Medium-temperature temperature-resistant clean fracturing fluid thickening agent as well as preparation method and application thereof

By using nanocellulose modified polyacrylamide and octadecylamine polyoxyethylene ether biquaternary ammonium salts in thickening agents, the problem of insufficient temperature resistance and shear resistance of existing thickening agents was solved, and the preparation It produces medium-temperature temperature-resistant clean fracturing liquid thickening agent with excellent temperature resistance and shear resistance, which is suitable for oil and gas exploration and development.

CN119081671AInactive Publication Date: 2024-12-06SANYA HONGYI PETROLEUM TECHNOLOGY CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411189565.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing synthetic thickeners have insufficient temperature resistance and shear resistance during oil layer fracturing, which cannot meet the application needs of higher requirements.

Method used

Using nanocellulose modified polyacrylamide and octadecylamine polyoxyethylene ether biquaternary ammonium salt as thickener, the medium temperature-resistant clean fracturing liquid thickener is prepared through specific polymerization and mixing steps. Enhance its mechanical strength and viscoelasticity.

Benefits of technology

It significantly improves the temperature resistance and shear resistance of the thickener, so that it maintains stable viscosity and thickening properties under high temperature and shear conditions, making it more suitable for fracturing applications in oil and gas exploration and development.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081671A_ABST
    Figure CN119081671A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of oil production engineering, and discloses a medium-temperature temperature-resistant clean fracturing fluid thickening agent as well as a preparation method and application thereof. The medium-temperature temperature-resistant clean fracturing fluid thickening agent is prepared from the following components in percentage by mass: 28 to 32 percent of nanocellulose modified polyacrylamide, 20 to 25 percent of octadecylamine polyoxyethylene ether biquaternary ammonium salt, 1 to 2 percent of dispersing agent and the balance of organic solvent, the preparation of the nano cellulose modified polyacrylamide comprises the following steps: mixing N-tert-butyl acrylamide, acrylamide, cellulose nano fibrils and water to obtain a mixed solution; and mixing the mixed solution with an initiator, and carrying out polymerization reaction to obtain the nano-cellulose modified polyacrylamide. After a network structure of the medium-temperature temperature-resistant clean fracturing fluid thickening agent is formed, the shear stability viscosity of the medium-temperature temperature-resistant clean fracturing fluid thickening agent is improved, the viscosity increasing and thickening performance of a polymer is better, and the medium-temperature temperature-resistant clean fracturing fluid thickening agent is more beneficial to carrying and migration of a proppant; the temperature resistance and the shearing resistance are excellent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of oil production engineering, and in particular to a medium-temperature heat-resistant clean fracturing fluid thickener and a preparation method and application thereof. Background Art

[0002] The process of hydraulic fracturing of oil layers is to use a high-pressure and large-displacement pump on the ground, and use the principle of liquid pressure transmission to inject a liquid with a certain viscosity, usually called fracturing fluid, into the oil layer at a pressure greater than the absorption capacity of the oil layer, and gradually increase the pressure in the wellbore, thereby creating high pressure at the bottom of the well. When this pressure is greater than the ground stress near the well wall and the tensile strength of the formation rock, cracks will be generated in the formation near the bottom of the well; continue to inject sand-carrying fluid with proppants, the cracks will extend forward and be filled with proppants, and after the well is shut down, the cracks will close on the proppants, thereby forming sand-filled cracks with certain geometric dimensions and high conductivity in the formation near the bottom of the well, so that the well can achieve the purpose of increasing production and injection. Thickener is the main additive in fracturing fluid. During fracturing operations, the thickener swells into a sol in water, and forms a high-viscosity gel after cross-linking, thereby achieving pressure transmission, formation of formation cracks and transport of proppants along the opened cracks.

[0003] Although the existing synthetic thickeners are low-cost, they have disadvantages such as poor temperature resistance, poor shear resistance, and low mechanical strength. For example, Chinese invention patent CN103951593A discloses a medium-temperature clean fracturing fluid thickener. Although the fracturing fluid thickener is easily degraded, its temperature resistance is poor. Another example is Chinese invention patent CN116396742A discloses a clean fracturing fluid thickener. Although it improves the temperature resistance and shear resistance of the fracturing fluid thickener, the improvement effect is not obvious and cannot meet higher requirements.

[0004] Therefore, it is of great significance to develop a medium-temperature resistant clean fracturing fluid thickener with excellent temperature resistance and strong shear resistance. Summary of the invention

[0005] In view of this, the present invention provides a medium-temperature heat-resistant clean fracturing fluid thickener and a preparation method and application thereof, so as to solve the problem that the existing artificial synthetic thickeners have low costs but have disadvantages such as poor temperature resistance and shear resistance.

