, polyoxypropanolamine ether, polyoxypropylene glycerol ether, polydimethylsiloxane, Defom6800, BYK-038, and Euka 272S; The first dispersant is one or a combination of any proportion of polyvinyl alcohol, polypropylene ether, polyacrylamide, triethylhexyl phosphoric acid, Euka 710S, BYK-220s, BYK-AT203; The leveling agent is one or a combination of any proportion of polyether modified polysiloxane, fluorocarbon polymer leveling agent, polydimethylsiloxane, BYK-306, Tego415, Efka3777; The pigment is one or a combination of any proportion of titanium dioxide R996, phthalocyanine blue, lemon yellow, carbon black H-315, and medium chrome yellow; The physical filler is one or a combination of any proportion of 800-mesh precipitated barium sulfate, 325-mesh talcum powder, 800-mesh feldspar powder, and 800-mesh wollastonite powder; The anti-aging agent is one or a combination of any proportion of benzotriazole, 2-hydroxy-4-octyloxybenzophenone, pentaerythritol tetrakis (2-cyano-3,3-diphenylacrylate), bis (2,2,6,6-tetramethyl-4-piperidinyl) sebacate, Feiyang GA392, and Feiyang GA1230; The thixotropic agent is one or a combination of any proportion of polyamide wax MT-PLUS, polyolefin wax, organic bentonite 140#, modified hydrogenated castor oil, BYK-410; The first solvent and the second solvent are one or a combination of any proportion of xylene, butyl acetate, toluene, propylene glycol methyl ether acetate, and ethyl acetate.

10. A method for preparing the flexible acrylic polyurethane topcoat according to any one of claims 1 to 9, characterized in that: The preparation process of component A is as follows: According to the formula, elastic expansion microsphere modified hydroxy acrylic resin, hyperbranched silicon modified saturated polyester resin, defoamer, first dispersant, leveling agent and part of first solvent are mixed uniformly to obtain mixture I; pigment, physical filler and thixotropic agent are gradually added to mixture I and dispersed uniformly, and when the material fineness is ≤30 μm, an anti-aging agent is added, and the remaining first solvent is used to adjust the viscosity of the product, and finally the product is filtered through a sieve to obtain the component A; The preparation process of component B is: According to the formula, the modified isocyanate mixed liquid and the second solvent are evenly dispersed, and the product is filtered through a sieve to obtain the component B; The preparation process of flexible acrylic polyurethane topcoat is: Mix component A and component B in a certain weight ratio and stir evenly to obtain the product.

Citation Information

Patent Citations

  • High-elasticity high-strength weather-resistant acrylic polyurethane coating and preparation method thereof

    CN113045979A

  • High-solid super-weather-resistant acrylic polyurethane finish paint and preparation method thereof

    CN118389038A