Rapid chain grate-rotary kiln production recovery method

By using cooked balls as heat transfer medium in the grate-rotary kiln system, production is quickly resumed, and the problems of long production time and unqualified quality are solved, achieving more efficient production and more stable pellet quality.

CN119082446APending Publication Date: 2024-12-06LINGYUAN IRON & STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411210631.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The grate-rotary kiln resumes production for a long time after the production is stopped. The raw balls accelerate the ringing in the rotary kiln, and a large number of unqualified finished pellets are generated in the early stage of production, affecting the output and quality.

Method used

Use cooked ball fabric to pass through the grate, rotary kiln and ring cooler in sequence. When the set temperature of the cooling section of the ring cooler is higher than the set temperature, use raw ball fabric. As a heat transfer medium, cooked balls are preheated and roasted through a grate and rotary kiln to quickly increase the temperature of each section of the ring cooler, shorten the production time, and avoid quality problems caused by drying and insufficient roasting of raw balls.

Benefits of technology

The production time is shortened, the production of raw bulbs is improved, and the powder generation and quality of unqualified finished pellets are avoided due to drying of raw bulbs and insufficient preheating are ensured that the pellets enter the blast furnace standard.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082446A_ABST
    Figure CN119082446A_ABST
Patent Text Reader

Abstract

The invention provides a rapid chain grate-rotary kiln production recovery method, and belongs to the technical field of steel smelting, and the method comprises the following steps: in a production recovery stage, distributing cooked balls, and enabling the cooked balls to sequentially pass through a chain grate, a rotary kiln and a circular cooler; and when the set cold section temperature of the circular cooler is higher than the set temperature, green pellets are adopted for material distribution. As a heat transfer medium, the cooked balls have a certain temperature after being heated by high-temperature hot air in the chain grate and the rotary kiln, the temperature of each section of the circular cooler can be quickly increased when the cooked balls enter the circular cooler, and the production recovery time of the rotary kiln is shortened. Meanwhile, the problem that ring formation is accelerated due to the fact that green pellets are cracked in a kiln due to insufficient drying, preheating and roasting is solved. And unqualified finished pellets caused by insufficient temperature can be avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of steel smelting, and more specifically, relates to a chain grate-rotary kiln rapid production recovery method. Background Art

[0002] The chain grate-rotary kiln method has many advantages, such as high production capacity of a single machine, strong adaptability to raw materials, ability to produce solvent pellets, easy control of kiln atmosphere, ability to produce metallized pellets, uniform roasting, applicability to various ore raw materials, high pellet quality, and less heat-resistant alloy required. It has attracted the attention of the steel industry and has developed rapidly. Its process feature is that the hot air (also divided into high temperature section and low temperature section) used to cool the pellets is generally returned to the rotary kiln and chain grate for use.

[0003] However, in the early stage of production, the heat brought by the materials in each section of the ring cooler was not available, which made it difficult to restore the material distribution. The machine could only produce at a slow speed and with a thin layer of materials. The recovery speed was slow, which affected the production and quality. It took a long time for the grate machine-rotary kiln to resume normal production after shutdown and maintenance. It usually took 6-7 hours from the grate machine distribution to the ring cooler discharge. After the temperature gradually increased, the amount of raw balls needed to be slowly increased. It took more than 12 hours from material distribution production to the restoration of normal production. In addition, the temperature gradient was unreasonable in the early stage of production, and the raw balls were not dried, preheated, and roasted sufficiently. The compressive strength of the preheated balls was low, and the quality of the pellets did not meet the standards for entering the rotary kiln. The preheated balls were easily broken when rolling in the rotary kiln, producing powder, which accelerated the formation of the rotary kiln ring. During the material distribution production, the temperature of each section was lower than normal, and the drying, preheating, and roasting were not complete. The pellets produced from the rotary kiln in the early stage of production did not meet the standards for entering the blast furnace, resulting in a large number of unqualified finished pellets, causing waste. Summary of the invention

[0004] The purpose of the present invention is to provide a method for quickly resuming production of a chain grate-rotary kiln, so as to solve the problems in the prior art of long recovery time of the chain grate-rotary kiln production recovery stage, accelerated ring formation of green balls in the rotary kiln, and production of some finished pellets of unqualified quality.

