Preparation method and application method of straw iron composite photosensitive salt absorption material

By ultrasonic reaction of straw cellulose with persulfate and ferrous ions and adding organic acids, straw iron composite photosensitive salt absorption material is prepared, which solves the harm of salt-alkali soil salt on crops and improves the salt ion adsorption capacity of the material , the improvement of saline-alkali land and the reduction of salinization risks have been achieved.

CN119081705APending Publication Date: 2024-12-06SHIHEZI UNIVERSITY
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411181729.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The prior art is difficult to effectively improve the salt absorption and control ability of straw to soil salt, resulting in the harm of soil salt in saline-alkali land to crop growth.

Method used

By pretreating straw cellulose, using persulfate composite solution and ferrous ions, performing ultrasonic reaction, adding organic acid solution to prepare straw iron composite photosensitive salt absorbing material, which improves the adsorption ability of salt ions under natural light , used to cover saline-alkali surfaces and reduce the risk of soil salinization.

Benefits of technology

It significantly improves the salt ion adsorption capacity of the material under natural light, effectively alleviates the problem of salinization in saline-alkali land, and reduces the harm to crops.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081705A_ABST
    Figure CN119081705A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of straw resource utilization, and discloses a preparation method and an application method of a straw-iron composite photosensitive salt absorption material. The method comprises the following steps: pretreating straws by using a persulfate composite solution, adding a ferrous ion composite solution, carrying out an ultrasonic reaction to obtain a straw iron-containing precursor substance, then adding an organic acid composite solution, and continuously reacting at a certain temperature to synthesize the straw iron composite photosensitive material. According to the composite material, the salt absorption capacity of the material can be improved through regulation and control of a self-structure microdomain under natural illumination. The composite material can be applied to improvement of saline-alkali soil and alleviation of the risk of soil salinization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of straw resource utilization and relates to a method for preparing a straw-iron composite photosensitive salt-absorbing material and an application method thereof. Background Art

[0002] my country produces about 1 billion tons of straw every year. The efficient utilization of straw resources is an important way to solve the problem of straw pollution. Straw fertilizer, feed, base material, energy and material are the main utilization methods of straw biomass materials. Among them, the preparation of high-performance environmental remediation materials after straw modification is an important means to increase its added value. For example, patent CN202410383539.3 discloses a super-hydrophobic esterified modified corn straw aerogel oil absorption material and a preparation method thereof. The straw cellulose pretreated with alkaline hydrogen peroxide is treated with an acetic acid-formic acid mixed solution to obtain an esterified modified corn straw, which is reacted through an aerogel process to obtain a super-hydrophobic esterified modified corn straw aerogel oil absorption material. Patent CN202410096992.6 discloses a method for predicting the salt absorption rate of decomposed straw in soil. By measuring the adsorption capacity of straw with different decomposition degrees to salt ions, a prediction equation for the salt absorption rate of straw is constructed. Patent CN202111092323.4 discloses a method for preparing calcium-modified straw biochar and a method for using it to simultaneously adsorb phosphate and tetracycline. After the straw is fully soaked in a calcium chloride solution, it is calcined at high temperature to obtain a calcium-modified straw biochar material with simultaneous adsorption of phosphate and tetracycline. Patent CN202111423639.7 discloses a method for preparing highly adsorbable corn straw charcoal and its application in the preparation of sustained-release drug preparations. The straw is mixed and ground with an alkaline solution containing potassium pyrophosphate and triethanolamine, and then calcined at high temperature under anaerobic conditions to obtain a biomass charcoal material with high adsorption performance. Therefore, the straw can be synthesized into a biomass material with a certain adsorption capacity through simple modification and treatment.

[0003] At present, my country has 478 million mu of saline-alkali arable land available. To make efficient use of these saline-alkali lands, we must first control the salinity in the soil and minimize the impact of soil salinity on crop growth. As a biomass resource, Li Yuyi et al. of the Chinese Academy of Agricultural Sciences (Journal of the Chinese Society of Agricultural Engineering, 2013, 29(23)) used straw return to the field to create a straw interlayer in the tillage layer through deep straw plowing and mulching, which hindered the upward movement of soil salt under the tillage layer, thereby creating a good habitat environment for the crop tillage layer. If the ability of straw to absorb and control soil salt can be further improved, the harm of soil salt to crops will be greatly reduced. Straw contains a large number of hydroxyl groups, which can produce carbonyl groups with salt ion coordination after oxidation modification. Therefore, the present invention pre-treats straw using a persulfate composite solution, adds a certain proportion of a ferrous ion mixed solution, and oxidizes straw cellulose by ultrasonic mild reaction at room temperature to prepare a straw iron-containing precursor material, and then adds an organic acid composite solution, fully reacts at a certain temperature, and synthesizes a straw iron composite photosensitive material. Under natural light conditions, the composite material has an increased adsorption capacity for salt ions. Covering the composite material on the surface of saline-alkali land can achieve the effect of reducing alkali and suppressing salt, and alleviate the harm of soil salinization. Summary of the invention

