High-adaptability two-component polyurethane adhesive and preparation method thereof
By designing a highly adaptable two-component polyurethane adhesive, the problem of unstable performance of traditional adhesives in low temperature environments is solved, and high bond strength and aging resistance in a wide temperature range are achieved. It is suitable for The bonding of PVC floors and other plastic and metal structural components has significant economic and environmental benefits.
Patent Information
- Application Number
- CN202411233540.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-12-06
AI Technical Summary
During the cold pressing and bonding of traditional PVC floors, the commonly used adhesives are unstable in low temperature environments, which can easily lead to problems such as foaming and cracking on the floor.
A highly adaptable two-component polyurethane adhesive is adopted, including the first component and the second component, the first component is modified from hydroxyl-terminated polyurethane prepolymer, polyether polyol, vegetable oil modified polyol, The second component consists of isocyanate, diluent and catalyst, and the process is processed through specific mixing ratios and processes to form high adhesion properties. and adhesives with low temperature resistance.
Provides high tensile bonding strength under 5 to 40°C, with resistance to brine aging and heat aging. It is suitable for bonding of PVC floors and other plastic and metal structural components. It has simple process and convenient operation. Significant economic and environmental benefits.
Smart Images

Figure CN119081619A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chemical materials and relates to an adhesive, in particular to a highly adaptable two-component polyurethane adhesive and a preparation method thereof. Background Art
[0002] PVC plastic floor is a new type of lightweight floor decoration material that is very popular in the world, also known as "lightweight floor material". It is a popular product in Europe, America, Japan and South Korea in Asia, and has been popular abroad. It has entered the Chinese market since the early 1980s. It has been widely recognized in large and medium-sized cities in China and is widely used, such as indoor homes, hospitals, schools, office buildings, factories, public places, supermarkets, businesses, stadiums and other places. "PVC plastic floor" refers to the floor produced by polyvinyl chloride materials. Specifically, it is made of polyvinyl chloride and its copolymer resin as the main raw materials, and fillers, plasticizers, stabilizers, colorants and other auxiliary materials are added. It is produced on a sheet-like continuous substrate through a coating process or by calendering, extrusion or extrusion process. It has the characteristics of cleanliness, neatness, elasticity, sound absorption, beauty, and generosity. It can be divided into two types: polyvinyl chloride coil floor and polyvinyl chloride block floor. It is not only green and environmentally friendly, light and thin, super wear-resistant, but also has high elasticity and super impact resistance, fireproof, non-slip and flame retardant. It is a kind of floor with good performance, wide range of uses and high cost performance far exceeding wooden floors, marble, ceramic tiles and other floors.
[0003] Two-component polyurethane adhesive is an adhesive product made based on the polyurethane system, mainly including two components A (mainly polyol) and B (polyisocyanate or terminal isocyanate prepolymer). When used, the two components A and B are mixed and applied to the substrate, and then the hydroxyl reacts with the isocyanate and cross-links and solidifies, so that the adherends are tightly bonded. Because it contains -NHCOO- or -NCO groups, these groups have strong polarity and can form hydrogen bonds with the active hydrogen on the surface of the material, so that the polyurethane has good adhesion. At the same time, the properties of the adhesive can be controlled by the ratio and structure of the soft segment and the hard segment in the polyurethane molecule, so as to adapt to various materials such as metals, plastics, packaging materials, insulation materials, building materials, and different bonding properties and process requirements. In addition, polyurethane adhesives also have excellent oil resistance, low temperature resistance, wear resistance and impact resistance, and are widely used in various industrial or civil fields.
[0004] However, in the traditional cold-pressing process of PVC flooring, in some special construction scenarios (such as winter), the commonly used adhesives are unstable in low temperature environments and have high viscosity problems, which can easily lead to problems such as bubbling and cracking of the floor.
[0005] In view of this, there is an urgent need to design a new adhesive to overcome at least some of the above-mentioned defects of existing adhesives. Summary of the invention
[0006] The invention provides a highly adaptable two-component polyurethane adhesive and a preparation method thereof. The two-component polyurethane adhesive has good adhesion not only to a PVC substrate but also to other plastic and metal structural components.