[0005] In order to achieve the above object, the present invention provides a chain grate-rotary kiln rapid production recovery method, comprising:

[0006] In the production resumption stage, the cooked balls are distributed so that they pass through the chain grate, rotary kiln and ring cooler in sequence;

[0007] When the set cold section temperature of the ring cooler is higher than the set temperature, green ball distribution is adopted.

[0008] Further, the use of cooked ball cloth in the recovery production stage includes:

[0009] Load the cooked balls into the ball making system;

[0010] The mature balls from the ball making system are transported to the tail of the chain grate for distribution;

[0011] Preheat the cooked balls in the chain grate;

[0012] The cooked balls in the chain grate are transported to the rotary kiln, and the cooked balls are roasted in the rotary kiln;

[0013] The ripe balls in the rotary kiln are transported to the ring cooler, and the ring cooler is heated by the ripe balls.

[0014] Furthermore, before loading the cooked balls into the ball making system, the process also includes:

[0015] For rotary kiln drying furnace.

[0016] Further, loading the cooked balls into the ball making system comprises:

[0017] The cooked balls are loaded into 4-5 pelletizing bins through the feeding belt. Each bin is loaded with 70-80t of material and each pelletizing plate has a discharge capacity of 35t / h.

[0018] Furthermore, the mature balls of the ball making system are conveyed to the tail of the chain grate machine for distribution, including:

[0019] Adjust the material layer thickness to 140mm-160mm.

[0020] Further, preheating the cooked balls in the chain grate includes:

[0021] Adjust the speed of the chain grate so that the cooked balls stay in the chain grate for 20-25 minutes.

[0022] Furthermore, preheating the cooked balls in the chain grate also includes:

[0023] The inlet temperature of the main electrostatic precipitator is adjusted to 150-170℃;

[0024] The inlet temperature of the multi-tube dust collector is adjusted to 380-410℃.

[0025] Further, roasting the cooked balls by a rotary kiln includes:

[0026] Coke oven gas and blast furnace gas are adjusted to maximum usage;

[0027] The cooked balls are roasted in a rotary kiln for 30-40 minutes.

[0028] Further, heating the ring cooler by using the cooked balls includes:

[0029] Adjust the speed of the ring cooler so that the thickness of the material layer in the ring cooler is 800mm;

[0030] The temperature of the ring cooling hood is adjusted to 650-850℃;

[0031] The temperature of the second-stage ring cooling hood is adjusted to 400-600℃;

[0032] The temperature of the three-stage ring-cooled smoke hood is adjusted to 150-300℃.

[0033] Furthermore, when the set cold section temperature of the ring cooler is higher than the set temperature, green ball distribution is adopted, including:

[0034] When the temperature of the third ring cooling stage of the ring cooler is higher than 150℃, 5-6 ball making systems are turned on with a discharge rate of 30t / h, and the raw balls are transported to the tail of the chain grate for distribution.

[0035] The beneficial effects of the present invention are: providing a chain grate-rotary kiln rapid production resumption method, which adopts cooked ball distribution in the production resumption stage, so that the cooked balls pass through the chain grate, rotary kiln and ring cooler in sequence; when the set cold section temperature of the ring cooler is higher than the set temperature, the raw ball distribution is adopted. The cooked balls are used as heat transfer medium, and have a certain temperature after being heated by high-temperature hot air in the chain grate and rotary kiln. When entering the ring cooler, the temperature of each section of the ring cooler can be rapidly increased, shortening the production resumption time. At the same time, the problem of insufficient drying, preheating and roasting of raw balls, which will cause a large amount of powder to burst in the kiln and accelerate ring formation, is avoided. It can also avoid the production of finished pellets with substandard quality due to insufficient temperature.

[0036] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] The above and other objects, features and advantages of the present invention will become more apparent through a more detailed description of exemplary embodiments of the present invention in conjunction with the accompanying drawings, wherein like reference numerals generally represent like components throughout the exemplary embodiments of the present invention.