[0004] The present invention adopts agricultural waste biomass resources to establish a method for preparing a straw iron composite photosensitive salt absorption material and its application. The method uses a persulfate composite solution to pretreat the straw, adds a ferrous ion composite solution, and obtains a straw iron-containing precursor material through ultrasonic reaction, and then adds an organic acid composite solution, and continues to react at a certain temperature to synthesize a straw iron composite photosensitive material. The composite material can improve the salt absorption capacity of the material through the regulation of its own structural microdomain under natural light. The composite material can be applied to saline-alkali land improvement to alleviate the risk of soil salinization.

[0005] The technical solution of the present invention:

[0006] A method for preparing a straw-iron composite photosensitive salt-absorbing material, comprising the following steps:

[0007] (1) After crushing fresh straw waste with a grass cutter, drying and dehydrating the straw at 50-60° C., crushing the straw into 50-200 mesh straw; adding the crushed straw to the prepared persulfate composite solution A, the straw and the persulfate composite solution A are mixed according to a mass g: volume ml ratio of 1:20, the persulfate composite solution A is compounded from persulfate, maleic acid and salicylic acid, dark reaction is carried out at room temperature for 1-2 days, and then adding iron ion composite solution B, the iron ion composite solution B is compounded from ferric pyrophosphate, sodium thiosulfate and urea; placing the reaction container in an ultrasonic device, the ultrasonic temperature is 30° C., the frequency is 20 kHz, the reaction is fully carried out for 3-5 hours, standing and solid-liquid separation, and drying at 60-80° C. for 8-10 hours to obtain a straw iron-containing precursor;

[0008] (2) Add the straw iron-containing precursor obtained above to the prepared terephthalic acid and fumaric acid solution, and control the solid-liquid ratio at 1: (10-20), wherein the solid-liquid ratio is mass g: volume ml; ultrasonically treat for 10-20 minutes at room temperature, fully react at 110-140°C for 1-10 hours, cool to room temperature, separate the solid and liquid, wash the solid material with anhydrous ethanol, N,N-dimethylformamide, and pure water for 2-3 times in sequence, and dry at 60-80°C for 8-10 hours to obtain a straw iron composite photosensitive salt-absorbing material.

[0009] The straw iron composite photosensitive salt-absorbing material is put into the salt solution at a solid-liquid ratio of 1: (50-100), wherein the solid-liquid ratio is mass g: volume ml; the solubility range of the salt solution is 5-20g / L, and the salt ions in the solution include Na + , K + , Ca 2+ Mg 2+ , Cl - 、SO 4 2- , react for 5-8 hours under natural light conditions, perform solid-liquid separation, determine the salt content in the supernatant solution, and analyze the salt absorption of the composite material.

[0010] The straw-iron composite photosensitive salt-absorbing material is added at a rate of 0.8-1.5 kg per square meter and evenly spread on the surface of saline-alkali soil. The surface soil is taken at a set time, the total salt content of the soil is measured, and the desalination effect of the composite material is evaluated.

[0011] The persulfate in the persulfate composite solution A includes sodium persulfate, potassium persulfate and ammonium persulfate.

[0012] The mass percentages of persulfate, maleic acid and salicylic acid in the persulfate composite solution A are 1%-5.0%, 0.1%-0.5% and 0.1%-0.2% respectively.

[0013] The mass percentages of ferric pyrophosphate, sodium thiosulfate and urea in the ferrous ion composite solution B are 0.1%-0.5%, 0.05%-0.2% and 0.5%-1.0% respectively.

[0014] The masses of terephthalic acid and fumaric acid in the terephthalic acid and fumaric acid solutions are 0.1%-0.2% and 0.1%-0.4% of the mass of the straw respectively.

