High-strength starch adhesive for artificial board as well as preparation method and use method of high-strength starch adhesive

The high-strength starch adhesive with chemical crosslinked structure solves the problems of insufficient water resistance and bonding strength of traditional starch adhesives, and achieves high-strength and environmentally friendly glue performance to meet the needs of artificial board manufacturing.

CN119081647AActive Publication Date: 2024-12-06NORTHEAST FORESTRY UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411369201.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-12-06
Estimated Expiration
2044-09-29

AI Technical Summary

Technical Problem

Traditional starch adhesives are insufficient in the production of artificial boards, which cannot meet the requirements of adhesives, and have potential harm to the environment and human health.

Method used

Using the preparation method of high-strength starch adhesive, by mixing oxidized starch, gelatin and crosslinking agent under certain conditions to form a chemical crosslinking structure and combine it with isocyanate to prepare high bonding strength and water resistance starch adhesive.

Benefits of technology

It has achieved the improvement of the bonding strength of high-strength starch adhesives, improved water resistance, avoided formaldehyde emission, met environmental protection and performance requirements, and had broad market prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081647A_ABST
    Figure CN119081647A_ABST
Patent Text Reader

Abstract

The invention relates to a high-strength starch adhesive for an artificial board as well as a preparation method and a use method of the high-strength starch adhesive, and belongs to the technical field of starch adhesives. In order to solve the problem that the water resistance and the bonding strength of the traditional starch adhesive cannot meet the production requirements of the artificial board, the invention provides the high-strength starch adhesive for the artificial board as well as the preparation method and the use method of the high-strength starch adhesive. The high-strength starch adhesive for the artificial board comprises the following components: a prefabricated material, dry-based starch and isocyanate, wherein the prefabricated material comprises oxidized starch, gelatin, a cross-linking agent and distilled water. The prepared high-strength starch adhesive for the artificial board is prepared by taking the renewable starch and the gelatin as main materials through chemical crosslinking, has the advantages of high bonding strength, good water resistance, no formaldehyde generation, environmental friendliness and the like, meets the requirements of national second-class plywood, and has a wide market prospect in the field of artificial board manufacturing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of starch adhesives, and in particular relates to a high-strength starch adhesive for artificial boards, a preparation method thereof and a use method thereof. Background Art

[0002] In modern furniture manufacturing, interior decoration and construction industries, wood-based panels are widely used due to their good physical and mechanical properties, dimensional stability and processing convenience. As a key material in the production process of wood-based panels, the performance of adhesives directly affects the quality and performance of wood-based panels. In order to ensure that wood-based panels can meet various usage conditions and environmental requirements, adhesives must meet the requirements of bonding strength, water resistance and environmental protection.

[0003] At present, the adhesives used in the production of artificial boards are mainly "trialdehyde adhesives", namely urea-formaldehyde resin, phenol-formaldehyde resin and melamine-formaldehyde resin. These adhesives will release free formaldehyde during use, causing harm to the environment and human health. Therefore, the development of environmentally friendly, formaldehyde-free adhesives is of great significance to the healthy development of the artificial board industry.

[0004] Starch adhesive is an adhesive made from starch as a base material modified by physical, chemical or biological methods. As a green and environmentally friendly adhesive, its research and application are expected to provide strong support for the environmental protection transformation of the wood-based panel industry. Since the starch main chain carries a large number of hydrophilic hydroxyl groups and fails to form an effective network cross-linking structure after bonding, its water resistance and bonding strength are relatively weak. Therefore, traditional starch adhesives cannot meet the requirements of wood-based panel production for adhesives. Summary of the invention

[0005] In order to solve the problem that the water resistance and bonding strength of traditional starch adhesives cannot meet the production requirements of artificial boards, the present invention provides a high-strength starch adhesive for artificial boards, a preparation method and a use method thereof.

[0006] The technical solution of the present invention:

[0007] A high-strength starch adhesive for artificial panels comprises the following components in parts by mass: 100 parts of prefabricated materials, 30 to 70 parts of dry-base starch and 10 to 30 parts of isocyanate; the prefabricated materials comprise the following components in parts by mass: 60 to 100 parts of oxidized starch, 80 to 100 parts of gelatin, 10 to 30 parts of a cross-linking agent and 600 to 1000 parts of distilled water.

[0008] Furthermore, the crosslinking agent is one or a combination of polyethylene glycol diglycidyl ether, bisphenol A diglycidyl ether, long-chain alkyl glycidyl ether, neopentyl glycol diglycidyl ether, polypropylene oxide diglycidyl ether, glycerol diglycidyl ether or 1,4-butanediol glycidyl ether.