[0038] Figure 1 A flow chart of a method for quickly resuming production of a chain grate-rotary kiln according to an embodiment of the present invention is shown.

[0039] Figure 2 A process diagram of a chain grate-rotary kiln rapid production recovery method according to an embodiment of the present invention is shown.

[0040] Figure 3 A process diagram of a chain grate-rotary kiln-ring cooler air system according to an embodiment of the present invention is shown.

[0041] Reference numerals:

[0042] 1. Chain grate; 11. Blast drying section; 12. Exhaust drying section; 13. Preheating section 1; 14. Preheating section 2; 15. Reheating fan; 16. Blast drying fan;

[0043] 2. Rotary kiln;

[0044] 3. Annular cooler; 31. Annular cooler stage 1; 32. Annular cooler stage 2; 33. Annular cooler stage 3; 34. Annular cooler stage 4; 35. Annular cooler blower;

[0045] 4. Ball making system; 41. Ball making bin; 42. Ball making plate. DETAILED DESCRIPTION

[0046] The preferred embodiments of the present invention will be described in more detail below. Although the preferred embodiments of the present invention are described below, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided to make the present invention more thorough and complete, and to fully convey the scope of the present invention to those skilled in the art.

[0047] like Figure 3 As shown, in normal production, the process flow of the chain grate-rotary kiln-annular cooler 3 air system is as follows: the hot air of the blast drying section 11 comes from the hot exhaust gas of the annular cooler 3 annular cooling section 33 greater than 150°C. The drying process removes part of the moisture inside the green balls, so that the green balls have a certain strength to withstand the pressure of the exhaust drying section 12. The temperature of the smoke hood of the exhaust drying section 12 comes from the hot air of the preheating second section 14 bellows extracted by the reheating fan 15, which further removes moisture, so that the dried pellets can safely withstand the temperature stress of the preheating stage. In the first preheating stage 13, hot air flow above 650℃ passes through the material layer to continue drying the raw balls and start oxidation, so as to ensure that the balls can withstand high temperatures above 1000℃ in the second preheating stage 14. The main heat source of the first preheating stage 13 is the hot exhaust gas from the second ring cooling stage 32 of the ring cooler 3, and a part of the hot air flow of about 1000℃ from the second preheating stage 14 is supplemented. The hot exhaust gas from the second ring cooling stage 32 of the ring cooler 3 directly enters the smoke hood of the first preheating stage 13 through the pipeline. In the second preheating stage 14, the balls are oxidized, decomposed and heated, and part of the consolidation and hardening is completed, so that the balls have a certain strength, can withstand the impact when falling from the chain grate 1 to the rotary kiln 2, and will not be broken during the movement of the rotary kiln 2. Its heat source comes from the hot air flow at the end of the kiln.

[0048] Table 1 Temperature of each section of chain grate 1 during normal production

[0049] project Blast drying section 11 Air drying section 12 Warm up for a period of 13 Preheating stage 2 14 Hood 40~100℃ 300~450℃ 650~850℃ 980~1030℃ Bellows 100~250℃ 100~200℃ 300~450℃ 400~550℃

[0050] Table 2 Temperature of each section of rotary kiln 2 during normal production

[0051]

[0052] Table 3 The temperatures of each section of the ring cooler 3 during normal production are as follows

[0053] Ring cooling section 31 Ring cooling second stage 32 Ring cooling three stages 33 Ring cooling four stages 34 950~1150℃ 700~850℃ >150℃ <150℃

[0054] Table 4 Temperature of each section of chain grate 1 when starting to distribute material

[0055] project Blast drying section 11 Air drying section 12 Warm up for a period of 13 Preheating stage 2 14 Hood 20~40℃ 100~200℃ 300-400℃ 600-700℃ Bellows Room temperature 50~100℃ 100~200℃ 200~300℃

[0056] Table 5 Temperature of each section of rotary kiln 2 when starting to distribute

[0057]