[0015] Beneficial effects of the present invention: The present invention uses waste biomass material straw, and sequentially pre-treats the straw with a persulfate composite solution to fully expose the hydroxyl groups of the straw fiber and increase the pore structure of the straw. Then, under the protective effect of urea molecules, the iron ions and the hydroxyl groups of the straw fibers form a stable hydrogen bond. Sodium thiosulfate further prevents the hydroxyl groups of the straw fibers from being oxidized, thereby increasing the stability of the straw fiber and iron ion system, and obtaining a straw iron-containing precursor substance. The substance is then added to an organic acid composite solution, and the reaction is continued at a certain temperature to obtain a straw iron composite photosensitive adsorption material. The composite material can improve the adsorption capacity of salt ions under natural light, thereby effectively removing salt from the surface of saline-alkali land and alleviating salt damage to crops. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 It is the salt absorption capacity of straw composite photosensitive material.

[0017] Figure 2 This is the application effect of straw composite photosensitive material. DETAILED DESCRIPTION

[0018] The specific implementation of the present invention is further described below in conjunction with the accompanying drawings and technical solutions.

[0019] Example 1 Effect of reaction temperature on salt absorption capacity of straw composite photosensitive material

[0020] Fresh straw waste is collected from farmland, crushed with a grass cutter, dried and dehydrated at 60°C, and crushed into 50-200 mesh materials with an ultrafine grinder. Take 20g of crushed straw and add it to 100mL of persulfate composite solution, in which the mass ratios of sodium persulfate, maleic acid and salicylic acid are 1.0%, 0.5% and 0.1% respectively. Dark reaction is carried out at room temperature for 1d, and then 20mL of ferrous ion composite solution is added, in which the mass proportions of ferric pyrophosphate, sodium thiosulfate and urea are 0.1%, 0.1% and 0.5% respectively. The reaction container is placed in an ultrasonic device, the ultrasonic temperature is 30°C, the frequency is 20kHz, and the reaction is fully carried out for 5h, then the solid-liquid separation is carried out, and the straw iron-containing precursor is obtained at 60°C for 10h. The prepared straw iron precursor material was added to 50 mL of organic acid solution, the mass of terephthalic acid and fumaric acid in the solution was 0.1 g and 0.3 g respectively, and ultrasonic treatment was performed at room temperature for 15 min, and the reaction was fully performed at 100°C, 120°C, and 160°C for 6 h. After cooling to room temperature, solid-liquid separation was performed, and the solid material was washed with anhydrous ethanol, N,N-dimethylformamide, and pure water for 2-3 times in sequence, and dried at 70°C for 10 h to obtain the straw iron composite photosensitive salt absorption material. The prepared composite materials were added to 50 mL of saline solution (salt content was 10 g / L), reacted under natural light for 5 h, and then solid-liquid separation was performed. The salt content in the supernatant solution was determined. The results are attached. Figure 1 The straw-iron composite photosensitive salt-absorbing material has a certain salt-absorbing capacity only under light, and the maximum salt absorption is 0.0415 g / g (composite material prepared under 120°C reaction temperature). With the increase of reaction temperature, the salt-absorbing capacity of the composite photosensitive material under light weakens.

[0021] Example 2 Effect of Sodium Persulfate Dosage on Salt Absorption Capacity of Straw Composite Photosensitive Material

[0022] Fresh straw waste is collected from farmland, crushed with a grass cutter, dried and dehydrated at 60°C, and crushed into 50-200 mesh materials with an ultrafine grinder. Take 20g of crushed straw and add it to 100mL of persulfate composite solution, in which the mass ratios of sodium persulfate, maleic acid and salicylic acid are 1.0%, 0.2% and 0.2% respectively. Dark reaction is carried out at room temperature for 1d, and then 20mL of ferrous ion composite solution is added, in which the mass proportions of ferric pyrophosphate, sodium thiosulfate and urea are 0.1%, 0.1% and 0.5% respectively. The reaction container is placed in an ultrasonic device, the ultrasonic temperature is 30°C, the frequency is 20kHz, and the reaction is fully carried out for 5h, then the solid-liquid separation is carried out, and the straw iron-containing precursor is obtained at 60°C for 10h. The prepared straw iron precursor material was added to 50 mL of organic acid solution, the mass of terephthalic acid and fumaric acid in the solution was 0.1 g and 0.3 g respectively, and ultrasonic was carried out for 15 min at room temperature, and fully reacted at 100 ° C for 6 h. After cooling to room temperature, solid-liquid separation was carried out, and the solid material was washed with anhydrous ethanol, N, N-dimethylformamide, and pure water for 2-3 times in sequence, and dried at 70 ° C for 10 h to obtain the straw iron composite photosensitive salt absorption material. According to the above synthesis method, only the amount of sodium persulfate was changed to 2%, 3%, 4% and 5% (mass ratio in the composite solution), and the straw iron composite photosensitive salt absorption material prepared under different sodium persulfate amounts was obtained. The results showed that under light conditions, with the increase of sodium persulfate dosage, the salt absorption of the prepared straw-iron composite photosensitive salt-absorbing material gradually increased, with a maximum of 0.0524g / g. Compared with non-light conditions, the salt absorption of the composite material increased by 45.3%, which further indicates that sodium persulfate can break the dense lignin fiber structure of straw and increase the material's loading capacity and binding force for iron.

