Comprehensive utilization method of fly ash

The method addresses the challenges of fly ash utilization by using hydrochloric acid to separate and recover valuable components for aluminum silicon alloys, achieving efficient and pollution-free production.

CN119082456APending Publication Date: 2024-12-06吴一峰
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310705590.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-06-05
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing methods for the comprehensive utilization of fly ash face challenges in separation and purification, leading to high energy consumption, high costs, and environmental pollution, limiting the effective extraction of valuable components such as aluminum and silicon.

Method used

A method utilizing concentrated hydrochloric acid to dissolve fly ash components under controlled conditions, followed by crystallization and pH adjustment to separate chloride salts, allowing for the recovery of aluminum oxide and silicon oxide, which are then used to produce aluminum silicon alloys.

Benefits of technology

This method achieves efficient and comprehensive utilization of fly ash resources, reducing energy consumption and environmental impact while producing high-quality aluminum silicon alloys without waste emissions.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a comprehensive utilization method of fly ash, and belongs to the technical field of comprehensive utilization of resources. According to the method, concentrated hydrochloric acid is used for decomposing fly ash. When the concentration of a certain chloride in the solution reaches saturation concentration, cooling to separate out crystals, and carrying out solid-liquid separation; all chloride crystals are dissolved again, and one of carbonate or hydroxide of alkali metal (sodium and potassium) or alkaline earth metal (calcium and magnesium) is used for neutralization reaction to adjust the PH value of the solution until the hydroxide is precipitated and separated out; and washing and drying the slag which mainly contains aluminum oxide, silicon oxide and the like after the hydrochloric acid is dissolved out, and then producing the aluminum-silicon alloy. According to the content of aluminum and silicon (9-80%) in the aluminum-silicon alloy, the content of aluminum oxide and the content of silicon oxide in the raw materials are adjusted through aluminum oxide and silica so that the aluminum oxide and the silicon oxide can meet the component index requirement of the alloy, the aluminum oxide and the silicon oxide are prepared into alloy production raw materials with carbon (a reducing agent), and the silicon-aluminum alloy is prepared through smelting at the temperature of 1800-2400 DEG C.
Need to check novelty before this filing date? Find Prior Art

Description

1. Technical field:

[0001] The invention relates to a comprehensive utilization method of fly ash, belonging to the technical field of comprehensive utilization of resources. 2. Background Technology

[0002] Fly ash is the solid residue left after coal combustion. It is the waste of coal-fired thermal power plants and is classified as industrial solid waste. For every ton of coal burned, 230 kg of fly ash will be produced. The traditional way to deal with fly ash is landfill, but it cannot fundamentally solve the pollution caused by fly ash to the environment. In recent years, fly ash has been used in construction and building materials. From the chemical composition point of view, fly ash is a low-grade aluminum resource. However, due to the low grade of aluminum, aluminum cannot be extracted by the soda lime method (sintering method, Bayer process). Acid method for aluminum extraction is the focus of research, but there are technical difficulties in separation and purification, which are directly related to the value and economic benefits of comprehensive resource utilization, and often have one or another deficiency. For example, the technical methods described in some patent documents: CN201811365307 A method for preparing aluminum chloride using fly ash, 1. A method for preparing crystalline aluminum chloride using fly ash, characterized in that it comprises the following steps: the first step, mixing the fly ash ground to 100-200 mesh with water in proportion to obtain a mixture, adding concentrated sulfuric acid to the mixture in batches in proportion, performing acid leaching reaction, and obtaining a mixed solution; the second step, adding water with a temperature greater than 80°C to the mixed solution in proportion, stirring evenly, and performing solid-liquid separation while hot to obtain aluminum sulfate leachate and leach residue; the third step, adding aluminum hydroxide to the aluminum sulfate leachate to adjust the pH to 1- 4. A concentrated solution is obtained by evaporating and concentrating by utilizing the heat of reaction, and the concentrated solution is cooled to less than 40° C. to obtain aluminum sulfate crystals without residual liquid; the fourth step is to dissolve the aluminum sulfate crystals in water at 70 to 90° C., keep warm and stir, and then perform temperature-controlled crystallization, and solid-liquid separation to obtain refined aluminum sulfate and a mother liquor recycled for dissolving aluminum sulfate crystals; the fifth step is to add ammonia water to the refined aluminum sulfate in proportion, and after the reaction is completed, solid-liquid separation to obtain aluminum hydroxide crystals and ammonium sulfate solution; the sixth step is to add hydrochloric acid to the aluminum hydroxide crystals in proportion, and after the reaction is completed, the temperature is lowered to room temperature to obtain crystals without residual liquid, and after being rinsed with water, low-temperature drying is performed at 30 to 50° C. to obtain crystalline aluminum chloride.

[0003] CN201810711260 A method for producing acid from fly ash and phosphogypsum and co-producing a coagulant for a waterproof plugging agent: The invention discloses a method for producing acid from fly ash and phosphogypsum and co-producing a coagulant for a waterproof plugging agent, comprising the steps of mixing fly ash, phosphogypsum, additives and modifiers and grinding them to form a raw meal, wherein the raw meal is fed into a kiln and roasted to obtain a clinker; the clinker is ground and dissolved with water, and then solid-liquid separation is performed, a flotation agent is added to the residue obtained by separation to float out sulfides, the flue gas generated after the sulfides are roasted is catalyzed by vanadium pentoxide, and then absorbed by concentrated sulfuric acid to produce acid; the separated solution is heated and evaporated to obtain sodium aluminate crystals, the sodium aluminate crystals are dried and ground into sodium aluminate powder, the sodium aluminate powder, water glass, aluminum sulfate and calcium oxide are mixed and stirred evenly to obtain a coagulant for a waterproof plugging agent. The invention has the characteristics of low production cost and good performance of the coagulant used for waterproof plugging agent, low processing cost of phosphogypsum and fly ash, and high added value.

[0004] CN201710088832 Method for producing high-purity aluminum oxide by sulfuric acid activation-hydrogen chloride crystallization: The present invention relates to a method for producing high-purity aluminum oxide by sulfuric acid activation-hydrogen chloride crystallization. The specific process is drying of fly ash raw materials, hot activation by concentrated sulfuric acid acid leaching, water dissolution, special filtration under acidic conditions, introduction of HCl gas to remove impurities and precipitate aluminum chloride crystals; filtering and washing crystals, calcining crystals into products, and recycling of filtrate. The present invention uses slurry to activate in a reactor, with high industrial efficiency; special filtration and deep desiliconization cost are low, impurity removal and crystallization are completed simultaneously by passing hydrogen chloride, filtrate is recycled and recycled, the overall process is short, and energy consumption is low; materials are fully recycled, and there is no waste gas or waste liquid emission; impurity removal and crystallization are completed in one step, which solves the problems of difficulty in activating fly ash in pulverized coal furnaces, removal of metal impurity ions under acidic conditions, and difficulty in thorough desiliconization. The overall process has been tested for each batch of 100 kg of fly ash, and the purity of the produced aluminum oxide is above 99.95%, there are no foreseeable industrialization technical problems, and the economic and social benefits are significant.

[0005] CN201610892000A method for extracting aluminum oxide from fly ash based on sulfuric acid slaking: The invention provides a method for extracting aluminum oxide from fly ash based on sulfuric acid slaking, and belongs to the technical field of comprehensive utilization of fly ash. Concentrated sulfuric acid and fly ash are mixed evenly and then slaking to obtain sulfated clinker, aluminum precipitation mother liquor or water is used to leach the clinker to obtain aluminum sulfate solution and high silicon slag, potassium, sodium or ammonium sulfate is added to the aluminum sulfate solution and mixed and stirred, aluminum is precipitated in the form of double salt, alum and aluminum precipitation mother liquor are filtered to obtain alum, alum is dried and dehydrated to obtain dehydrated alum, dehydrated alum is reduced and roasted to obtain reduced roasted sand, the roasted sand is washed with water, and then metallurgical grade alumina is produced through alkali leaching, seeding and calcining processes. The method strengthens the decomposition of aluminum silicate minerals in fly ash through sulfuric acid slaking, uses double salt to precipitate aluminum instead of concentrated crystallization precipitation aluminum, and uses reduction roasting to reduce the decomposition temperature of aluminum sulfate, and has the advantages of low energy consumption, high aluminum recovery rate, easy solution of equipment material, and high quality of alumina products.