[0009] Furthermore, the isocyanate is one or a combination of polymethylene polyphenyl isocyanate, toluene diisocyanate TDI, isophorone diisocyanate IPDI, diphenylmethane diisocyanate MDI, dicyclohexylmethane diisocyanate HMDI, hexamethylene diisocyanate HDI or lysine diisocyanate.

[0010] A method for preparing a high-strength starch adhesive for artificial boards comprises the following steps:

[0011] Step 1: preparing the prefabricated material: fully mixing and stirring the oxidized starch, gelatin and distilled water, and then adding a cross-linking agent and continuing the reaction for a certain period of time to obtain the prefabricated material;

[0012] Step 2: preparing starch adhesive: when using, the prefabricated material prepared in step 1, dry starch and isocyanate are mixed and stirred evenly according to parts by mass to obtain starch adhesive.

[0013] Furthermore, the sufficient mixing and stirring in step 1 is sufficient stirring at 60-80° C. for 30 minutes.

[0014] Furthermore, the continued reaction in step 1 is carried out at 60-80° C. for 2-4 hours.

[0015] A method for using a high-strength starch adhesive for artificial boards. When using, the starch adhesive is evenly applied on a wood veneer, and the amount of adhesive applied on one side of the board is 200 to 300 g / m 2 , the bonding is completed after pre-pressing and hot pressing.

[0016] Furthermore, the pre-pressing is performed for 30 minutes under a pressure of 2 to 5 MPa.

[0017] Furthermore, the hot pressing is performed by using a hot press machine at a temperature of 110 to 130° C. and a pressure of 2 to 3 MPa for 10 minutes.

[0018] Furthermore, the method also includes placing the hot-pressed artificial board in an environment for 24 hours to eliminate internal stress.

[0019] Beneficial effects of the present invention:

[0020] The high-strength starch adhesive for artificial panels prepared by the present invention is prepared by chemical cross-linking with renewable starch and gelatin as main materials, has the advantages of high bonding strength, good water resistance, no formaldehyde generation, environmental friendliness, low cost, etc., meets the national requirements for Class II plywood, and has broad market prospects in the field of artificial panel manufacturing. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1This is a photograph of the fracture surface of the plate after the wet tensile test of the high-strength starch adhesive prepared in Example 1;

[0022] Figure 2 This is a photograph of the fracture surface of the plate after the wet tensile test of the high-strength starch adhesive prepared in Example 5;

[0023] Figure 3 This is a photograph of the fracture surface of the board after the wet-strength tensile test of the starch adhesive prepared in Comparative Example 1. DETAILED DESCRIPTION

[0024] The technical solution of the present invention is further described below in conjunction with the embodiments, but it is not limited thereto. Any modification or equivalent replacement of the technical solution of the present invention without departing from the spirit and scope of the technical solution of the present invention shall be included in the protection scope of the present invention. The process equipment or devices not specifically noted in the following embodiments are all conventional equipment or devices in the art. If not specifically specified, the raw materials used in the embodiments of the present invention can be obtained commercially; if not specifically specified, the technical means used in the embodiments of the present invention are all conventional means well known to those skilled in the art.

[0025] Example 1

[0026] This embodiment provides a high-strength starch adhesive and uses it in the preparation of plywood.

[0027] The method for preparing the high-strength starch adhesive for artificial panels provided in this embodiment comprises the following steps:

[0028] Step 1, preparing the prefabricated material: 100 parts of oxidized starch, 80 parts of gelatin and 800 parts of distilled water are fully mixed, stirred in a 70°C water bath for 30 minutes, and then 15 parts of polyethylene glycol diglycidyl ether are added, and the reaction is continued at 75°C with stirring for 2 hours to obtain the prefabricated material;

[0029] Step 2, preparing starch adhesive: when using, 100 parts of the prefabricated material prepared in step 1, 50 parts of dry starch and 10 parts of polymethylene polyphenyl isocyanate are mixed and stirred evenly to obtain starch adhesive.

[0030] The starch adhesive prepared in this example is used to prepare plywood, and the specific method is as follows:

[0031] Apply starch adhesive evenly on the wood veneer, with the amount of adhesive applied on one side of the board being 240g / m 2 , pre-press at 3MPa for 30min, take out the plywood, put it in a hot press, and press it at 3MPa for 10min at a temperature of 120℃ to obtain the plywood.

[0032] Example 2

[0033] This embodiment provides a high-strength starch adhesive and uses it in the preparation of plywood.