[0007] To solve the above technical problem, according to one aspect of the present invention, the following technical solution is adopted:
[0008] A highly adaptable two-component polyurethane adhesive, comprising: a first component and a second component;
[0009] The first component includes hydroxyl-terminated polyurethane prepolymer, polyether polyol B, vegetable oil-modified polyol, modified polyester polyol, chain extender, water scavenger, adhesion promoter, plasticizer and filler;
[0010] The second component includes isocyanate B, a diluent and a catalyst.
[0011] As an embodiment of the present invention, the mixing ratio of the first component to the second component is 8-15:6-11;
[0012] The raw materials for preparing the first component include, by weight: 20 to 40 parts of hydroxyl-terminated polyurethane prepolymer, 2 to 10 parts of polyether polyol B, 0.01 to 40 parts of vegetable oil-modified polyol, 10 to 60 parts of modified polyester polyol, 0.1 to 3 parts of chain extender, 3 to 9 parts of dehydrating agent, 0.05 to 0.5 parts of adhesion promoter, 0.05 to 1.5 parts of plasticizer and 10 to 50 parts of filler;
[0013] The raw materials for preparing the second component include, by weight: 20 to 40 parts of isocyanate B, 40 to 80 parts of diluent and 0.01 to 0.5 parts of catalyst.
[0014] As an embodiment of the present invention, the hydroxyl-terminated polyurethane prepolymer comprises: isocyanate A, polyether polyol A and castor oil;
[0015] The polyether polyol B comprises at least one of polyoxypropylene diol, polyoxypropylene triol and polytetrahydrofuran diol, and has a molecular weight of 400-2000 g / mol;
[0016] The vegetable oil modified polyol includes at least one of castor oil, soybean oil polyol, palm oil polyol, linseed oil polyol and cashew nut shell oil polyol, with a hydroxyl value of 20-450 mgKOH / g and a molecular weight of 400-3000 g / mol.
[0017] As an embodiment of the present invention, the isocyanate A includes at least one of 4,4'-MDI, MDI-50, polymeric MDI, TDI100, TDI80, HDI, and IPDI;
[0018] The polyether polyol A comprises at least one of polyoxypropylene diol, polyoxypropylene triol and polytetrahydrofuran diol, and has a molecular weight of 300-3000 g / mol;
[0019] As an embodiment of the present invention, the modified polyester polyol is selected from aromatic modified polyester polyols, with a hydroxyl value of 20-300 mgKOH / g and a molecular weight of 500-6000 g / mol;
[0020] The monomer of the aromatic modified polyester polyol includes at least one of a small molecule diol, a vegetable oil polyol, and an aromatic dicarboxylic acid / anhydride / ester;
[0021] The aromatic dicarboxylic acid / anhydride / ester includes at least one of an aromatic dicarboxylic acid, an aromatic dicarboxylic acid anhydride, and an aromatic dicarboxylic acid ester;
[0022] The aromatic dicarboxylic acid / anhydride / ester includes at least one of phthalic anhydride, isophthalic acid, terephthalic acid, trimellitic anhydride, dimethyl terephthalate, diethyl terephthalate, dimethyl isophthalate, diethyl isophthalate, dimethyl phthalate, and diethyl phthalate;
[0023] The chain extender is a compound that can promote the extension and expansion of the molecular chain, also known as a chain growth agent;
[0024] The dehydrating agent is a compound that has an adsorption effect on water molecules;
[0025] The adhesion promoter includes at least one of a silane coupling agent and a titanate coupling agent;
[0026] The plasticizer is a cold-resistant plasticizer, including at least one of phthalates, benzoates, aliphatic diacid esters, alkyl sulfonate phenyl esters or phosphates;
[0027] The filler includes at least one of titanium dioxide, fumed silica, wollastonite, heavy calcium carbonate, light calcium carbonate, quartz powder, kaolin and talc.