[0006] CN201610065399A method for preparing water glass using fly ash from a common circulating fluidized bed: The present invention provides a method for preparing water glass using fly ash from a common circulating fluidized bed, the method comprising reacting sulfuric acid with fly ash under low temperature roasting conditions, dissolving Al2O3, Fe2O3, and FeO in the fly ash, and then using a caustic solution to hydrothermally extract SiO2 in the acid leaching residue at high temperature to prepare water glass. The method provided by the present invention is a method for preparing water glass without special requirements for equipment, low temperature roasting, and capable of efficiently utilizing SiO2 in fly ash. The method provided by the present invention can dissolve 90% to 96% of aluminum oxide in fly ash, 98% to 100% of iron oxide; 70% to 78% of silicon dioxide in the acid leaching residue is converted into liquid-4 type water glass with a modulus greater than 2.2. The technical solution provided by the present invention makes full use of fly ash resources, has a simple manufacturing process, low production cost, and is suitable for large-scale production.

[0007] CN201410823508 A method for extracting aluminum oxide from fly ash: The present invention relates to a method for extracting aluminum oxide from fly ash. The method comprises: (1) mixing fly ash and ammonium sulfate to form granules; (2) roasting the granules in a two-stage fluidized roasting system; (3) adding dilute sulfuric acid to the clinker to dissolve the material, filtering, and the filtrate is a NH4Al(SO4)2 crude liquid; (4) removing impurities from the above solution by a combined method, filtering, and obtaining NH4Al(SO4)2 semen; (5) the NH4Al(SO4)2 semen separated by the above impurities absorbs ammonia released during the roasting reaction, and the ammonia reacts with the NH4Al(SO4)2 semen to generate Al(OH)3; (6) calcining the above precipitate Al(OH)3 at 1100°C to obtain Al2O3. The invention adopts a two-stage fluidized roasting system of fly ash and ammonium sulfate roasting, combined impurities and oxygen-enriched combustion, which solves the problems of high corrosion, roasting wall sticking, agglomeration and coking of equipment in the background technology.

[0008] CN201710153494 Method for preparing pseudo-boehmite using high-aluminum fly ash as raw material: The present invention provides a method for preparing pseudo-boehmite using high-aluminum fly ash as raw material, comprising the following steps: 1) acid dissolving high-aluminum fly ash, followed by filtering to obtain acid slag and aluminum sulfate solution; 2) adding sodium carbonate and limestone to the acid slag to obtain raw material slurry; 3) calcining the raw material slurry to obtain clinker; 4) dissolving the clinker using a dissolution adjustment liquid, followed by filtering to obtain calcium-silicon slag and sodium aluminate solution; 5) mixing the aluminum sulfate solution with the sodium aluminate solution and reacting until the pH value of the reaction solution reaches 8-10, then gelling, aging and filtering the reaction solution, washing and drying the filter cake obtained by filtration to obtain pseudo-boehmite. The method of the present invention has low material flow, most of the materials can be recycled, no toxic and harmful substances are discharged, has good economic and social benefits, and is suitable for industrial promotion and application.

[0009] CN201310755180 A method for preparing aluminum sulfate by leaching fly ash with sulfuric acid: The present invention relates to a method for preparing aluminum sulfate by leaching fly ash with sulfuric acid, comprising the following steps: (1) grinding the fly ash to 300-500 meshes and roasting at 105-110°C for 60-90 min; (2) soaking the fly ash obtained in step (1) in concentrated sulfuric acid for 60-90 min under stirring conditions of 20-40 r / min, with the soaking temperature being 220-330°C; (3) filtering to separate the solid from the liquid, then boiling the solid with water at a temperature of 85-90°C, washing the dissolved slag 2-3 times, and then returning the washing waste liquid to the boiling container; (4) evaporating and concentrating the liquid obtained in step (3) at a concentration temperature of 110-120°C, and then drying the solid at 80°C for 2h to obtain the product crystalline aluminum sulfate. The present invention utilizes fly ash, a waste pollutant of power plants, as a raw material to prepare crystalline aluminum sulfate under normal pressure conditions. Aluminum sulfate can be used as an industrial product and can also be used as a chemical raw material to prepare high-value-added products such as high-purity alumina. In addition, the method has the characteristics of wide raw material sources and low cost.

[0010] CN201310026762 Method for producing metallurgical grade sandy alumina by mixed roasting of fly ash and ammonium sulfate: The present invention relates to a method for producing alumina by utilizing industrial solid waste, and in particular to a method for producing metallurgical grade sandy alumina by mixed roasting of fly ash and ammonium sulfate. The method comprises the following steps: raw material preparation, clinker burning, clinker dissolution, silicon slag separation and washing, ammonium aluminum sulfate solution decomposition, crude aluminum hydroxide separation and washing, crude aluminum hydroxide desulfurization and low-temperature Bayer process treatment. The advantages and effects of the present invention: The present invention does not add any additives, and the fly ash does not need to be roasted at high temperature for activation. Alumina in the fly ash can be effectively extracted, and the extraction rate of alumina can reach more than 85%.

[0011] CN201110438078 Method for extracting aluminum oxide from fly ash based on grinding and acid leaching process: The present invention relates to a method for extracting aluminum oxide from fly ash based on grinding and acid leaching process. The commonly used method for extracting aluminum oxide from fly ash has a long process flow, single furnace roasting, and does not fully consider the removal of impurities. The present invention grinds fly ash ultrafinely; then dissolves it with concentrated sulfuric acid to obtain a slurry containing aluminum sulfate; obtains an aluminum sulfate solution after solid-liquid separation; removes impurity ions in the solution by a combined impurity removal method; then evaporates and concentrates the aluminum sulfate concentrate to precipitate aluminum sulfate crystals; obtains aluminum oxide by two-stage combined fluidized roasting; and recovers sulfur trioxide in the flue gas to form sulfuric acid for recycling. The grinding process of the present invention can grind fly ash ultrafinely, further reduce the fineness of fly ash, and effectively improve the reaction efficiency of subsequent dissolution; its combined impurity removal method removes impurity ions in aluminum sulfate solution, has a simple process, and has a high impurity removal efficiency; the two-stage combined fluidized roasting process consumes less energy, and the sulfur trioxide after roasting is recycled and reused, thereby reducing costs.

[0012] CN201010281025 Process for extracting metallurgical grade alumina by treating high-aluminum fly ash with sulfuric acid method: The present invention discloses a process for extracting metallurgical grade alumina by treating high-aluminum fly ash with sulfuric acid method, comprising the steps of mixing high-aluminum fly ash with dilute sulfuric acid to prepare raw ore pulp A; dissolving the raw ore pulp A to obtain acid slag B and crude aluminum sulfate liquid C; purifying the crude aluminum sulfate liquid C by controlled filtration and removing iron to obtain pure aluminum sulfate solution D; sending the pure aluminum sulfate solution D to an evaporation process for evaporation to remove water in the pure aluminum sulfate solution D and precipitate aluminum sulfate in the pure aluminum sulfate solution D; and sending the aluminum sulfate E to an aluminum sulfate roasting process, where the aluminum sulfate E is decomposed after roasting to obtain aluminum oxide F and SO3 gas G. The present invention adopts sulfuric acid method to treat high-aluminum fly ash, dissolves alumina in the high-aluminum fly ash, and obtains metallurgical-grade alumina that meets national standards through separation, washing, filtering, roasting and other processes, so that the fly ash is reasonably utilized, and the cost is low, the economy is reasonable, and the impact on equipment is small.