[0006] In order to achieve the above object, the present invention adopts the following technical solution:

[0007] The present invention provides a medium-temperature heat-resistant clean fracturing fluid thickener, comprising the following components in percentage by mass:

[0008] Nanocellulose modified polyacrylamide 28-32%, octadecylamine polyoxyethylene ether diquaternary ammonium salt 20-25%, dispersant 1-2%, and the balance is organic solvent;

[0009] The preparation of nanocellulose modified polyacrylamide comprises the following steps:

[0010] N-tert-butyl acrylamide, acrylamide, cellulose nanofibrils and water are mixed to obtain a mixed solution; the mixed solution is mixed with an initiator and then subjected to polymerization reaction to obtain nanocellulose modified polyacrylamide.

[0011] Preferably, the dispersant includes one or more of Tween 40, Tween 60 and Tween 80.

[0012] Preferably, the organic solvent includes one or more of methanol, ethanol, isopropanol and ethylene glycol.

[0013] Preferably, the specific steps of mixing N-tert-butylacrylamide, acrylamide, cellulose nanofibrils and water are:

[0014] Firstly, N-tert-butylacrylamide, cellulose nanofibrils and water are homogeneously mixed, and then acrylamide is added thereto.

[0015] Preferably, the mass ratio of the N-tert-butylacrylamide, acrylamide and cellulose nanofibrils is 1:5-8:0.02-0.05; and the dosage ratio of the cellulose nanofibrils and water is 0.02-0.05 g:10-15 mL.

[0016] Preferably, the initiator comprises ammonium persulfate and / or sodium bisulfite; and the mass ratio of the N-tert-butylacrylamide to the initiator is 1:0.05-0.07.

[0017] Preferably, the polymerization reaction temperature is 60-70° C., and the polymerization reaction time is 4-6 hours.

[0018] The present invention also provides a method for preparing the medium-temperature heat-resistant clean fracturing fluid thickener, comprising the following steps:

[0019] The nanocellulose modified polyacrylamide, the dispersant and the organic solvent are first mixed, and then octadecylamine polyoxyethylene ether diquaternary ammonium salt is added thereto for second mixing to obtain a medium-temperature resistant clean fracturing fluid thickener.

[0020] Preferably, the stirring speed of the first mixing is 200-300 r / min; the stirring speed of the second mixing is 400-500 r / min; and the time of the first mixing and the second mixing is independently 20-40 min.

[0021] The present invention also provides application of the medium-temperature heat-resistant clean fracturing fluid thickener in oil and gas exploration and development.

[0022] It can be seen from the above technical solution that compared with the prior art, the present invention has the following beneficial effects:

[0023] (1) In the nanocellulose modified polyacrylamide, the polymer formed by N-tert-butyl acrylamide and acrylamide forms a steric hindrance in aqueous solution by relying on the branched groups on the molecular side chains, thereby enhancing the rigidity of the molecular chain and improving the mechanical strength. The introduction of nanocellulose crystals into the polymer further enhances the mechanical strength of the polymer, thereby improving the temperature resistance and shear strength of the obtained medium-temperature resistant clean fracturing fluid thickener.

[0024] (2) In the medium-temperature heat-resistant clean fracturing fluid thickener, octadecylamine polyoxyethylene ether diquaternary ammonium salt has two cationic sites, which can easily form unique worm-like micelles in water, making its aqueous solution have excellent viscoelasticity and shear resistance; at the same time, the active groups carried by octadecylamine polyoxyethylene ether diquaternary ammonium salt itself will combine with the active groups in the nanocellulose modified polyacrylamide structure, so that octadecylamine polyoxyethylene ether diquaternary ammonium salt enters the nanocellulose modified polyacrylamide structure, further improving the temperature resistance and shear strength of the obtained medium-temperature clean fracturing fluid thickener.