[0028] As an embodiment of the present invention, the isocyanate B includes at least one of polymethylene polyphenyl polyisocyanate PAPI, dicyclohexylmethane diisocyanate HMDI, HDI dimer, HDI trimer, HDI biuret or TDI-TMP, HDI-TMP adduct;
[0029] The diluent includes at least one of ethyl acetate, butyl acetate or butanone, acetone, and dichloromethane, and the diluent is diluted with the diluent to a dilution with NCO%=10%;
[0030] The catalyst comprises at least one of bismuth isooctanoate, bismuth laurate, bismuth neodecanoate, zinc neodecanoate and zinc isooctanoate catalyst.
[0031] According to another aspect of the present invention, the following technical solution is adopted: a method for preparing the above-mentioned highly adaptable two-component polyurethane adhesive, the preparation method comprising:
[0032] Step S1, preparing a first component;
[0033] Dewatering the raw materials;
[0034] According to the formula, isocyanate A, polyether polyol A and castor oil are reacted at 70-90° C. for 2-4 hours to obtain a hydroxyl-terminated polyurethane prepolymer;
[0035] The polyether polyol B, the vegetable oil modified polyol, the modified polyester polyol, the chain extender, the water scavenger, the adhesion promoter, the plasticizer, the filler and the hydroxyl terminated polyurethane prepolymer are uniformly mixed, and the foam is removed and filtered to obtain the first component, and the first component is sealed and stored;
[0036] Step S2, preparing a second component;
[0037] Dehydrating the raw materials;
[0038] According to the formula, isocyanate B is mixed with a diluent and a catalyst, and then dispersed at 30-40°C for 1-2 hours to obtain a second component, which is then sealed and stored;
[0039] Step S3, mechanically mixing the first component and the second component, and placing the mixture on a substrate to obtain the highly adaptable two-component polyurethane adhesive.
[0040] As an embodiment of the present invention, in the step S3, the substrate is applied by brushing, scraping, rolling or spraying.
[0041] As an embodiment of the present invention, in step S1, all raw materials are subjected to water removal treatment to control the moisture content to ≤ 0.05%.
[0042] As an embodiment of the present invention, in step S2, all raw materials are dehydrated to control the moisture content to ≤ 0.05%.
[0043] The beneficial effect of the present invention is that the highly adaptable two-component polyurethane adhesive and the preparation method thereof proposed by the present invention not only have good adhesion to PVC substrates, but also have good adhesion to other plastic and metal structural components.
[0044] The invention can be used for bonding PVC floor substrates, has the characteristics of high adaptability in construction, has high tensile bonding strength when bonding at 5-40°C, and has excellent salt water aging resistance and heat aging resistance. The highly adaptable two-component polyurethane adhesive of the present application has a simple preparation process, is easy to operate, and has significant economic, social and environmental benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 The present invention is a flowchart of a method for preparing a highly adaptable two-component polyurethane adhesive in one embodiment of the present invention. DETAILED DESCRIPTION
[0046] The preferred embodiments of the present invention are described in detail below with reference to the accompanying drawings.
[0047] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.
[0048] The description in this section is only for several typical embodiments, and the present invention is not limited to the scope of the embodiments. The same or similar prior art means and some technical features in the embodiments are mutually replaced within the scope of the present invention.
[0049] Unless otherwise indicated, implied from the context, or customary in the prior art, all parts and percentages in this application are based on weight, and the test and characterization methods used are all current as of the filing date of this application. Where applicable, the contents of any patent, patent application or publication referred to in this application are fully incorporated herein by reference, and their equivalent patent families are also incorporated by reference, especially the definitions of synthesis techniques, product and processing designs, polymers, comonomers, initiators or catalysts disclosed in these documents in the art. If the definition of a specific term disclosed in the prior art is inconsistent with any definition provided in this application, the definition of the term provided in this application shall prevail.