[0013] CN201010117032 Method for producing hydrated silicon dioxide and aluminum-iron water treatment agent using fly ash: A method for producing hydrated silicon dioxide and aluminum-iron water treatment agent using fly ash as raw material, wherein the fly ash is crushed to less than 500 microns, mixed and stirred with the co-solvent NaF in proportion, mixed with water and concentrated sulfuric acid, and then subjected to a first-stage leaching to dissolve and separate Al, Fe and glass; the separated glass is subjected to a second-stage leaching, gel preparation, pH adjustment, isolation and heating, aging, filtration and washing, vacuum drying, and fine grinding to produce solid ultrafine silicon dioxide; the Al and Fe crystals separated by the first-stage leaching are neutralized, oxidized, alkalized, precipitated and filtered to obtain an iron-containing filter cake and a polyaluminum sulfate filtrate; the iron-containing filter cake is activated, stabilized and emulsified to obtain solid polyferric sulfate, wherein a part of the polyaluminum sulfate filtrate is evaporated, activated, stabilized and emulsified to obtain solid polyaluminum sulfate, and the other part is used to prepare AlF3 product. The invention has the beneficial effects of high added value, higher comprehensive utilization degree, stronger practicality, and simple and easy process, equipment and operation.

[0014] CN200510048274 A method for extracting aluminum oxide from fly ash: the fly ash is ground and roasted for activation, and then heated with H2SO4 solution for reaction, the leached aluminum oxide is dissolved with hot water, concentrated and cooled to precipitate aluminum sulfate crystals, heated and dehydrated to obtain anhydrous aluminum sulfate, and further heated and decomposed to obtain γ-Al2O3, and further prepared to obtain metallurgical grade aluminum oxide. The present invention adopts a new fly ash activation technology, does not use any co-solvent at normal pressure, and can effectively leach aluminum oxide from fly ash with H2SO4, and the dissolution rate of aluminum oxide can reach more than 85%. The present invention treats fly ash into various types of aluminum salts and aluminum oxides, and realizes the refined comprehensive utilization of fly ash.

[0015] CN201210102794 A method for preparing aluminum oxide from fly ash from a power plant: grinding fly ash, leaching with concentrated sulfuric acid to obtain aluminum sulfate solution, concentrating and cooling to precipitate aluminum sulfate crystals, dissolving aluminum sulfate with hydrochloric acid, then introducing HCl gas to saturate the solution to obtain AlCl3.6H2O crystals, reacting AlCl3.6H2O with ammonium hydroxide solution or liquid ammonia or ammonium bicarbonate solution or ammonium carbonate solution to obtain aluminum hydroxide and ammonium chloride solution, calcining aluminum hydroxide to obtain aluminum oxide, replacing ammonium chloride with magnesium oxide to obtain ammonia gas and magnesium chloride, and hydrolyzing magnesium chloride to obtain magnesium oxide and hydrochloric acid for recycling.

[0016] CN201210124115 A method for leaching aluminum oxide in fly ash by microwave acid dissolution: grind fly ash to less than 200 mesh and put it into a microwave reactor; add water to a certain liquid-solid ratio and mix evenly; add 98% concentrated sulfuric acid according to the theoretical acid consumption value of aluminum oxide and other cationic oxides in fly ash and mix evenly; carry out microwave heating reaction under stirring in a closed system, separate solid and liquid, wash until the filter residue is close to neutral, and obtain aluminum sulfate solution. The present invention uses sulfuric acid as a leaching agent and microwaves as a heating source to leach aluminum oxide in fly ash, changes the traditional heating method, makes full use of the high frequency and penetration of microwave heating, makes the fly ash and sulfuric acid system generate heat evenly, accelerates the reaction of sulfuric acid and fly ash particles, thereby increasing the dissolution rate of aluminum oxide in fly ash, greatly shortens the reaction time, and improves the dissolution rate of aluminum oxide, making the dissolution rate of aluminum oxide greater than 90%. Microwave acid dissolution can reduce energy consumption and save energy.

[0017] CN201110208699A method for extracting aluminum oxide from fly ash: the method comprises the following steps: finely grinding the fly ash and removing iron from it; heating and decomposing ammonium sulfate to prepare ammonium bisulfate and ammonia; mixing the fly ash after iron removal with ammonium sulfate and sintering to generate solid matter and ammonia; dissolving the solid matter generated after sintering to obtain a solution containing ammonium aluminum sulfate; crystallizing the solution containing ammonium aluminum sulfate to obtain solid ammonium aluminum sulfate; dissolving the solid ammonium aluminum sulfate and preparing a solution to react with ammonia or ammonia water to generate aluminum hydroxide and ammonium sulfate; roasting the aluminum hydroxide to obtain aluminum oxide. The method for extracting aluminum oxide from fly ash of the present invention prepares ammonium bisulfate and co-produces ammonia, so that the reaction of ammonium sulfate and fly ash is easy to control, the method is simple, the by-products are few and it is easy to realize industrial application.

[0018] CN201110288031 A method for extracting aluminum oxide from fly ash using potassium sulfate: The commonly used alkaline process for extracting aluminum oxide from fly ash has a long process flow, complex equipment, and poor economic benefits, which restricts large-scale application. The present invention roasts and activates fly ash or mechanically grinds and activates it, then the obtained solid is dissolved by sulfuric acid and filtered to remove solid residues, potassium sulfate solid is added to the solution, potassium aluminum sulfate solution is obtained after a period of reaction, and impurities in the solution are removed by chemical or resin adsorption methods, and the solution is crystallized to obtain solid potassium aluminum sulfate dodecahydrate, and potassium aluminum sulfate dodecahydrate is roasted to obtain aluminum oxide, potassium sulfate solid and sulfur trioxide gas, and the solid phase is washed and filtered to obtain an aluminum oxide product. The present invention obtains potassium aluminum sulfate solid by cooling crystallization method, which reduces energy consumption; impurities can be effectively removed during crystallization, reducing the investment in impurity removal system; potassium sulfate and sulfuric acid can be recycled, and industrial production has high economic benefits.

[0019] Some of the above methods use activation pretreatment processes such as sintering, alkali sintering or acid sintering, which consume a lot of energy and have high costs; basically, there are problems of one kind or another in separation and purification, making it difficult to realize the value of comprehensive utilization of fly ash.

[0020] Strong acids (concentrated hydrochloric acid, concentrated nitric acid, and concentrated sulfuric acid) can decompose fly ash under high temperature and high pressure to generate corresponding soluble salts. When using concentrated hydrochloric acid and concentrated nitric acid, the insoluble matter includes silicon oxide; when using concentrated sulfuric acid, the insoluble matter includes silicon oxide, insoluble sulfates, etc. Considering the production cost and other factors, it is more advantageous to use hydrochloric acid or sulfuric acid.

[0021] Under high temperature and high pressure, concentrated hydrochloric acid can basically dissolve all components in fly ash except silicon oxide to generate soluble chloride. The main chemical reaction formula is as follows:

[0022] Al2O3+6HCl=2AlCl3+3H2O

[0023] Fe2O3+6HCl=2FeCl3+3H2O

[0024] CaO+2HCl=CaCl2+H2O

[0025] MgO+2HCl=MgCl2+H2O

[0026] Li2O+2HCl=2LiCl+H2O

[0027] Na2O+2HCl=2NaCl+H2O

[0028] K2O+2HCl=2KCl+H2O

[0029] Re2O3+6HCl=2ReCl3+3H2O (Re is a rare earth element)

[0030] By controlling the reaction temperature, reaction time and hydrochloric acid concentration, 60-80% of the aluminum oxide and titanium oxide can be kept from dissolving and form slag together with silicon oxide, becoming the raw material for producing aluminum silicon alloy or aluminum silicon titanium alloy.