[0034] The method for preparing the high-strength starch adhesive for artificial panels provided in this embodiment comprises the following steps:

[0035] Step 1, preparing the prefabricated material: 100 parts of oxidized starch, 80 parts of gelatin and 800 parts of distilled water are fully mixed, stirred in a 70°C water bath for 30 minutes, and then 15 parts of bisphenol A diglycidyl ether are added, and the reaction is continued at 80°C for 2 hours to obtain the prefabricated material;

[0036] Step 2, preparing starch adhesive: when using, 100 parts of the prefabricated material prepared in step 1, 50 parts of dry starch and 10 parts of polymethylene polyphenyl isocyanate are mixed and stirred evenly to obtain starch adhesive.

[0037] The starch adhesive prepared in this example is used to prepare plywood, and the specific method is as follows:

[0038] Apply starch adhesive evenly on the wood veneer, with the amount of adhesive applied on one side of the board being 240g / m 2 , pre-press at 3MPa for 30min, take out the plywood, put it in a hot press, and press it at 3MPa for 10min at a temperature of 120℃ to obtain the plywood.

[0039] Example 3

[0040] This embodiment provides a high-strength starch adhesive and uses it in the preparation of plywood.

[0041] The method for preparing the high-strength starch adhesive for artificial panels provided in this embodiment comprises the following steps:

[0042] Step 1, preparing the prefabricated material: 100 parts of oxidized starch, 80 parts of gelatin and 800 parts of distilled water are fully mixed, stirred in a 70°C water bath for 30 minutes, and then 15 parts of alkyl glycidyl ether are added, and the reaction is continued at 70°C with stirring for 2 hours to obtain the prefabricated material;

[0043] Step 2, preparing starch adhesive: when using, 100 parts of the prefabricated material prepared in step 1, 50 parts of dry starch and 10 parts of polymethylene polyphenyl isocyanate are mixed and stirred evenly to obtain starch adhesive.

[0044] The starch adhesive prepared in this example is used to prepare plywood, and the specific method is as follows:

[0045] Apply starch adhesive evenly on the wood veneer, with the amount of adhesive applied on one side of the board being 240g / m 2, pre-press at 3MPa for 30min, take out the plywood, put it in a hot press, and press it at 3MPa for 10min at a temperature of 120℃ to obtain the plywood.

[0046] Example 4

[0047] This embodiment provides a high-strength starch adhesive and uses it in the preparation of plywood.

[0048] The method for preparing the high-strength starch adhesive for artificial panels provided in this embodiment comprises the following steps:

[0049] Step 1, preparing the prefabricated material: 100 parts of oxidized starch, 50 parts of gelatin and 800 parts of distilled water are fully mixed, stirred in a 75°C water bath for 30 minutes, and then 20 parts of alkyl glycidyl ether are added, and the reaction is continued under stirring at 75°C for 2 hours to obtain the prefabricated material;

[0050] Step 2, preparing starch adhesive: when using, 100 parts of the prefabricated material prepared in step 1, 50 parts of dry starch and 10 parts of polymethylene polyphenyl isocyanate are mixed and stirred evenly to obtain starch adhesive.

[0051] The starch adhesive prepared in this example is used to prepare plywood, and the specific method is as follows:

[0052] Apply starch adhesive evenly on the wood veneer, with the amount of adhesive applied on one side of the board being 240g / m 2 , pre-press at 3MPa for 30min, take out the plywood, put it in a hot press, and press it at 3MPa for 10min at a temperature of 120℃ to obtain the plywood.

[0053] Example 5

[0054] This embodiment provides a high-strength starch adhesive and uses it in the preparation of plywood.

[0055] The method for preparing the high-strength starch adhesive for artificial panels provided in this embodiment comprises the following steps:

[0056] Step 1, preparing the prefabricated material: 100 parts of oxidized starch, 80 parts of gelatin and 800 parts of distilled water are fully mixed, stirred in a 70°C water bath for 30 minutes, and then 20 parts of polyethylene glycol diglycidyl ether are added, and the reaction is continued under stirring at 75°C for 2 hours to obtain the prefabricated material;

[0057] Step 2, preparing starch adhesive: when using, 100 parts of the prefabricated material prepared in step 1, 50 parts of dry starch and 10 parts of polymethylene polyphenyl isocyanate are mixed and stirred evenly to obtain starch adhesive.