[0050] Numerical ranges in this application are approximate values, so unless otherwise specified, they may include numerical values outside the range. Numerical ranges include all numerical values from the lower limit to the upper limit increased by 1 unit, provided that there is an interval of at least 2 units between any lower value and any higher value. For example, if the recorded component, physical or other properties (such as molecular weight, melt index, etc.) are 100 to 1000, it means that all single values are clearly listed, such as 100, 101, 102, etc., and all sub-ranges, such as 100 to 166, 155 to 170, 198 to 200, etc. For a range containing a numerical value less than 1 or containing a fraction greater than 1 (such as 1.1, 1.5, etc.), 1 unit is appropriately regarded as 0.0001, 0.001, 0.01 or 0.1. For a range containing a single digit less than 10 (such as 1 to 5), 1 unit is usually regarded as 0.1. These are only specific examples of what is intended to be expressed, and all possible combinations of values between the lowest and highest values listed are considered to be clearly recorded in this application. It should also be noted that the terms "first", "second", etc. in this article do not limit the order of precedence, but are only used to distinguish substances with different structures.
[0051] When used with respect to chemical compounds, unless expressly specified otherwise, the singular includes all isomeric forms and vice versa (e.g., "hexane" includes all isomers of hexane, individually or collectively). In addition, nouns using "a," "an," or "the" also include their plural forms unless expressly specified otherwise.
[0052] The terms "comprising", "including", "having" and their derivatives do not exclude the presence of any other components, steps or processes, and are irrelevant to whether these other components, steps or processes are disclosed in this application. To eliminate any doubt, unless explicitly stated, all compositions using the terms "comprising", "including", or "having" in this application may include any additional additives, adjuvants or compounds. On the contrary, except for those necessary for operating performance, the term "essentially consisting of..." excludes any other components, steps or processes from the scope of any description of the term below. The term "consisting of..." does not include any components, steps or processes that are not specifically described or listed. Unless explicitly stated, the term "or" refers to the listed individual members or any combination thereof.
[0053] The description of the steps in each embodiment in the specification is only for the convenience of explanation, and the implementation method of the present application is not limited by the order of implementation of the steps.
[0054] The invention discloses a highly adaptable two-component polyurethane adhesive, which comprises: a first component and a second component; the first component comprises a hydroxyl-terminated polyurethane prepolymer, polyether polyol B, vegetable oil-modified polyol, modified polyester polyol, a chain extender, a water scavenger, an adhesion promoter, a plasticizer and a filler; and the second component comprises isocyanate B, a diluent and a catalyst.
[0055] In one embodiment of the present invention, the mixing ratio of the first component to the second component is 8-15:6-11; in terms of mass fractions, the raw materials for preparing the first component include: 20-40 parts of hydroxyl-terminated polyurethane prepolymer, 2-10 parts of polyether polyol B, 0.01-40 parts of vegetable oil-modified polyol, 10-60 parts of modified polyester polyol, 0.1-3 parts of chain extender, 3-9 parts of dewatering agent, 0.05-0.5 parts of adhesion promoter, 0.05-1.5 parts of plasticizer and 10-50 parts of filler; in terms of mass fractions, the raw materials for preparing the second component include: 20-40 parts of isocyanate B, 40-80 parts of diluent and 0.01-0.5 parts of catalyst.
[0056] In one embodiment of the present invention, the hydroxyl-terminated polyurethane prepolymer comprises: isocyanate A, polyether polyol A and castor oil; the polyether polyol B comprises at least one of polyoxypropylene diol, polyoxypropylene triol and polytetrahydrofuran diol, and the molecular weight is 400-2000g / mol; in one embodiment, the polyether polyol B is polytetrahydrofuran diol (PTMG) with a molecular weight of 500-1000g / mol. The vegetable oil modified polyol comprises at least one of castor oil, soybean oil polyol, palm oil polyol, linseed oil polyol and cashew nut shell oil polyol, and the hydroxyl value is 20-450mgKOH / g and the molecular weight is 400-3000g / mol.