[0031] The chlorides that enter the solution can utilize the differences in solubility and concentration to precipitate the corresponding chloride salt crystals through the crystallization of the saturated solution. When a certain salt in the dissolving solution reaches the saturated concentration, it can be separated by precipitating the corresponding chloride crystals, creating conditions for further separation and purification of each component element. The mother liquor after separation and crystallization is supplemented with acid and returned to the dissolution process.

[0032] Saturated solubility of main chlorides:

[0033] Ferrous chloride hexahydrate: 920 g / l (20°C);

[0034] Aluminum chloride hexahydrate: 700 g / l (20°C);

[0035] Calcium chloride: 740 g / l (20°C);

[0036] Magnesium chloride: 740 g / l (20°C);

[0037] Sodium chloride: 360 g / l (20°C);

[0038] Potassium chloride: 253 g / l (20°C);

[0039] Lithium chloride: 670 g / l (20°C);

[0040] Rare earth chloride: 500g / l (20℃).

[0041] Compounds with similar concentrations and saturated solubility will form co-crystals and co-precipitations, such as ferric chloride hexahydrate and aluminum chloride hexahydrate, calcium chloride and magnesium chloride, sodium chloride and potassium chloride, lithium chloride and rare earth chloride, etc. Therefore, for mixtures that form co-crystals and co-precipitations, other methods need to be used for further separation and purification.

[0042] For the co-crystallization and co-precipitation formed by ferric chloride hexahydrate and aluminum chloride hexahydrate, the pH value of the solution can be adjusted by a neutralization reaction with a carbonate or hydroxide of an alkali metal (sodium, potassium) or alkaline earth metal (calcium, magnesium), so that ferric hydroxide and aluminum hydroxide are precipitated respectively, and aluminum and iron are separated and purified. If the cheapest and most readily available calcium carbonate is used, the reaction is as follows:

[0043] 3CaCO3+2FeCl3+3H2O=3CaCl2+2Fe(OH)3↓+3CO2↑

[0044] 3CaCO3+2AlCl3+3H2O=3CaCl2+2Al(OH)3↓+3CO2↑

[0045] The pH value for complete precipitation of iron hydroxide is 3.8, while the pH value for the beginning precipitation of aluminum hydroxide is 3.8. Therefore, the pH value of the solution can be adjusted to precipitate iron hydroxide first, and then the pH value of the solution can be further adjusted to precipitate aluminum hydroxide after filtering and separating the precipitate. The pH value of the solution can be adjusted to 5 with calcium carbonate or calcium hydroxide. Under this condition, aluminum hydroxide cannot be completely precipitated. Only part of aluminum hydroxide is precipitated and basic aluminum chloride is generated. Sodium carbonate (or sodium hydroxide) is needed to adjust the pH value of the solution to 11 to completely precipitate aluminum hydroxide. The separated iron hydroxide is washed, dried, and dehydrated at high temperature (500°C) to generate iron oxide, which is used for steel smelting, iron red pigment, etc. The separated aluminum hydroxide is washed, dried, and calcined at high temperature (1200°C) to generate α-Al2O3. Residual impurities such as iron oxide are leached with dilute hydrochloric acid to obtain high-purity aluminum oxide.

[0046] The co-crystallization and co-precipitation formed by lithium chloride and rare earth chloride can be redissolved and the pH value of the solution can be adjusted with sodium carbonate to precipitate rare earth oxide first, which can be filtered and washed to obtain mixed rare earth oxide. Sodium carbonate can be used to adjust the pH value of the filtrate to precipitate lithium carbonate, which can be filtered and washed to obtain lithium carbonate.

[0047] The main components of fly ash: aluminum oxide, silicon oxide, etc., as well as other medium and trace elements can be separated, or single oxides can be obtained, or mixed oxides for preparing alloy materials can be obtained, such as silicon oxide and aluminum oxide; silicon oxide, aluminum oxide and titanium oxide. Aluminum alloy materials are a large category of metal aluminum applications, such as cast aluminum alloy-aluminum silicon alloy materials, cast aluminum and deformed aluminum alloy-aluminum silicon titanium alloy materials, etc. Therefore, relative to the preparation of alloy materials, it is sufficient to separate the usable raw materials without purifying them to single oxides. Such as silicon oxide and aluminum oxide; silicon oxide, aluminum oxide and titanium oxide; a mixture of iron oxide and aluminum oxide.

[0048] Calcium carbonate and other substances added in the process flow form incremental byproducts such as calcium chloride, which are crystallized and dried to obtain anhydrous calcium chloride. Calcium chloride can be used as antifreeze, snow melting agent, desiccant, and is also widely used in the pharmaceutical, chemical, food, fertilizer and other industries.

[0049] If sodium carbonate, magnesium carbonate, etc. are used as neutralizing precipitants, by-products such as magnesium chloride and sodium chloride are produced, which are all useful for coating.

[0050] The mother liquor and washing liquid of each stage can be combined together, and hydrochloric acid can be added to decompose fly ash.

[0051] The acid treatment of fly ash has the following significant advantages: the acid treatment process can be used for fly ash of any material composition and component content; the components of fly ash can be effectively separated and extracted. Single substances such as iron oxide and pigment-grade iron red, high-purity aluminum oxide, silicon oxide, lithium carbonate, rare earth oxide, etc. can be obtained, and high-quality alloy production raw materials such as cast aluminum alloy-aluminum silicon alloy materials, cast aluminum and deformed aluminum alloy-aluminum silicon titanium alloy materials, soft magnetic alloy-iron aluminum alloy materials, etc. can also be obtained; it can achieve a pollution-free green industrial process without waste slag, wastewater, and waste gas emissions.

[0052] 90% of alumina production is used to produce aluminum metal, and most of the aluminum metal is used to produce aluminum alloys.

[0053] Silicon aluminum alloy and high silicon aluminum alloy, which account for about 30% of the alloy market, are binary alloys of Si and Al. High silicon aluminum alloy materials can maintain the excellent properties of silicon and aluminum, and the content of Si and Al is quite rich. The alloy density is 2.4-2.7g / cm3, and the thermal expansion coefficient is between 7-20ppm / ℃. Increasing the silicon content can significantly reduce the density and thermal expansion coefficient of the alloy material. At the same time, high silicon aluminum alloy also has good thermal conductivity, high specific strength and rigidity, good plating performance with gold, silver, copper and nickel, can be welded with the substrate, and is easy for precision machining. It is used for electronic packaging materials, especially in high-tech fields such as aerospace, space technology and portable electronic devices.

[0054] Hypoeutectic silicon aluminum alloy contains 9-12% silicon; eutectic silicon aluminum alloy contains 11-13% silicon; hypereutectic silicon aluminum alloy has a silicon content of more than 12%, mainly 15-20%; those with a silicon content of more than 22% are called high-silicon aluminum alloys, of which 25-70% is the main content, and the highest silicon alloy in the world can reach 80%.

[0055] Some patents involve the production of aluminum-silicon-iron alloy by ore thermal reduction. For example: CN1614043A, using 3500KVA ore thermal furnace to produce aluminum-silicon-iron alloy; CN115029559A, a method for producing deoxidized alloy using red mud; CN202011267925, a method for preparing aluminum-silicon-iron alloy and grading purification using high-aluminum fly ash. Carbon is used as a reducing agent to prepare aluminum-silicon-iron alloy, and then the alloy ingot is heated and controlled to separate the aluminum-silicon alloy through a porous filter plate in an ultra-gravity centrifugal device; CN201910009814 is a method for preparing aluminum-silicon alloy from low-grade resources, using magnetic separation to remove iron, mixing tailings with ammonium bisulfate solution, heating to remove iron, reducing iron to 0.5%, and using electrolysis to produce aluminum-silicon alloy; CN200910013204 uses bauxite flotation tailings to produce primary aluminum-silicon alloy by electrothermal method. Iron is removed with hydrochloric acid. The filter residue is mixed with coal and pulp waste liquid to make balls, dried, and heated in an electric arc furnace at 2300-2500°C to obtain a primary aluminum-silicon alloy; CN91111016 discloses a method for directly smelting silicon-aluminum alloy in an electric arc furnace, which uses bauxite and silica as raw materials, charcoal and petroleum coke as reducing agents, and directly smelts in an electric arc furnace and refines with gas solvent to produce a silicon-aluminum alloy containing 4-15% aluminum, etc.