[0058] Table 6 Temperature of each section of the ring cooler 3 when starting to distribute the material

[0059] Ring cooling section 31 Ring cooling second stage 32 Ring cooling three stages 33 Ring cold four 34 Room temperature Room temperature Room temperature Room temperature

[0060] As can be seen from Table 1-6, when the material is distributed in the recovery production stage, the temperature of the entire system is low, most of the heat is lost in the drying and preheating of the raw balls, and there is no material in the annular cooler 3 to provide heat. A thin material layer is required for the distribution of raw balls, and the speed of the chain grate 1 should not be too fast. According to production practice experience, the speed of the chain grate 1 is generally 0.5m-1m / min, and the material layer thickness is 20mm-30mm (the speed of the chain grate 1 in normal production is 2.8m-3.1m / min, and the material layer thickness is 140-160mm). After the roasted material enters the annular cooler 3 and reaches the annular cooling stage 33, the material causes the temperature of the annular cooling stage 33 to begin to rise to a certain temperature before the material amount can be gradually increased. This recovery method takes a long time and produces a certain amount of unqualified pellets.

[0061] This embodiment provides a method for quickly resuming production of a chain grate machine-rotary kiln, such as Figure 1-2 As shown, including:

[0062] In the production recovery stage, the cooked balls are distributed so that they pass through the chain grate 1, rotary kiln 2 and ring cooler 3 in sequence;

[0063] When the set cold section temperature of the ring cooler 3 is higher than the set temperature, green ball distribution is adopted.

[0064] Specifically, the present invention changes the raw ball distribution in the production recovery process into cooked ball distribution. The cooked ball is a pellet that has been calcined and consolidated at high temperature, with a drum strength of more than 95%, a compressive strength of more than 2200N, and stable physical and chemical components. The cooked ball, as a heat transfer medium, is heated by high-temperature hot air in the chain grate 1 and the rotary kiln 2 to a certain temperature. When entering the ring cooler 3, the temperature of each section of the ring cooler 3 can be rapidly increased. When the temperature of each section of the ring cooler 3 reaches the normal production requirement, the raw ball distribution is restored and normal production is started, shortening the production recovery time of the rotary kiln 2 and increasing the output of the rotary kiln 2. At the same time, the problem of insufficient drying, preheating, and calcining of the raw ball, which causes a large amount of powder to burst in the kiln and accelerates ring formation, can be avoided. The production of finished pellets with substandard quality due to insufficient temperature can also be avoided, thereby saving raw fuel resources. In addition, after the cooked ball enters the ring cooler 3, the heat is circulated to the chain grate 1 and the rotary kiln 2 through the ring cooling blower 35, avoiding heat waste and preventing the production of heated balls.

[0065] Optionally, the recovery phase uses cooked ball cloth including:

[0066] Loading the cooked balls into the ball making system 4;

[0067] The cooked balls from the ball making system 4 are transported to the tail of the chain grate 1 for distribution;

[0068] Preheating the cooked balls in the chain grate 1;

[0069] The cooked balls in the chain grate 1 are transported to the rotary kiln 2, and the cooked balls are roasted in the rotary kiln 2;

[0070] The cooked balls in the rotary kiln 2 are transported to the ring cooler 3, and the ring cooler 3 is heated by the cooked balls.

[0071] Optionally, before loading the cooked balls into the ball making system 4, the process further comprises:

[0072] Two systems of rotary kiln.

[0073] Preferably, loading the cooked balls into the ball making system 4 comprises:

[0074] The cooked balls are loaded into 4-5 ball-making bins 41 through a feeding belt, each ball-making bin 41 is loaded with 70-80t of material, and each ball-making disk 42 has a discharge capacity of 35t / h.

[0075] Specifically, all the pelletizing bins 41 can be opened to shorten the time for resuming production. When distributing materials, each pelletizing bin 41 is loaded with 70-80t of materials, and each pelletizing plate 42 discharges 35t / h of materials, which can be maintained for 2-2.5h. The time for the cooked balls to pass through the chain grate 1, rotary kiln 2, and ring cooler 3 to the finished product belt is about 2h. The cooked balls are cooled by the ring cooler 3, and the temperature of each section of the ring cooler 3 is increased. After the cooked balls are consumed, the normal production conditions are just met.