[0057] In one embodiment of the present invention, the isocyanate A includes at least one of 4,4'-MDI, MDI-50, polymeric MDI, TDI100, TDI80, HDI, and IPDI; the polyether polyol A includes at least one of polyoxypropylene diol, polyoxypropylene triol, and polytetrahydrofuran diol, and has a molecular weight of 300-3000 g / mol; in one embodiment, the polyether polyol A is a polyoxypropylene diol with a molecular weight of 500-1000 g / mol.
[0058] In one embodiment of the present invention, the modified polyester polyol is selected from aromatic modified polyester polyols, having a hydroxyl value of 20-300 mgKOH / g and a molecular weight of 500-6000 g / mol; the monomer of the aromatic modified polyester polyol includes at least one of a small molecule diol, a vegetable oil polyol, and an aromatic dicarboxylic acid / anhydride / ester.
[0059] The aromatic dicarboxylic acid / anhydride / ester includes at least one of aromatic dicarboxylic acids, aromatic dicarboxylic acid anhydrides, and aromatic dicarboxylic acid esters; in one embodiment, the aromatic dicarboxylic acid / anhydride / ester includes at least one of phthalic anhydride, isophthalic acid, terephthalic acid, trimellitic anhydride, dimethyl terephthalate, diethyl terephthalate, dimethyl isophthalate, diethyl isophthalate, dimethyl phthalate, and diethyl phthalate.
[0060] The chain extender is a compound that can promote the extension and expansion of the molecular chain, also known as a chain extender. The chain extender is generally a small molecule compound containing two functional groups, such as diols, diamines, ethanolamine, etc. In one embodiment, the chain extender includes one or more of diethylene glycol, propylene glycol, 1,4-butanediol, trimethylolpropane, triethanolamine, 1,4-cyclohexanediol, and hydrogenated bisphenol A.
[0061] The dehydrating agent is a compound that has an adsorption effect on water molecules; in one embodiment, the dehydrating agent includes one or more of anhydrous calcium chloride, barium oxide, calcium oxide, magnesium sulfate, calcium sulfate, calcium hydride, and molecular sieve activation powder.
[0062] The adhesion promoter includes at least one of a silane coupling agent and a titanate coupling agent; the plasticizer is a cold-resistant plasticizer, including at least one of phthalates, benzoates, aliphatic diacids, alkyl sulfonate phenyl esters or phosphates; the filler includes at least one of titanium dioxide, fumed silica, wollastonite, heavy calcium carbonate, light calcium carbonate, quartz powder, kaolin and talc.
[0063] In one embodiment of the present invention, the isocyanate B includes at least one of polymethylene polyphenyl polyisocyanate PAPI, dicyclohexylmethane diisocyanate HMDI, HDI dimer, HDI trimer, HDI biuret or TDI-TMP, HDI-TMP adduct. The diluent includes at least one of ethyl acetate, butyl acetate or butanone, acetone, and dichloromethane, and is diluted with the diluent to a diluent with NCO%=10%. The catalyst includes at least one of bismuth isooctanoate, bismuth laurate, bismuth neodecanoate, zinc neodecanoate, and zinc isooctanoate catalyst.
[0064] The present invention further discloses a method for preparing the highly adaptable two-component polyurethane adhesive. Figure 1 FIG. 1 is a flow chart of a method for preparing a highly adaptable two-component polyurethane adhesive according to an embodiment of the present invention; please refer to FIG. Figure 1 , the preparation method comprises:
[0065] [Step S1] preparing a first component;
[0066] All raw materials are dehydrated to control the moisture content to less than or equal to 0.05%;
[0067] According to the formula, isocyanate A, polyether polyol A and castor oil are reacted at 70-90° C. for 2-4 hours to obtain a hydroxyl-terminated polyurethane prepolymer;
[0068] The polyether polyol B, the vegetable oil modified polyol, the modified polyester polyol, the water removing agent, the adhesion promoter, the plasticizer, the filler and the hydroxyl terminated polyurethane prepolymer are uniformly mixed, and the first component is obtained after defoaming and filtering, and the first component is sealed and stored;
[0069] [Step S2] preparing a second component;
[0070] All raw materials are dehydrated to control the moisture content to less than or equal to 0.05%;
[0071] According to the formula, isocyanate B is mixed with a diluent and a catalyst, and then dispersed at 30-40°C for 1-2 hours to obtain a second component, which is then sealed and stored;
[0072] [Step S3] Mechanically mix the first component and the second component, and apply the mixture on a substrate to obtain the highly adaptable two-component polyurethane adhesive. In one embodiment, the adhesive is applied on the substrate by brushing, scraping, rolling or spraying.