[0025] (3) The medium-temperature heat-resistant clean fracturing fluid thickener obtained by the present invention has excellent temperature resistance and shear resistance. After the network structure of the medium-temperature heat-resistant clean fracturing fluid thickener of the present invention is formed, its shear stable viscosity is improved, the polymer viscosity and thickening performance are better, and it is more conducive to the carrying and migration of the proppant. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0027] Figure 1 The present invention is a flow chart for preparing the medium-temperature heat-resistant clean fracturing fluid thickener. DETAILED DESCRIPTION

[0028] The present invention provides a medium-temperature heat-resistant clean fracturing fluid thickener, comprising the following components in percentage by mass:

[0029] Nanocellulose modified polyacrylamide 28-32%, octadecylamine polyoxyethylene ether diquaternary ammonium salt 20-25%, dispersant 1-2%, and the balance is organic solvent;

[0030] The preparation of nanocellulose modified polyacrylamide comprises the following steps:

[0031] N-tert-butyl acrylamide, acrylamide, cellulose nanofibrils and water are mixed to obtain a mixed solution; the mixed solution is mixed with an initiator and then subjected to polymerization reaction to obtain nanocellulose modified polyacrylamide.

[0032] In the present invention, the dosage of the nanocellulose modified polyacrylamide is preferably 29-31%, more preferably 30%; the dosage of the octadecylamine polyoxyethylene ether diquaternary ammonium salt is preferably 21-24%, more preferably 22-23%; the dosage of the dispersant is preferably 1.5%; the balance is organic solvent.

[0033] In the present invention, the dispersant includes one or more of Tween 40, Tween 60 and Tween 80.

[0034] In the present invention, the organic solvent includes one or more of methanol, ethanol, isopropanol and ethylene glycol.

[0035] In the present invention, the specific steps of mixing N-tert-butylacrylamide, acrylamide, cellulose nanofibrils and water are:

[0036] Firstly, N-tert-butylacrylamide, cellulose nanofibrils and water are homogeneously mixed, and then acrylamide is added thereto.

[0037] In the present invention, the mass ratio of N-tert-butylacrylamide, acrylamide and cellulose nanofibrils is preferably 1:5-8:0.02-0.05, and more preferably 1:6-7:0.03-0.04; the dosage ratio of cellulose nanofibrils and water is preferably 0.02-0.05g:10-15mL, and more preferably 0.03-0.04g:12-14mL.

[0038] In the present invention, the initiator comprises ammonium persulfate and / or sodium bisulfite; the mass ratio of the N-tert-butylacrylamide to the initiator is preferably 1:0.05-0.07, and more preferably 1:0.06-0.065.

[0039] In the present invention, the polymerization reaction temperature is preferably 60-70°C, more preferably 62-68°C, more preferably 63-65°C; the polymerization reaction time is preferably 4-6h, more preferably 4.5-5.5h, more preferably 5h.

[0040] In the present invention, after the polymerization reaction is completed, the obtained product is dried; the drying temperature is preferably 50 to 80°C, more preferably 60 to 75°C, and more preferably 65 to 70°C.

[0041] The present invention also provides a method for preparing the medium-temperature heat-resistant clean fracturing fluid thickener, comprising the following steps:

[0042] The nanocellulose modified polyacrylamide, the dispersant and the organic solvent are first mixed, and then octadecylamine polyoxyethylene ether diquaternary ammonium salt is added thereto for second mixing to obtain a medium-temperature resistant clean fracturing fluid thickener.

[0043] In the present invention, the stirring speed of the first mixing is preferably 200-300 r / min, more preferably 220-280 r / min, more preferably 250-260 r / min; the stirring speed of the second mixing is preferably 400-500 r / min, more preferably 420-480 r / min, more preferably 450-460 r / min; the time of the first mixing and the second mixing is independently preferably 20-40 min, more preferably 25-35 min, more preferably 30 min.

[0044] The present invention also provides application of the medium-temperature heat-resistant clean fracturing fluid thickener in oil and gas exploration and development.

[0045] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0046] Example 1

[0047] Preparation of nanocellulose modified polyacrylamide: 4 g of N-tert-butyl acrylamide, 0.2 g of cellulose nanofibrils and 40 mL of water were homogenized by a homogenizer, and then 20 g of acrylamide was added thereto to obtain a mixed solution; the mixed solution was mixed with 0.2 g of ammonium persulfate and then polymerized at 65° C. for 5.5 h, and vacuum dried at 65° C. to obtain nanocellulose modified polyacrylamide;

[0048] Preparation of medium temperature resistant clean fracturing fluid thickener:

[0049] Raw materials: 32% nanocellulose modified polyacrylamide, 25% octadecylamine polyoxyethylene ether diquaternary ammonium salt, 1% Tween 40, and the balance is methanol;

[0050] Method: According to the above-mentioned raw material dosages, nanocellulose modified polyacrylamide, Tween 40 and methanol are first mixed, the stirring speed of the first mixing is 250r / min, and the first mixing time is 30min. Then, octadecylamine polyoxyethylene ether diquaternary ammonium salt is added thereto for second mixing, the stirring speed of the second mixing is 450r / min, and the second mixing time is 35min, to obtain a medium-temperature resistant clean fracturing fluid thickener.