[0056] There are many reports on the use of ore thermal reduction to smelt aluminum silicon iron and aluminum silicon alloys. However, most of the research work is to prepare aluminum silicon iron alloys, and aluminum silicon alloys are generally prepared using low-iron high-quality raw materials.

[0057] The method of the present invention is to use concentrated hydrochloric acid to remove iron, calcium, magnesium, sodium, potassium, gallium, lithium and part of aluminum from fly ash, and then crystallize and separate a certain chloride salt from the saturated solution of the corresponding chloride salt by a crystallization method, so that each component is initially separated. After the separated chloride is redissolved, the acidity of the dissolving solution is adjusted with calcium carbonate (or calcium hydroxide) and sodium carbonate (or sodium hydroxide), and iron hydroxide, aluminum hydroxide, etc. are precipitated respectively. The mother liquor after solid-liquid separation can be recycled after supplementing with concentrated hydrochloric acid. When a certain salt in the mother liquor reaches a saturated state, the temperature is lowered to precipitate crystals, and solid-liquid separation is performed. Crystalline salts such as calcium chloride, magnesium chloride, sodium chloride, potassium chloride, gallium chloride, and lithium chloride can be obtained respectively. The filter residue after hydrochloric acid dissolution mainly contains aluminum oxide and silicon oxide, etc., and after washing and drying, it is used to produce aluminum silicon alloy. According to the aluminum and silicon (9-80%) content of aluminum-silicon alloy, alumina and silica are used to adjust the aluminum oxide and silicon oxide content of the raw material to meet the alloy's component index requirements, and then mixed with carbon (reducing agent) to form the alloy production raw material, and smelted at a temperature of 1800℃-2400℃ to produce silicon-aluminum alloy. III. Summary of the invention

[0058] The present invention mainly includes the following contents and steps:

[0059] a. Use chemical analysis methods to analyze the content of the main components in fly ash: Al2O3, Fe2O3, TiO2, CaO, MgO, Na2O, K2O, etc.;

[0060] b. According to the weight of Fe2O3, CaO and MgO in fly ash material and the chemical reaction formula:

[0061] Fe2O3+6HCl=2FeCl3+3H2O; CaO+2HCl=CaCl2+H2O; MgO+2HCl=MgCl2+H2O, calculate the amount of hydrochloric acid required for complete reaction, and add 10-50% excess hydrochloric acid;

[0062] c. Solid content: 10-40%, reaction temperature: 100-150°C, pressure: 0.1-0.8MPa, react for 1-5h under stirring, and separate the solid and liquid;

[0063] d. The dissolving liquid can be used to decompose fly ash after adding concentrated hydrochloric acid; when the concentration of certain chlorides of iron, aluminum, calcium, magnesium, sodium, potassium, gallium, lithium, etc. in the solution reaches saturation, the temperature is lowered to precipitate crystals, and the solid-liquid separation is carried out; iron chloride, aluminum chloride, calcium chloride, magnesium chloride, sodium chloride, potassium chloride, gallium chloride, lithium chloride, etc. can be crystallized and precipitated respectively;

[0064] e. Re-dissolve the chloride crystals: adjust the pH value of the chloride solution to pH=3.8 with calcium carbonate powder (or calcium hydroxide), precipitate iron hydroxide, filter, wash, and dry (to 500°C) to make iron oxide; adjust the pH value to pH=11 with sodium carbonate (or sodium hydroxide) to precipitate aluminum hydroxide; other chloride solutions can also be adjusted to pH values ​​with sodium carbonate (or sodium hydroxide) until hydroxide precipitates; f. After the filter residue is dissolved with hydrochloric acid, wash and dry it, and then use aluminum oxide and Silica is used to adjust the aluminum oxide and silicon oxide contents of the raw materials to meet the composition index requirements of the alloy, and is mixed with carbon (reducing agent) to form the raw material for alloy production. The amount of carbon required for the complete reaction is calculated according to the reaction formula of Al2O3+1.5C=2Al+1.5CO2; SiO2+C=Si+CO2, and 0-20% is added on the basis of this amount. A mineral thermal reduction furnace is used with slag-free submerged arc high-temperature smelting technology. At a temperature of 1800-2400°C, the smelting reaction is continued for 30min-3h, and the material is continuously added from the upper part and discharged from the lower outlet to cast the aluminum silicon alloy.

[0065] The positive beneficial effects of the present invention are:

[0066] The present invention adopts the method of acid dissolution to leach iron, calcium, magnesium, sodium, potassium, gallium, lithium and part of aluminum in fly ash, so as to obtain aluminum oxide and silicon oxide dissolution slag, and smelt to produce aluminum silicon alloy. The corresponding chloride crystals are crystallized from the saturated solution of certain chloride salts (ferric chloride, aluminum chloride, calcium chloride, magnesium chloride, sodium chloride, potassium chloride, gallium chloride, lithium chloride, etc.) by the crystallization method. After the salt crystals are redissolved, the corresponding hydroxide is precipitated by adjusting the pH value of the solution.

[0067] Compared with the existing acid method research, no pretreatment steps such as calcination, alkali calcination or acid calcination are used, thus avoiding high energy consumption and high pollution. The strong dissolving ability of hydrochloric acid allows most of the iron, calcium, magnesium, sodium, potassium, and a small part of aluminum in the fly ash to dissolve into the solution, thus achieving efficient and comprehensive utilization of fly ash.

[0068] The method of the present invention can realize the efficient and comprehensive utilization of fly ash, fully realize its resource value, and can achieve no emission of "three wastes" during and after the industrialization process. 4. Specific implementation methods

[0069] The following examples are only intended to further illustrate the present invention and are not intended to limit the present invention.

[0070] Embodiment 1:

[0071] Follow these steps:

[0072] a. Use chemical analysis methods to analyze the main components in fly ash: Al2O3, Fe2O3, TiO2, CaO, MgO, Na2O, K2O, etc.;

[0073] b. According to the weight of Fe2O3, CaO and MgO in fly ash material and the chemical reaction formula:

[0074] Fe2O3+6HCl=2FeCl3+3H2O; CaO+2HCl=CaCl2+H2O; MgO+2HCl=MgCl2+H2O, calculate the amount of hydrochloric acid required for complete reaction, and add 10% excess hydrochloric acid;

[0075] c. Solid content: 10-40%, reaction temperature: 100°C, pressure: 0.1MPa, react for 2h under stirring, and separate the solid and liquid;

[0076] d. The dissolving liquid can be recycled after supplementing with concentrated hydrochloric acid; when the concentration of chlorides of iron, aluminum, calcium, magnesium, sodium, potassium, gallium, lithium, etc. in the solution reaches saturation, the corresponding chlorides are crystallized by cooling and solid-liquid separation is performed; iron chloride, aluminum chloride, calcium chloride, magnesium chloride, sodium chloride, potassium chloride, gallium chloride, lithium chloride, etc. can be crystallized and precipitated respectively;

[0077] e. Redissolve the chloride crystals separately: adjust the pH value of the chloride solution to pH=3.8 with calcium carbonate powder, precipitate iron hydroxide, filter, wash, and dry (to 500° C.) to produce iron oxide; adjust the pH value of the filtrate to pH=11 with sodium carbonate (or sodium hydroxide), and precipitate aluminum hydroxide;

[0078] f. The residue after hydrochloric acid dissolution is washed and dried. According to the aluminum and silicon (9-80%) contents of aluminum-silicon alloy, the aluminum oxide and silicon oxide contents of the raw material are adjusted with aluminum oxide and silica to meet the composition index requirements of the alloy, and then mixed with carbon (reducing agent) to form the alloy production raw material. The amount of carbon required for the complete reaction is calculated according to the reaction formula of Al2O3+1.5C=2Al+1.5CO2; SiO2+C=Si+CO2, and 1% is added to this amount. The smelting reaction is continued for 2 hours in a mineral heat reduction furnace with slag-free submerged arc high-temperature smelting technology at a temperature of 1900°C. The material is continuously added at the upper part and discharged from the lower outlet to cast the aluminum-silicon alloy.