[0076] Preferably, conveying the cooked balls of the ball making system 4 to the tail of the chain grate 1 for distribution includes:

[0077] Adjust the material layer thickness to 140mm-160mm.

[0078] Specifically, when laying out cooked balls, there is no need to consider the problem of raw balls bursting due to insufficient drying and preheating caused by too thick a material layer in the initial stage of production. The physical and chemical properties of cooked balls are stable, and there is no risk of bursting or differentiation. The thickness of the material layer can be controlled according to normal production.

[0079] Preferably, preheating the cooked balls in the chain grate 1 comprises:

[0080] Adjust the speed of chain grate 1 so that the cooked balls stay in chain grate 1 for 20-25 minutes.

[0081] Specifically, the residence time of the cooked balls in the chain grate 1 is substantially the same as the residence time in normal production, and the cooked balls serve as a heat transfer medium to absorb part of the heat.

[0082] Preferably, preheating the cooked balls in the chain grate 1 also includes:

[0083] The inlet temperature of the main electrostatic precipitator is adjusted to 150-170℃;

[0084] The inlet temperature of the multi-tube dust collector is adjusted to 380-410℃.

[0085] Specifically, the cooked balls do not need to be dried or preheated to remove moisture, and the inlet temperature of the main electrostatic precipitator and the inlet temperature of the multi-tube dust collector can be reduced as much as possible, which can reduce heat waste and protect the equipment at the same time.

[0086] Preferably, roasting the cooked balls by the rotary kiln 2 comprises:

[0087] The cooked balls are roasted in a rotary kiln 2 for 30-40 minutes;

[0088] Coke oven gas and blast furnace gas are adjusted to maximum usage.

[0089] Specifically, the cooked balls absorb heat as a heat transfer medium in the rotary kiln 2, and the coke oven gas and blast furnace gas are adjusted to the maximum amount to heat the cooked balls as quickly as possible. The residence time of the cooked balls in the rotary kiln 2 is roughly the same as the residence time in normal production. As a heat transfer medium, the cooked balls are further heated by the blast furnace gas and coke oven gas in the rotary kiln 2 to ensure that the cooked balls carry sufficient heat.

[0090] Preferably, heating the ring cooler 3 by using the cooked balls comprises:

[0091] Adjust the speed of the ring cooler 3 to make the material layer thickness of the ring cooler 3 800mm; ensure that the material layer thickness of the ring cooler 3 can more effectively utilize the heat of the cooling air, improve thermal efficiency, and control the temperature of each section of the smoke hood of the ring cooler 3 within a reasonable range.

[0092] The temperature of the smoke hood of the first ring cooling section 31 is adjusted to 650-850° C. The smoke hood of the first ring cooling section 31 is used as a secondary heat source supplement in the rotary kiln 2 . Appropriate temperature control can increase the roasting temperature in the rotary kiln 2 .

[0093] The temperature of the hood of the second stage of ring cooling 32 is adjusted to 400-600℃; the hot air of the hood of the second stage of ring cooling 32 is transported to the hood of the first stage of preheating 13 through a pipeline, and serves as the heat source of the first stage of preheating 13 of the chain grate machine 1. 400-600℃ can ensure the drying and preheating effect when 5-6 ball-making disks 42 are arranged to make raw balls.

[0094] The temperature of the three-stage 33 smoke hood of the ring cooling is adjusted to 150-300℃. It is a preparation for the raw ball distribution. At the same time, controlling the reasonable temperature range can also avoid the red balls from the finished product belt.

[0095] Preferably, when the set cold section temperature of the ring cooler 3 is higher than the set temperature, green ball distribution is adopted, including:

[0096] When the temperature of the third ring cooling section 33 of the ring cooler 3 is higher than 150°C, 5-6 ball making systems 4 are turned on with a discharge rate of 30t / h, and the raw balls are transported to the tail of the chain grate 1 for distribution.