[0073] Example 1
[0074] A method for preparing a highly adaptable two-component polyurethane adhesive comprises the following steps:
[0075] [Step S1] Preparation of component A (first component), the ingredients and weight proportions of component A are as follows:
[0076] 25 parts of hydroxyl terminated polyurethane prepolymer
[0077] 6 parts of polyoxypropylene glycol (700 g / mol)
[0078] Castor oil modified polyol (1000g / mol) 10 parts
[0079] Phthalic anhydride modified polyester polyol (1200g / mol) 10 parts
[0080] 0.5 parts of diethylene glycol
[0081] 8 parts of anhydrous calcium chloride
[0082] 1170 0.12 copies
[0083] 0.2 parts of methyl benzoate
[0084] 40 parts of heavy calcium carbonate
[0085] 10 parts of light calcium carbonate.
[0086] The components and weight proportions of the hydroxyl-terminated polyurethane prepolymer are as follows:
[0087] MDI - 505 parts;
[0088] 10 parts of polyoxypropylene glycol (400 g / mol);
[0089] 10 parts of castor oil.
[0090] The preparation method of the component A is as follows: first, all the raw materials are dehydrated to a water content of less than 500 ppm; then, according to the formula, 5 parts of MDI-50, 10 parts of polyoxypropylene diol (400 g / mol), and 10 parts of castor oil are reacted at 70-90° C. for 2-4 hours, and after the isocyanate group reaction is completed, a hydroxyl-terminated polyurethane prepolymer is obtained for standby use; then, 6 parts of polyoxypropylene diol (700 g / mol), 10 parts of castor oil-modified polyol (1000 g / mol), 10 parts of phthalic anhydride-modified polyester polyol (1200 g / mol), 0.5 parts of diethylene glycol, 8 parts of anhydrous calcium chloride, 0.12 parts of 11700, 0.2 parts of methyl benzoate, 40 parts of heavy calcium carbonate, and 10 parts of light calcium carbonate are uniformly mixed with the hydroxyl-terminated polyurethane prepolymer, and the mixture is degassed and filtered to obtain the component A, which is sealed and stored for standby use.
[0091] [Step S2] Preparation of component B (second component), the ingredients and weight proportions of component B are as follows:
[0092] 30 parts of polymethylene polyphenyl polyisocyanate PAPI;
[0093] 63 parts of ethyl acetate;
[0094] 0.15 parts of bismuth isooctanoate.
[0095] The preparation method of the B component is as follows: first, the raw materials are dehydrated to a moisture content of less than 500ppm; then, 30 parts by mass of polymethylene polyphenyl polyisocyanate, 63 parts by mass of ethyl acetate, and 0.15 parts by mass of bismuth isooctanoate are mixed according to the formula, and then dispersed at 30-40°C for 1-2h to obtain the B component, which needs to be sealed and stored for standby use. The mass ratio of the obtained A component to the B component is 10:8.
[0096] The formula of hydroxyl terminated polyurethane prepolymer 1-5 is shown in Table 1.
[0097] Table 1 Synthesis formula of hydroxyl terminated polyurethane prepolymer
[0098]
[0099] The preparation process of Examples 2-5 is as shown in Example 1, and the formulas are shown in Tables 2 and 3.