[0051] Example 2

[0052] Preparation of nanocellulose modified polyacrylamide: 5 g of N-tert-butyl acrylamide, 0.1 g of cellulose nanofibrils and 50 mL of water were homogenized by a homogenizer, and then 25 g of acrylamide was added thereto to obtain a mixed solution; the mixed solution was mixed with 0.25 g of ammonium persulfate and then polymerized at 68° C. for 5 h, and then vacuum dried at 65° C. to obtain nanocellulose modified polyacrylamide;

[0053] Preparation of medium temperature resistant clean fracturing fluid thickener:

[0054] Raw materials: 30% nanocellulose modified polyacrylamide, 22% octadecylamine polyoxyethylene ether diquaternary ammonium salt, 1.5% Tween 80, and the balance is ethanol;

[0055] Method: According to the above-mentioned raw material dosages, nanocellulose modified polyacrylamide, Tween 80 and ethanol are first mixed at a stirring speed of 300 r / min and a first mixing time of 40 min. Then, octadecylamine polyoxyethylene ether diquaternary ammonium salt is added thereto for a second mixing at a stirring speed of 450 r / min and a second mixing time of 40 min to obtain a medium-temperature resistant clean fracturing fluid thickener.

[0056] Example 3

[0057] Preparation of nanocellulose modified polyacrylamide: 3 g of N-tert-butyl acrylamide, 0.12 g of cellulose nanofibrils and 36 mL of water were homogenized by a homogenizer, and then 15 g of acrylamide was added thereto to obtain a mixed solution; the mixed solution was mixed with 0.18 g of ammonium persulfate and then polymerized at 60° C. for 6 h, and then vacuum dried at 65° C. to obtain nanocellulose modified polyacrylamide;

[0058] Preparation of medium temperature resistant clean fracturing fluid thickener:

[0059] Raw materials: 28% nanocellulose modified polyacrylamide, 20% octadecylamine polyoxyethylene ether diquaternary ammonium salt, 1.5% Tween 80, and the balance is ethylene glycol;

[0060] Method: According to the above-mentioned raw material dosages, nanocellulose modified polyacrylamide, Tween 80 and ethylene glycol are first mixed at a stirring speed of 280 r / min and a first mixing time of 40 min. Then, octadecylamine polyoxyethylene ether diquaternary ammonium salt is added thereto for a second mixing at a stirring speed of 450 r / min and a second mixing time of 35 min to obtain a medium-temperature resistant clean fracturing fluid thickener.

[0061] Comparative Example 1

[0062] The difference from Example 1 is that the addition of cellulose nanofibrils is omitted during the preparation of nanocellulose-modified polyacrylamide. The rest is the same as Example 1.

[0063] Comparative Example 2

[0064] The difference from Example 1 is that the amount of cellulose nanofibrils used in the preparation of nanocellulose-modified polyacrylamide is 0.05 g. Others are the same as Example 1.

[0065] Comparative Example 3

[0066] The difference from Example 1 is that the amount of cellulose nanofibrils used in the preparation of nanocellulose-modified polyacrylamide is 0.4 g. The rest is the same as Example 1.

[0067] Comparative Example 4

[0068] The difference from Example 1 is that the amount of octadecylamine polyoxyethylene ether diquaternary ammonium salt used in the preparation of the medium-temperature heat-resistant clean fracturing fluid thickener is 17%. Others are the same as Example 1.

[0069] Comparative Example 5

[0070] The difference from Example 1 is that the amount of octadecylamine polyoxyethylene ether diquaternary ammonium salt used in the preparation of the medium-temperature heat-resistant clean fracturing fluid thickener is 28%. Others are the same as Example 1.

[0071] Comparative Example 6

[0072] The difference from Example 1 is that the stirring speed of the first mixing in the preparation process of the medium-temperature heat-resistant clean fracturing fluid thickener is 450 r / min. The rest is the same as Example 1.

[0073] Comparative Example 7

[0074] The difference from Example 1 is that the stirring speed of the second mixing during the preparation of the medium-temperature heat-resistant clean fracturing fluid thickener is 250 r / min. The rest is the same as Example 1.