[0058] The starch adhesive prepared in this example is used to prepare plywood, and the specific method is as follows:

[0059] Apply starch adhesive evenly on the wood veneer, with the amount of adhesive applied on one side of the board being 240g / m 2 , pre-press at 3MPa for 30min, take out the plywood, put it in a hot press, and press it at 3MPa for 10min at a temperature of 120℃ to obtain the plywood.

[0060] Example 6

[0061] This embodiment provides a high-strength starch adhesive and uses it in the preparation of plywood.

[0062] The method for preparing the high-strength starch adhesive for artificial panels provided in this embodiment comprises the following steps:

[0063] Step 1, preparing the prefabricated material: 100 parts of oxidized starch, 80 parts of gelatin and 800 parts of distilled water are fully mixed, stirred in a 70°C water bath for 30 minutes, and then 15 parts of polyethylene glycol diglycidyl ether are added, and the reaction is continued under stirring at 75°C for 2 hours to obtain the prefabricated material;

[0064] Step 2, preparing starch adhesive: when using, 100 parts of the prefabricated material prepared in step 1, 70 parts of dry starch and 10 parts of polymethylene polyphenyl isocyanate are mixed and stirred evenly to obtain starch adhesive.

[0065] The starch adhesive prepared in this example is used to prepare plywood, and the specific method is as follows:

[0066] Apply starch adhesive evenly on the wood veneer, with the amount of adhesive applied on one side of the board being 240g / m 2 , pre-press at 3MPa for 30min, take out the plywood, put it in a hot press, and press it at 3MPa for 10min at a temperature of 120℃ to obtain the plywood.

[0067] Example 7

[0068] This embodiment provides a high-strength starch adhesive and uses it in the preparation of plywood.

[0069] The method for preparing the high-strength starch adhesive for artificial panels provided in this embodiment comprises the following steps:

[0070] Step 1, preparing the prefabricated material: 100 parts of oxidized starch, 80 parts of gelatin and 800 parts of distilled water are fully mixed, stirred in a 70°C water bath for 30 minutes, and then 15 parts of polyethylene glycol diglycidyl ether are added, and the reaction is continued under stirring at 75°C for 2 hours to obtain the prefabricated material;

[0071] Step 2, preparing starch adhesive: when using, 100 parts of the prefabricated material prepared in step 1, 50 parts of dry starch and 15 parts of polymethylene polyphenyl isocyanate are mixed and stirred evenly to obtain starch adhesive.

[0072] The starch adhesive prepared in this example is used to prepare plywood, and the specific method is as follows:

[0073] Apply starch adhesive evenly on the wood veneer, with the amount of adhesive applied on one side of the board being 240g / m 2 , pre-press at 3MPa for 30min, take out the plywood, put it in a hot press, and press it at 3MPa for 10min at a temperature of 120℃ to obtain the plywood.

[0074] Comparative Example 1

[0075] This comparative example provides a starch adhesive and uses it in the preparation of plywood.

[0076] The preparation method of the starch adhesive provided in this comparative example comprises the following steps:

[0077] Step 1, preparing the prefabricated material: 100 parts of oxidized starch, 80 parts of gelatin and 800 parts of distilled water are fully mixed, stirred in a 70°C water bath for 30 minutes, and then continued to stir at 75°C for 2 hours to obtain the prefabricated material;

[0078] Step 2, preparing starch adhesive: when using, 100 parts of the prefabricated material prepared in step 1, 50 parts of dry starch and 10 parts of polymethylene polyphenyl isocyanate are mixed and stirred evenly to obtain starch adhesive.

[0079] The starch adhesive prepared in this comparative example is used for the preparation of plywood, and the specific method is as follows:

[0080] Apply starch adhesive evenly on the wood veneer, with the amount of adhesive applied on one side of the board being 240g / m 2 , pre-press at 3MPa for 30min, take out the plywood, put it in a hot press, and press it at 3MPa for 10min at a temperature of 120℃ to obtain the plywood.

[0081] The bonding performance of the starch adhesives prepared using Examples 1 to 7 and Comparative Example 1 was tested. According to the national standard GB / T17657-2013 "Test methods for physical and chemical properties of wood-based panels and veneer wood-based panels", the shear strength of the plywood in the dry state and the wet state was tested, and the dry shear strength and wet shear strength data of the plywood obtained are shown in Table 1.