[0079] Embodiment 2:

[0080] Follow these steps:

[0081] a. Use chemical analysis methods to analyze the content of the main components in fly ash: Al2O3, Fe2O3, TiO2, CaO, MgO, Na2O, K2O, etc.;

[0082] b. According to the weight of Fe2O3, CaO and MgO in fly ash material and the chemical reaction formula:

[0083] Fe2O3+6HCl=2FeCl3+3H2O; CaO+2HCl=CaCl2+H2O; MgO+2HCl=MgCl2+H2O, calculate the amount of hydrochloric acid required for complete reaction, and add 10% excess hydrochloric acid;

[0084] c. Solid content: 10-40%, reaction temperature: 100°C, pressure: 0.1MPa, react for 3h under stirring, and separate the solid and liquid;

[0085] d. The dissolving liquid can be recycled after supplementing with concentrated hydrochloric acid; when the concentration of chlorides of iron, aluminum, calcium, magnesium, sodium, potassium, gallium, lithium, etc. in the solution reaches saturation, the corresponding chlorides are crystallized by cooling and solid-liquid separation is performed; iron chloride, aluminum chloride, calcium chloride, magnesium chloride, sodium chloride, potassium chloride, gallium chloride, lithium chloride, etc. can be crystallized and precipitated respectively;

[0086] e. Redissolve the chloride crystals separately: adjust the pH value of the chloride solution to pH=3.8 with calcium carbonate powder, precipitate iron hydroxide, filter, wash, and dry (to 500° C.) to produce iron oxide; adjust the pH value of the filtrate to pH=11 with sodium carbonate (or sodium hydroxide), and precipitate aluminum hydroxide;

[0087] f. The residue after hydrochloric acid dissolution is washed and dried. According to the aluminum and silicon (9-80%) contents of aluminum-silicon alloy, the aluminum oxide and silicon oxide contents of the raw material are adjusted with aluminum oxide and silica to meet the composition index requirements of the alloy, and then mixed with carbon (reducing agent) to form the alloy production raw material. The amount of carbon required for the complete reaction is calculated according to the reaction formula of Al2O3+1.5C=2Al+1.5CO2; SiO2+C=Si+CO2, and 5% is added to this amount. The smelting reaction is continued for 2 hours in a mineral heat reduction furnace with slag-free submerged arc high-temperature smelting technology at a temperature of 1900°C, and the material is continuously added from the upper part and discharged from the lower outlet to cast the aluminum-silicon alloy.

[0088] Embodiment 3:

[0089] Follow these steps:

[0090] a. Use chemical analysis methods to analyze the main components in fly ash: Al2O3, Fe2O3, TiO2, CaO, MgO, Na2O, K2O, etc.;

[0091] b. According to the weight of Fe2O3, CaO and MgO in fly ash material and the chemical reaction formula:

[0092] Fe2O3+6HCl=2FeCl3+3H2O; CaO+2HCl=CaCl2+H2O; MgO+2HCl=MgCl2+H2O, calculate the amount of hydrochloric acid required for complete reaction, and add 10% excess hydrochloric acid;

[0093] c. Solid content: 10-40%, reaction temperature: 100°C, pressure: 0.1MPa, reaction for 4h under stirring, solid-liquid separation;

[0094] d. The dissolving liquid can be recycled after supplementing with concentrated hydrochloric acid; when the concentration of chlorides of iron, aluminum, calcium, magnesium, sodium, potassium, gallium, lithium, etc. in the solution reaches saturation, the corresponding chlorides are crystallized by cooling and solid-liquid separation is performed; iron chloride, aluminum chloride, calcium chloride, magnesium chloride, sodium chloride, potassium chloride, gallium chloride, lithium chloride, etc. can be crystallized and precipitated respectively;

[0095] e. Redissolve the chloride crystals separately: adjust the pH value of the chloride solution to pH=3.8 with calcium carbonate powder, precipitate iron hydroxide, filter, wash, and dry (to 500° C.) to produce iron oxide; adjust the pH value of the filtrate to pH=11 with sodium carbonate (or sodium hydroxide), and precipitate aluminum hydroxide;

[0096] f. The residue after hydrochloric acid dissolution is washed and dried. According to the aluminum and silicon (9-80%) contents of aluminum-silicon alloy, the aluminum oxide and silicon oxide contents of the raw material are adjusted with aluminum oxide and silica to meet the composition index requirements of the alloy, and then mixed with carbon (reducing agent) to form the alloy production raw material. The amount of carbon required for the complete reaction is calculated according to the reaction formula of Al2O3+1.5C=2Al+1.5CO2; SiO2+C=Si+CO2, and 10% is added to this amount. The smelting reaction is continued for 2 hours in a mineral heat reduction furnace with slag-free submerged arc high-temperature smelting technology at a temperature of 1900°C. The material is continuously added at the upper part and discharged from the lower outlet to cast the aluminum-silicon alloy.

[0097] Embodiment 4:

[0098] Follow these steps:

[0099] a. Use chemical analysis methods to analyze the content of the main components in fly ash: Al2O3, Fe2O3, TiO2, CaO, MgO, Na2O, K2O, etc.;

[0100] b. According to the weight of Fe2O3, CaO and MgO in fly ash material and the chemical reaction formula:

[0101] Fe2O3+6HCl=2FeCl3+3H2O; CaO+2HCl=CaCl2+H2O; MgO+2HCl=MgCl2+H2O, calculate the amount of hydrochloric acid required for complete reaction, and add 10% excess hydrochloric acid;

[0102] c. Solid content: 10-40%, reaction temperature: 120°C, pressure: 0.2MPa, reaction for 1h under stirring, solid-liquid separation;

[0103] d. The dissolving liquid can be recycled after supplementing with concentrated hydrochloric acid; when the concentration of chlorides of iron, aluminum, calcium, magnesium, sodium, potassium, gallium, lithium, etc. in the solution reaches saturation, the corresponding chlorides are crystallized by cooling and solid-liquid separation is performed; iron chloride, aluminum chloride, calcium chloride, magnesium chloride, sodium chloride, potassium chloride, gallium chloride, lithium chloride, etc. can be crystallized and precipitated respectively;

[0104] e. Redissolve the chloride crystals separately: adjust the pH value of the chloride solution to pH=3.8 with calcium carbonate powder, precipitate iron hydroxide, filter, wash, and dry (to 500° C.) to produce iron oxide; adjust the pH value of the filtrate to pH=11 with sodium carbonate (or sodium hydroxide), and precipitate aluminum hydroxide;

[0105] f. The residue after hydrochloric acid dissolution is washed and dried. According to the aluminum and silicon (9-80%) contents of aluminum-silicon alloy, the aluminum oxide and silicon oxide contents of the raw material are adjusted with aluminum oxide and silica to meet the composition index requirements of the alloy, and then mixed with carbon (reducing agent) to form the alloy production raw material. The amount of carbon required for the complete reaction is calculated according to the reaction formula of Al2O3+1.5C=2Al+1.5CO2; SiO2+C=Si+CO2, and 20% is added to this amount. The smelting reaction is continued for 2 hours in a mineral heat reduction furnace with slag-free submerged arc high-temperature smelting technology at a temperature of 2000°C. The material is continuously added at the upper part and discharged from the lower outlet to cast the aluminum-silicon alloy.