[0075] Performance testing and results:

[0076] (1) Shear resistance: at 25°C, 170s -1 The viscosity of the medium-temperature heat-resistant clean fracturing fluid thickeners obtained in Examples 1 to 3 and Comparative Examples 1 to 7 at 0 min and 60 min was tested by a rheometer while maintaining shearing;

[0077] (2) Degelling performance: 5% cyclohexane was added at 80° C. (simulated formation temperature) to test the viscosity of the medium-temperature resistant clean fracturing fluid thickeners obtained in Examples 1 to 3 and Comparative Examples 1 to 7 at 0 min and 360 min;

[0078] (3) Temperature resistance: The medium temperature heat resistant clean fracturing fluid thickeners obtained in Examples 1 to 3 and Comparative Examples 1 to 7 were treated at 90° C. for 30 min and at 170 s -1 The viscosity of the medium-temperature heat-resistant clean fracturing fluid thickeners obtained in Examples 1 to 3 and Comparative Examples 1 to 7 after constant temperature treatment at 0 min and 90 min was tested by a rheometer.

[0079] The above test results are shown in Table 1.

[0080] Table 1 Performance of the medium temperature resistant clean fracturing fluid thickener obtained in Examples 1 to 3 and Comparative Examples 1 to 7

[0081]

[0082] It can be seen from Table 1 that the medium-temperature heat-resistant clean fracturing fluid thickener obtained by the present invention has excellent temperature resistance and shear resistance; after the network structure of the medium-temperature heat-resistant clean fracturing fluid thickener of the present invention is formed, its shear stable viscosity is improved, the polymer viscosity and thickening performance are better, and it is more conducive to the carrying and migration of the proppant.

[0083] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A medium temperature resistant clean fracturing fluid thickener, characterized in that: The components include the following mass percentages: Nanocellulose modified polyacrylamide 28-32%, octadecylamine polyoxyethylene ether diquaternary ammonium salt 20-25%, dispersant 1-2%, and the balance is organic solvent; The preparation of nanocellulose modified polyacrylamide comprises the following steps: N-tert-butyl acrylamide, acrylamide, cellulose nanofibrils and water are mixed to obtain a mixed solution; the mixed solution is mixed with an initiator and then subjected to polymerization reaction to obtain nanocellulose modified polyacrylamide.

2. The medium temperature resistant clean fracturing fluid thickener according to claim 1, characterized in that: The dispersant includes one or more of Tween 40, Tween 60 and Tween 80.

3. The medium temperature resistant clean fracturing fluid thickener according to claim 1 or 2, characterized in that: The organic solvent includes one or more of methanol, ethanol, isopropanol and ethylene glycol.

4. The medium temperature resistant clean fracturing fluid thickener according to claim 3, characterized in that: The specific steps of mixing N-tert-butylacrylamide, acrylamide, cellulose nanofibrils and water are as follows: Firstly, N-tert-butylacrylamide, cellulose nanofibrils and water are homogeneously mixed, and then acrylamide is added thereto.

5. The medium temperature resistant clean fracturing fluid thickener according to claim 4, characterized in that: The mass ratio of N-tert-butyl acrylamide, acrylamide and cellulose nanofibrils is 1:5-8:0.02-0.05; the dosage ratio of cellulose nanofibrils and water is 0.02-0.05 g:10-15 mL.

6. The medium temperature resistant clean fracturing fluid thickener according to claim 4 or 5, characterized in that: The initiator includes ammonium persulfate and / or sodium bisulfite; the mass ratio of the N-tert-butylacrylamide to the initiator is 1:0.05-0.

07.

7. The medium temperature resistant clean fracturing fluid thickener according to claim 1, 2, 4 or 5, characterized in that: The polymerization reaction temperature is 60-70° C., and the polymerization reaction time is 4-6 hours.

8. The method for preparing the medium-temperature heat-resistant clean fracturing fluid thickener according to any one of claims 1 to 7, characterized in that: The steps include: The nanocellulose modified polyacrylamide, the dispersant and the organic solvent are first mixed, and then octadecylamine polyoxyethylene ether diquaternary ammonium salt is added thereto for second mixing to obtain a medium-temperature resistant clean fracturing fluid thickener.

9. The method for preparing the medium-temperature heat-resistant clean fracturing fluid thickener according to claim 8, characterized in that: The stirring speed of the first mixing is 200-300 r / min; the stirring speed of the second mixing is 400-500 r / min; and the time of the first mixing and the second mixing is independently 20-40 min.

10. Use of the medium-temperature, heat-resistant and clean fracturing fluid thickener according to any one of claims 1 to 7 in oil and gas exploration and development.