[0082] Table 1

[0083] type Dry strength (MPa) Wet strength (MPa) Comparative Example 1 1.56±0.16 0.19±0.02 Example 1 7.93±0.03 1.40±0.13 Example 2 2.38±0.29 0.80±0.05 Example 3 2.65±0.35 0.46±0.09 Example 4 7.73±0.39 0.33±0.04 Example 5 2.63±0.58 1.64±0.15 Example 6 6.30±0.39 1.99±0.33 Example 7 7.91±0.03 2.00±0.24

[0084] From the comparison of the data in Table 1, it can be seen that the starch adhesive prepared by the present invention has the advantages of high bonding strength, good water resistance, no formaldehyde generation, environmental friendliness, low cost, etc., meets the national requirements for Class II boards, and has broad market prospects in the field of artificial board manufacturing.

[0085] Figure 1-Figure 3 The photographs of the fracture surfaces of the boards after the wet strength tensile test of the adhesives prepared in Example 1, Example 5 and Comparative Example 1 are shown in sequence; it can be seen from the fracture surfaces of the boards that the high-strength starch adhesive prepared by the present invention has good bonding strength and wood breakage rate, and the wet strength is increased from 0.19 MPa to 1.40 MPa and 1.64 MPa, and the bonding stability in a humid environment is significantly improved.

Claims

1. A high-strength starch adhesive for artificial boards, characterized in that: The prefabricated material comprises the following components in parts by weight: 100 parts of prefabricated material, 30 to 70 parts of dry starch and 10 to 30 parts of isocyanate; the prefabricated material comprises the following components in parts by weight: 60 to 100 parts of oxidized starch, 80 to 100 parts of gelatin, 10 to 30 parts of a cross-linking agent and 600 to 1000 parts of distilled water.

2. The high-strength starch adhesive for artificial boards according to claim 1, characterized in that: The crosslinking agent is one or a combination of polyethylene glycol diglycidyl ether, bisphenol A diglycidyl ether, long-chain alkyl glycidyl ether, neopentyl glycol diglycidyl ether, polypropylene oxide diglycidyl ether, glycerol diglycidyl ether or 1,4-butanediol glycidyl ether.

3. A high-strength starch adhesive for artificial boards according to claim 1 or 2, characterized in that: The isocyanate is one or a combination of polymethylene polyphenyl isocyanate, toluene diisocyanate TDI, isophorone diisocyanate IPDI, diphenylmethane diisocyanate MDI, dicyclohexylmethane diisocyanate HMDI, hexamethylene diisocyanate HDI or lysine diisocyanate.

4. A method for preparing a high-strength starch adhesive for artificial panels as claimed in any one of claims 1 to 3, characterized in that: The steps include: Step 1: preparing the prefabricated material: fully mixing and stirring the oxidized starch, gelatin and distilled water, and then adding a cross-linking agent and continuing the reaction for a certain period of time to obtain the prefabricated material; Step 2: preparing starch adhesive: when using, the prefabricated material prepared in step 1, dry starch and isocyanate are mixed and stirred evenly according to parts by mass to obtain starch adhesive.

5. The method for preparing the high-strength starch adhesive for artificial panels according to claim 4, characterized in that: The thorough mixing and stirring in step 1 is thorough stirring at 60-80° C. for 30 minutes.

6. The method for preparing the high-strength starch adhesive for artificial panels according to claim 4 or 5, characterized in that: The continued reaction in step 1 is carried out at 60-80° C. for 2-4 hours.

7. A method for using the high-strength starch adhesive for artificial panels as claimed in any one of claims 1 to 3, characterized in that: When using, apply the starch adhesive evenly on the wood veneer, and the amount of glue applied on one side of the board is 200-300g / m 2 , the bonding is completed after pre-pressing and hot pressing.

8. The method for using the high-strength starch adhesive for artificial panels according to claim 7, characterized in that: The pre-pressing is performed under a pressure of 2 to 5 MPa for 30 minutes.

9. The method for using the high-strength starch adhesive for artificial panels according to claim 8, characterized in that: The hot pressing is performed by using a hot press machine at a temperature of 110 to 130° C. and a pressure of 2 to 3 MPa for 10 minutes.

10. The method for using the high-strength starch adhesive for artificial panels according to claim 9, characterized in that: It also includes placing the hot-pressed artificial board in an environment for 24 hours to eliminate internal stress.

Citation Information

Patent Citations

  • Method for preparing aldehyde-free veneer boards by biological oil starch adhesives

    CN102642222A

  • Natural polymer water-soluble adhesive and preparation method thereof

    CN103074006A

  • Oxidized starch adhesive and preparation method thereof

    CN104861892A

  • Adhesive for artificial board and preparation method of adhesive

    CN105153998A

  • Preparation method of environment-friendly adhesive

    CN108314975A