[0106] Embodiment 5:

[0107] Follow these steps:

[0108] a. Use chemical analysis methods to analyze the content of the main components in fly ash: Al2O3, Fe2O3, TiO2, CaO, MgO, Na2O, K2O, etc.;

[0109] b. According to the weight of Fe2O3, CaO and MgO in fly ash material and the chemical reaction formula:

[0110] Fe2O3+6HCl=2FeCl3+3H2O; CaO+2HCl=CaCl2+H2O; MgO+2HCl=MgCl2+H2O, calculate the amount of hydrochloric acid required for complete reaction, and add 20% excess hydrochloric acid;

[0111] c. Solid content: 10-40%, reaction temperature: 130°C, pressure: 0.3MPa, reaction for 1h under stirring, solid-liquid separation;

[0112] d. The dissolving liquid can be recycled after supplementing with concentrated hydrochloric acid; when the concentration of chlorides of iron, aluminum, calcium, magnesium, sodium, potassium, gallium, lithium, etc. in the solution reaches saturation, the corresponding chlorides are crystallized by cooling and solid-liquid separation is performed; iron chloride, aluminum chloride, calcium chloride, magnesium chloride, sodium chloride, potassium chloride, gallium chloride, lithium chloride, etc. can be crystallized and precipitated respectively;

[0113] e. Redissolve the chloride crystals separately: adjust the pH value of the chloride solution to pH=3.8 with calcium carbonate powder, precipitate iron hydroxide, filter, wash, and dry (to 500° C.) to produce iron oxide; adjust the pH value of the filtrate to pH=11 with sodium carbonate (or sodium hydroxide), and precipitate aluminum hydroxide;

[0114] f. The residue after hydrochloric acid dissolution is washed and dried. According to the aluminum and silicon (9-80%) contents of aluminum-silicon alloy, the aluminum oxide and silicon oxide contents of the raw material are adjusted with aluminum oxide and silica to meet the composition index requirements of the alloy, and then mixed with carbon (reducing agent) to form the alloy production raw material. The amount of carbon required for the complete reaction is calculated according to the reaction formula of Al2O3+1.5C=2Al+1.5CO2; SiO2+C=Si+CO2, and 10% is added to this amount. The smelting reaction is continued for 2 hours in a mineral heat reduction furnace with slag-free submerged arc high-temperature smelting technology at a temperature of 2100°C, and the material is continuously added from the upper part and discharged from the lower outlet to cast the aluminum-silicon alloy.

[0115] Embodiment 6:

[0116] Follow these steps:

[0117] a. Use chemical analysis methods to analyze the content of the main components in fly ash: Al2O3, Fe2O3, TiO2, CaO, MgO, Na2O, K2O, etc.;

[0118] b. According to the weight of Fe2O3, CaO and MgO in fly ash material and the chemical reaction formula:

[0119] Fe2O3+6HCl=2FeCl3+3H2O; CaO+2HCl=CaCl2+H2O; MgO+2HCl=MgCl2+H2O, calculate the amount of hydrochloric acid required for complete reaction, and add 20% excess hydrochloric acid;

[0120] c. Solid content: 10-40%, reaction temperature: 150°C, pressure: 0.5MPa, reaction for 1h under stirring, solid-liquid separation;

[0121] d. The dissolving liquid can be recycled after supplementing with concentrated hydrochloric acid; when the concentration of chlorides of iron, aluminum, calcium, magnesium, sodium, potassium, gallium, lithium, etc. in the solution reaches saturation, the corresponding chlorides are crystallized by cooling and solid-liquid separation is performed; iron chloride, aluminum chloride, calcium chloride, magnesium chloride, sodium chloride, potassium chloride, gallium chloride, lithium chloride, etc. can be crystallized and precipitated respectively;

[0122] e. Redissolve the chloride crystals separately: adjust the pH value of the chloride solution to pH=3.8 with calcium carbonate powder, precipitate iron hydroxide, filter, wash, and dry (to 500° C.) to produce iron oxide; adjust the pH value of the filtrate to pH=11 with sodium carbonate (or sodium hydroxide), and precipitate aluminum hydroxide;

[0123] f. The residue after hydrochloric acid dissolution is washed and dried. According to the aluminum and silicon (9-80%) contents of aluminum-silicon alloy, the aluminum oxide and silicon oxide contents of the raw material are adjusted with aluminum oxide and silica to meet the composition index requirements of the alloy, and then mixed with carbon (reducing agent) to form the alloy production raw material. The amount of carbon required for the complete reaction is calculated according to the reaction formula of Al2O3+1.5C=2Al+1.5CO2; SiO2+C=Si+CO2, and 5% is added to this amount. The smelting reaction is continued for 2 hours in a mineral heat reduction furnace with slag-free submerged arc high-temperature smelting technology at a temperature of 2200°C. The material is continuously added at the upper part and discharged from the lower outlet to be cast into aluminum-silicon alloy.

[0124] Embodiment 7:

[0125] Follow these steps:

[0126] a. Use chemical analysis methods to analyze the content of the main components in fly ash: Al2O3, Fe2O3, TiO2, CaO, MgO, Na2O, K2O, etc.;

[0127] b. According to the weight of Fe2O3, CaO and MgO in fly ash material and the chemical reaction formula:

[0128] Fe2O3+6HCl=2FeCl3+3H2O; CaO+2HCl=CaCl2+H2O; MgO+2HCl=MgCl2+H2O, calculate the amount of hydrochloric acid required for complete reaction, and add 30% excess hydrochloric acid;

[0129] c. Solid content: 10-40%, reaction temperature: 120°C, pressure: 0.2MPa, react for 2h under stirring, and separate the solid and liquid;

[0130] d. The dissolving liquid can be recycled after supplementing with concentrated hydrochloric acid; when the concentration of chlorides of iron, aluminum, calcium, magnesium, sodium, potassium, gallium, lithium, etc. in the solution reaches saturation, the corresponding chlorides are crystallized by cooling and solid-liquid separation is performed; iron chloride, aluminum chloride, calcium chloride, magnesium chloride, sodium chloride, potassium chloride, gallium chloride, lithium chloride, etc. can be crystallized and precipitated respectively;

[0131] e. Redissolve the chloride crystals separately: adjust the pH value of the chloride solution to pH=3.8 with calcium carbonate powder, precipitate iron hydroxide, filter, wash, and dry (to 500° C.) to produce iron oxide; adjust the pH value of the filtrate to pH=11 with sodium carbonate (or sodium hydroxide), and precipitate aluminum hydroxide;

[0132] f. The residue after hydrochloric acid dissolution is washed and dried. According to the aluminum and silicon (9-80%) contents of aluminum-silicon alloy, the aluminum oxide and silicon oxide contents of the raw material are adjusted with aluminum oxide and silica to meet the composition index requirements of the alloy, and then mixed with carbon (reducing agent) to form the alloy production raw material. The amount of carbon required for the complete reaction is calculated according to the reaction formula of Al2O3+1.5C=2Al+1.5CO2; SiO2+C=Si+CO2, and 10% is added to this amount. The smelting reaction is continued for 1 hour in a mineral heat reduction furnace with slag-free submerged arc high-temperature smelting technology at a temperature of 2300°C, and the material is continuously added from the upper part and discharged from the lower outlet to cast the aluminum-silicon alloy.