[0023] Example 3 Effect of organic acid reaction time on salt absorption capacity of straw composite photosensitive material

[0024] Fresh straw waste is collected from farmland, crushed with a grass cutter, dried and dehydrated at 60°C, and crushed into 50-200 mesh materials with an ultrafine grinder. Take 20g of crushed straw and add it to 100mL of persulfate composite solution, in which the mass ratios of sodium persulfate, maleic acid and salicylic acid are 1.0%, 0.5% and 0.1% respectively. Dark reaction is carried out at room temperature for 1d, and then 20mL of ferrous ion composite solution is added, in which the mass proportions of ferric pyrophosphate, sodium thiosulfate and urea are 0.1%, 0.1% and 0.5% respectively. The reaction container is placed in an ultrasonic device, the ultrasonic temperature is 30°C, the frequency is 20kHz, and the reaction is fully carried out for 5h, then the solid-liquid separation is carried out, and the straw iron-containing precursor is obtained at 60°C for 10h. The prepared straw iron precursor material was added to 50 mL of organic acid solution, the mass of terephthalic acid and fumaric acid in the solution was 0.1 g and 0.3 g respectively, and ultrasonic was carried out for 15 min at room temperature, and fully reacted at 100 ° C for 1 h. After cooling to room temperature, solid-liquid separation was carried out, and the solid material was washed with anhydrous ethanol, N, N-dimethylformamide, and pure water for 2-3 times in sequence, and dried at 70 ° C for 10 h to obtain the straw iron composite photosensitive salt absorption material. According to the above synthesis method, only the organic acid reaction time was changed to 2h, 5h, 8h, and 10h, and the straw iron composite photosensitive salt absorption material prepared under different reaction times was obtained. The results showed that under light conditions, with the increase of organic acid reaction time, the salt absorption of the prepared straw-iron composite photosensitive salt-absorbing material showed an increasing trend, with a maximum of 0.0524g / g; among them, compared with non-light conditions, the salt absorption of the composite material increased by 58.2%, which further shows that adding organic acid can effectively improve the generation efficiency of straw-iron composite materials and improve the salt absorption capacity of the material.

[0025] Example 4 Effect of reaction time on salt absorption capacity of straw composite photosensitive material

[0026] Fresh straw waste is collected from farmland, crushed with a grass cutter, dried and dehydrated at 60°C, and crushed into 50-200 mesh materials with an ultrafine grinder. 10g of crushed straw is added to 50mL of persulfate composite solution, in which the mass ratios of sodium persulfate, maleic acid and salicylic acid are 2.0%, 0.4% and 0.2%, respectively. Dark reaction is carried out at room temperature for 2 days, and then 10mL of ferrous ion composite solution is added, in which the mass proportions of ferric pyrophosphate, sodium thiosulfate and urea are 0.5%, 0.2% and 1.0%, respectively. The reaction container is placed in an ultrasonic device, the ultrasonic temperature is 30°C, the frequency is 20kHz, and the reaction is fully carried out for 5h, then the solid-liquid separation is carried out, and the straw iron-containing precursor is obtained at 60°C for 10h. The prepared straw iron precursor material was added to 50 mL of organic acid solution, the masses of terephthalic acid and fumaric acid in the solution were 0.2 g and 0.6 g respectively, and ultrasonicated for 15 min at room temperature, and fully reacted at 100 ° C for 1 h. After cooling to room temperature, solid-liquid separation was performed, and the solid material was washed with anhydrous ethanol, N, N-dimethylformamide, and pure water for 2-3 times in sequence, and dried at 70 ° C for 10 h to obtain a straw iron composite photosensitive salt-absorbing material. Repeat the experiment in the above manner, changing the final reaction time to 3 h and 5 h. The prepared composite materials were added to 50 mL of saline solution (salt content of 10 g / L), reacted under natural light for 5 h, and then solid-liquid separation was performed. The salt content in the supernatant solution was determined. The results are attached. Figure 2 The maximum salt absorption of the straw-iron composite photosensitive salt-absorbing material prepared under the reaction conditions of 3h is 0.29g / g. Similarly, the composite photosensitive material basically does not absorb salt under light-proof conditions.