[0100] Table 2 Preparation formula of component A in Example 2-5
[0101]
[0102]
[0103] Table 3 Preparation formula of component B in Examples 2-5
[0104]
[0105]
[0106] The two-component polyurethane adhesives prepared in the above five embodiments were tested for open time and adhesive peeling performance. The test results are shown in Table 4.
[0107] Table 4 Test results of bonding and peeling performance of two-component polyurethane adhesive
[0108]
[0109] It can be seen that the highly adaptable adhesive of the present invention has an open time of 30-50 minutes, a wide tolerance for construction temperature, high adaptability (5°C, 40°C), a bonding strength of >40Mpa, and wide adaptability to different plastic substrates such as PVC and PE.
[0110] In summary, the highly adaptable two-component polyurethane adhesive and the preparation method thereof proposed in the present invention use a two-component polyurethane adhesive, which not only has good adhesion to PVC substrates, but also has good adhesion to other plastic and metal structural components.
[0111] The invention can be used for bonding PVC floor substrates, has the characteristics of high adaptability in construction, has high tensile bonding strength when bonding at 5-40°C, and has excellent salt water aging resistance and heat aging resistance. The highly adaptable two-component polyurethane adhesive of the present application has a simple preparation process, is easy to operate, and has significant economic, social and environmental benefits.
[0112] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0113] The description and application of the present invention here are illustrative, and it is not intended to limit the scope of the present invention to the above-mentioned embodiments. The effects or advantages involved in the embodiments may not be embodied in the embodiments due to interference from various factors, and the description of the effects or advantages is not used to limit the embodiments. The deformation and change of the embodiments disclosed here are possible, and the replacement of the embodiments and the various equivalent parts are well known to those of ordinary skill in the art. It should be clear to those skilled in the art that the present invention can be implemented in other forms, structures, arrangements, proportions, and with other components, materials and parts without departing from the spirit or essential features of the present invention. Other deformations and changes can be made to the embodiments disclosed here without departing from the scope and spirit of the present invention.
Claims
1. A highly adaptable two-component polyurethane adhesive, characterized in that: The highly adaptable two-component polyurethane adhesive comprises: a first component and a second component; The first component includes hydroxyl-terminated polyurethane prepolymer, polyether polyol B, vegetable oil-modified polyol, modified polyester polyol, chain extender, water scavenger, adhesion promoter, plasticizer and filler; The second component includes isocyanate B, a diluent and a catalyst.
2. The highly adaptable two-component polyurethane adhesive according to claim 1, characterized in that: The mixing ratio of the first component to the second component is 8-15:6-11; The raw materials for preparing the first component include, by weight: 20 to 40 parts of hydroxyl-terminated polyurethane prepolymer, 2 to 10 parts of polyether polyol B, 0.01 to 40 parts of vegetable oil-modified polyol, 10 to 60 parts of modified polyester polyol, 0.1 to 3 parts of chain extender, 3 to 9 parts of dehydrating agent, 0.05 to 0.5 parts of adhesion promoter, 0.05 to 1.5 parts of plasticizer and 10 to 50 parts of filler; The raw materials for preparing the second component include, by weight: 20 to 40 parts of isocyanate B, 40 to 80 parts of diluent and 0.01 to 0.5 parts of catalyst.
3. The highly adaptable two-component polyurethane adhesive according to claim 1, characterized in that: The hydroxyl-terminated polyurethane prepolymer comprises: isocyanate A, polyether polyol A and castor oil; The polyether polyol B comprises at least one of polyoxypropylene diol, polyoxypropylene triol and polytetrahydrofuran diol, and has a molecular weight of 400-2000 g / mol; The vegetable oil modified polyol includes at least one of castor oil, soybean oil polyol, palm oil polyol, linseed oil polyol and cashew nut shell oil polyol, with a hydroxyl value of 20-450 mgKOH / g and a molecular weight of 400-3000 g / mol.