[0097] Specifically, the hot air from the third ring cooling section 33 enters the bellows of the blast drying section 11 of the chain grate machine 1 through the blast drying fan 16. When the temperature of the third ring cooling section 33 is greater than 150°C, the conditions for laying raw balls are met. When laying raw balls, the material on the grate bed of the chain grate machine 1 is preliminarily dried to remove water attached to the raw balls, while preventing the lower raw balls from being too wet.

[0098] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.

Claims

1. A chain grate-rotary kiln rapid production recovery method, characterized in that: include: In the production recovery stage, the cooked balls are distributed so that the cooked balls pass through the chain grate (1), the rotary kiln (2) and the ring cooler (3) in sequence; When the set cold section temperature of the ring cooler (3) is higher than the set temperature, green ball distribution is adopted.

2. A chain grate-rotary kiln rapid production recovery method according to claim 1, characterized in that: The cooked ball fabrics used in the production resumption phase include: Loading the cooked balls into a ball making system (4); The cooked balls from the ball making system (4) are transported to the tail of the chain grate machine (1) for distribution; Preheating the cooked balls in a chain grate (1); The ripe balls in the chain grate (1) are transported to the rotary kiln (2), and the ripe balls are roasted in the rotary kiln (2); The ripe balls in the rotary kiln (2) are transported to the ring cooler (3), and the ring cooler (3) is heated by the ripe balls.

3. A chain grate-rotary kiln rapid production recovery method according to claim 2, characterized in that: Before the cooked balls are loaded into the ball making system (4), the following steps are also included: The rotary kiln (2) is used for drying.

4. A chain grate-rotary kiln rapid production recovery method according to claim 2, characterized in that: Loading the cooked balls into the ball making system (4) comprises: The cooked balls are loaded into 4-5 ball-making bins (41) through a feeding belt, each ball-making bin (41) is loaded with 70-80t of material, and each ball-making disk (42) has a discharge rate of 35t / h.

5. The method for rapid recovery of production of a chain grate-rotary kiln according to claim 2, characterized in that: The process of conveying the mature balls of the ball making system (4) to the tail of the chain grate (1) for distribution comprises: Adjust the material layer thickness to 140mm-160mm.

6. A chain grate-rotary kiln rapid production recovery method according to claim 2, characterized in that: Preheating the cooked balls in the chain grate (1) includes: The speed of the chain grate (1) is adjusted so that the cooked balls stay in the chain grate (1) for 20-25 minutes.

7. A chain grate-rotary kiln rapid production recovery method according to claim 6, characterized in that: Preheating the cooked balls in the chain grate (1) also includes: The inlet temperature of the main electrostatic precipitator is adjusted to 150-170℃; The inlet temperature of the multi-tube dust collector is adjusted to 380-410℃.

8. The method for rapid production recovery of a chain grate-rotary kiln according to claim 2, characterized in that: The method of roasting the cooked balls by the rotary kiln (2) comprises: Coke oven gas and blast furnace gas are adjusted to maximum usage; The cooked balls are roasted in a rotary kiln (2) for 30-40 minutes.

9. A chain grate-rotary kiln rapid production recovery method according to claim 2, characterized in that: The method of heating the ring cooler (3) by using the cooked balls comprises: Adjust the speed of the ring cooler (3) so that the material layer thickness of the ring cooler (3) is 800 mm; The temperature of the smoke hood of the ring cooling section (31) is adjusted to 650-850°C; The temperature of the smoke hood of the second ring cooling stage (32) is adjusted to 400-600°C; The temperature of the smoke hood of the third stage (33) of the ring cooling is adjusted to 150-300°C.

10. A chain grate-rotary kiln rapid production recovery method according to claim 1, characterized in that: When the set cold section temperature of the ring cooler (3) is higher than the set temperature, the green ball distribution is adopted, including: When the temperature of the third ring cooling section (33) of the ring cooler (3) is higher than 150°C, 5-6 pelletizing systems (4) are turned on with a discharge rate of 30 t / h to transport the raw pellets to the tail of the chain grate (1) for distribution.