Claims

1. A method for preparing a straw-iron composite photosensitive salt-absorbing material, characterized in that: Here are the steps: (1) After crushing fresh straw waste with a grass cutter, drying and dehydrating the straw at 50-60° C., crushing the straw into 50-200 mesh straw; adding the crushed straw to the prepared persulfate composite solution A, the straw and the persulfate composite solution A are mixed according to a mass g: volume ml ratio of 1:20, the persulfate composite solution A is compounded from persulfate, maleic acid and salicylic acid, dark reaction is carried out at room temperature for 1-2 days, and then adding iron ion composite solution B, the iron ion composite solution B is compounded from ferric pyrophosphate, sodium thiosulfate and urea; placing the reaction container in an ultrasonic device, the ultrasonic temperature is 30° C., the frequency is 20 kHz, the reaction is fully carried out for 3-5 hours, standing and solid-liquid separation, and drying at 60-80° C. for 8-10 hours to obtain a straw iron-containing precursor; (2) Add the straw iron-containing precursor obtained above to the prepared terephthalic acid and fumaric acid solution, and control the solid-liquid ratio at 1: (10-20), wherein the solid-liquid ratio is mass g: volume ml; ultrasonically treat for 10-20 minutes at room temperature, fully react at 110-140°C for 1-10 hours, cool to room temperature, separate the solid and liquid, wash the solid material with anhydrous ethanol, N,N-dimethylformamide, and pure water for 2-3 times in sequence, and dry at 60-80°C for 8-10 hours to obtain a straw iron composite photosensitive salt-absorbing material.

2. The method for preparing the straw-iron composite photosensitive salt-absorbing material according to claim 1, characterized in that: The persulfate in the persulfate composite solution A includes sodium persulfate, potassium persulfate and ammonium persulfate.

3. The method for preparing the straw-iron composite photosensitive salt-absorbing material according to claim 1, characterized in that: The mass percentages of persulfate, maleic acid and salicylic acid in the persulfate composite solution A are 1%-5.0%, 0.1%-0.5% and 0.1%-0.2% respectively.

4. The method for preparing the straw-iron composite photosensitive salt-absorbing material according to claim 1, characterized in that: The mass percentages of ferric pyrophosphate, sodium thiosulfate and urea in the ferrous ion composite solution B are 0.1%-0.5%, 0.05%-0.2% and 0.5%-1.0% respectively.

5. The method for preparing the straw-iron composite photosensitive salt-absorbing material according to claim 1, characterized in that: The masses of terephthalic acid and fumaric acid in the terephthalic acid and fumaric acid solutions are 0.1%-0.2% and 0.1%-0.4% of the mass of the straw respectively.

6. Application of the straw-iron composite photosensitive salt-absorbing material obtained by the method for preparing the straw-iron composite photosensitive salt-absorbing material according to any one of claims 1 to 5, characterized in that: The straw iron composite photosensitive salt-absorbing material is put into the salt solution at a solid-liquid ratio of 1: (50-100), wherein the solid-liquid ratio is mass g: volume ml; the solubility range of the salt solution is 5-20g / L, and the salt ions in the solution include Na + , K + , Ca 2+ Mg 2+ , Cl - 、SO4 2- , react for 5-8 hours under natural light conditions, perform solid-liquid separation, determine the salt content in the supernatant solution, and analyze the salt absorption of the composite material.

7. The use according to claim 6, characterized in that: The straw-iron composite photosensitive salt-absorbing material is added at a rate of 0.8-1.5 kg per square meter and evenly spread on the surface of saline-alkali soil. The surface soil is taken at a set time, the total salt content of the soil is measured, and the desalination effect of the composite material is evaluated.

Citation Information

Patent Citations

  • Preparation method of high-adsorbability corn stalk charcoal and application of high-adsorbability corn stalk charcoal in preparation of drug sustained release preparation

    CN114192107A

  • Preparation method of calcium modified straw biochar and method for synchronously adsorbing phosphate and tetracycline by using calcium modified straw biochar

    CN115055159A

  • Prediction method for salt absorption rate of decomposed straw in soil

    CN117929641A

  • Super-hydrophobic esterification modified corn straw aerogel oil absorption material and preparation method thereof

    CN118122283A