4. The highly adaptable two-component polyurethane adhesive according to claim 3, characterized in that: The isocyanate A includes at least one of 4,4'-MDI, MDI-50, polymeric MDI, TDI 100, TDI80, HDI, and IPDI; The polyether polyol A comprises at least one of polyoxypropylene diol, polyoxypropylene triol and polytetramethylene glycol, and has a molecular weight of 300-3000 g / mol.
5. The highly adaptable two-component polyurethane adhesive according to claim 1, characterized in that: The modified polyester polyol is selected from aromatic modified polyester polyols, having a hydroxyl value of 20-300 mgKOH / g and a molecular weight of 500-6000 g / mol; The monomer of the aromatic modified polyester polyol includes at least one of a small molecule diol, a vegetable oil polyol, and an aromatic dicarboxylic acid / anhydride / ester; The aromatic dicarboxylic acid / anhydride / ester includes at least one of an aromatic dicarboxylic acid, an aromatic dicarboxylic acid anhydride, and an aromatic dicarboxylic acid ester; The aromatic dicarboxylic acid / anhydride / ester includes at least one of phthalic anhydride, isophthalic acid, terephthalic acid, trimellitic anhydride, dimethyl terephthalate, diethyl terephthalate, dimethyl isophthalate, diethyl isophthalate, dimethyl phthalate, and diethyl phthalate; The chain extender is a compound that promotes the extension and expansion of the molecular chain, also known as a chain growth agent; The dehydrating agent is a compound that has an adsorption effect on water molecules; The adhesion promoter includes at least one of a silane coupling agent and a titanate coupling agent; The plasticizer is a cold-resistant plasticizer, including at least one of phthalates, benzoates, aliphatic diacid esters, alkyl sulfonate phenyl esters or phosphates; The filler includes at least one of titanium dioxide, fumed silica, wollastonite, heavy calcium carbonate, light calcium carbonate, quartz powder, kaolin and talc.
6. The highly adaptable two-component polyurethane adhesive according to claim 1, characterized in that: The isocyanate B includes at least one of polymethylene polyphenyl polyisocyanate PAPI, dicyclohexylmethane diisocyanate HMDI, HDI dimer, HDI trimer, HDI biuret or TDI-TMP, HDI-TMP adduct; The diluent includes at least one of ethyl acetate, butyl acetate or butanone, acetone, and dichloromethane, and the diluent is diluted with the diluent to a dilution with NCO%=10%; The catalyst comprises at least one of bismuth isooctanoate, bismuth laurate, bismuth neodecanoate, zinc neodecanoate and zinc isooctanoate catalyst.
7. A method for preparing the highly adaptable two-component polyurethane adhesive according to any one of claims 1 to 6, characterized in that: The preparation method comprises: Step S1, preparing a first component; Dewatering the raw materials; According to the formula, isocyanate A, polyether polyol A and castor oil are reacted at 70-90° C. for 2-4 hours to obtain a hydroxyl-terminated polyurethane prepolymer; The polyether polyol B, the vegetable oil modified polyol, the modified polyester polyol, the water removing agent, the adhesion promoter, the plasticizer, the filler and the hydroxyl terminated polyurethane prepolymer are uniformly mixed, and the first component is obtained after defoaming and filtering, and the first component is sealed and stored; Step S2, preparing a second component; Dehydrating the raw materials; According to the formula, isocyanate B is mixed with a diluent and a catalyst, and then dispersed at 30-40°C for 1-2 hours to obtain a second component, which is then sealed and stored; Step S3, mechanically mixing the first component and the second component, and placing the mixture on a substrate to obtain the highly adaptable two-component polyurethane adhesive.
8. The preparation method according to claim 7, characterized in that: In the step S3, the coating is applied on the substrate by brushing, scraping, rolling or spraying.
9. The preparation method according to claim 7, characterized in that: In step S1, all raw materials are subjected to water removal treatment to control the moisture content to ≤ 0.05%.
10. The preparation method according to claim 7, characterized in that: In step S2, all raw materials are dehydrated to control the moisture content to ≤ 0.05%.
Citation Information
Cited By
Two-component polyurethane structural adhesive and preparation method thereof
CN120005558A