[0133] Embodiment 8:

[0134] Follow these steps:

[0135] a. Use chemical analysis methods to analyze the content of the main components in fly ash: Al2O3, Fe2O3, TiO2, CaO, MgO, Na2O, K2O, etc.;

[0136] b. According to the weight of Fe2O3, CaO and MgO in fly ash material and the chemical reaction formula:

[0137] Fe2O3+6HCl=2FeCl3+3H2O; CaO+2HCl=CaCl2+H2O; MgO+2HCl=MgCl2+H2O, calculate the amount of hydrochloric acid required for complete reaction, and add 30% excess hydrochloric acid;

[0138] c. Solid content: 10-40%, reaction temperature: 100°C, pressure: 0.1MPa, react for 3h under stirring, and separate the solid and liquid;

[0139] d. The dissolving liquid can be recycled after supplementing with concentrated hydrochloric acid; when the concentration of chlorides of iron, aluminum, calcium, magnesium, sodium, potassium, gallium, lithium, etc. in the solution reaches saturation, the corresponding chlorides are crystallized by cooling and solid-liquid separation is performed; iron chloride, aluminum chloride, calcium chloride, magnesium chloride, sodium chloride, potassium chloride, gallium chloride, lithium chloride, etc. can be crystallized and precipitated respectively;

[0140] e. Redissolve the chloride crystals separately: adjust the pH value of the chloride solution to pH=3.8 with calcium carbonate powder, precipitate iron hydroxide, filter, wash, and dry (to 500° C.) to produce iron oxide; adjust the pH value of the filtrate to pH=11 with sodium carbonate (or sodium hydroxide), and precipitate aluminum hydroxide;

[0141] f. The residue after hydrochloric acid dissolution is washed and dried. According to the aluminum and silicon (9-80%) contents of aluminum-silicon alloy, the aluminum oxide and silicon oxide contents of the raw material are adjusted with aluminum oxide and silica to meet the composition index requirements of the alloy, and then mixed with carbon (reducing agent) to form the alloy production raw material. The amount of carbon required for the complete reaction is calculated according to the reaction formula of Al2O3+1.5C=2Al+1.5CO2; SiO2+C=Si+CO2, and 10% is added to this amount. The smelting reaction is continued for 2 hours in a mineral heat reduction furnace with slag-free submerged arc high-temperature smelting technology at a temperature of 2000°C. The material is continuously added at the upper part and discharged from the lower outlet to cast the aluminum-silicon alloy.

[0142] Embodiment 9:

[0143] Follow these steps:

[0144] a. Use chemical analysis methods to analyze the main components in fly ash: Al2O3, Fe2O3, TiO2, CaO, MgO, Na2O, K2O, etc.;

[0145] b. According to the weight of Fe2O3, CaO and MgO in fly ash material and the chemical reaction formula:

[0146] Fe2O3+6HCl=2FeCl3+3H2O; CaO+2HCl=CaCl2+H2O; MgO+2HCl=MgCl2+H2O, calculate the amount of hydrochloric acid required for complete reaction, and add 30% excess hydrochloric acid;

[0147] c. Solid content: 10-40%, reaction temperature: 120°C, pressure: 0.2MPa, react for 3h under stirring, and separate the solid and liquid;

[0148] d. The dissolving liquid can be recycled after supplementing with concentrated hydrochloric acid; when the concentration of chlorides of iron, aluminum, calcium, magnesium, sodium, potassium, gallium, lithium, etc. in the solution reaches saturation, the corresponding chlorides are crystallized by cooling and solid-liquid separation is performed; iron chloride, aluminum chloride, calcium chloride, magnesium chloride, sodium chloride, potassium chloride, gallium chloride, lithium chloride, etc. can be crystallized and precipitated respectively;

[0149] e. Redissolve the chloride crystals separately: adjust the pH value of the chloride solution to pH=3.8 with calcium carbonate powder, precipitate iron hydroxide, filter, wash, and dry (to 500° C.) to produce iron oxide; adjust the pH value of the filtrate to pH=11 with sodium carbonate (or sodium hydroxide), and precipitate aluminum hydroxide;

[0150] f. The residue after hydrochloric acid dissolution is washed and dried. According to the aluminum and silicon (9-80%) contents of aluminum-silicon alloy, the aluminum oxide and silicon oxide contents of the raw material are adjusted with alumina and silica to meet the composition index requirements of the alloy, and then mixed with carbon (reducing agent) to form the alloy production raw material. The amount of carbon required for the complete reaction is calculated according to the reaction formula of Al2O3+1.5C=2Al+1.5CO2; SiO2+C=Si+CO2, and 20% is added to this amount. The smelting reaction is continued for 3 hours in a mineral heat reduction furnace with slag-free submerged arc high-temperature smelting technology at a temperature of 2200°C, and the material is continuously added from the upper part and discharged from the lower outlet to cast the aluminum-silicon alloy.

[0151] Embodiment 10:

[0152] Follow these steps:

[0153] a. Use chemical analysis methods to analyze the main components in fly ash: Al2O3, Fe2O3, TiO2, CaO, MgO, Na2O, K2O, etc.;

[0154] b. According to the weight of Fe2O3, CaO and MgO in fly ash material and the chemical reaction formula:

[0155] Fe2O3+6HCl=2FeCl3+3H2O; CaO+2HCl=CaCl2+H2O; MgO+2HCl=MgCl2+H2O, calculate the amount of hydrochloric acid required for complete reaction, and add 20% excess hydrochloric acid;

[0156] c. Solid content: 10-40%, reaction temperature: 130°C, pressure: 0.3MPa, react for 3h under stirring, and separate the solid and liquid;

[0157] d. The dissolving liquid can be recycled after supplementing with concentrated hydrochloric acid; when the concentration of chlorides of iron, aluminum, calcium, magnesium, sodium, potassium, gallium, lithium, etc. in the solution reaches saturation, the corresponding chlorides are crystallized by cooling and solid-liquid separation is performed; iron chloride, aluminum chloride, calcium chloride, magnesium chloride, sodium chloride, potassium chloride, gallium chloride, lithium chloride, etc. can be crystallized and precipitated respectively;

[0158] e. Redissolve the chloride crystals separately: adjust the pH value of the chloride solution to pH=3.8 with calcium carbonate powder, precipitate iron hydroxide, filter, wash, and dry (to 500° C.) to produce iron oxide; adjust the pH value of the filtrate to pH=11 with sodium carbonate (or sodium hydroxide), and precipitate aluminum hydroxide;

[0159] f. The residue after hydrochloric acid dissolution is washed and dried. According to the aluminum and silicon (9-80%) contents of aluminum-silicon alloy, the aluminum oxide and silicon oxide contents of the raw material are adjusted with aluminum oxide and silica to meet the composition index requirements of the alloy, and then mixed with carbon (reducing agent) to form the alloy production raw material. The amount of carbon required for the complete reaction is calculated according to the reaction formula of Al2O3+1.5C=2Al+1.5CO2; SiO2+C=Si+CO2, and 5% is added to this amount. The smelting reaction is continued for 2 hours in a mineral heat reduction furnace with slag-free submerged arc high-temperature smelting technology at a temperature of 2100°C. The material is continuously added at the upper part and discharged from the lower outlet to cast the aluminum-silicon alloy.

[0160] Embodiment 11:

[0161] Follow these steps:

[0162] a. Use chemical analysis methods to analyze the main components in fly ash: Al2O3, Fe2O3, TiO2, CaO, MgO, Na2O, K2O, etc.;

[0163] b. According to the weight of Fe2O3, CaO and MgO in fly ash material and the chemical reaction formula:

[0164] Fe2O3+6HCl=2FeCl3+3H2O; CaO+2HCl=CaCl2+H2O; MgO+2HCl=MgCl2+H2O, calculate the amount of hydrochloric acid required for complete reaction, and add 20% excess hydrochloric acid;

[0165] c. Solid content: 10-40%, reaction temperature: 150°C, pressure: 0.5MPa, react for 2h under stirring, and separate the solid and liquid;

[0166] d. The dissolving liquid can be recycled after supplementing with concentrated hydrochloric acid; when the concentration of chlorides of iron, aluminum, calcium, magnesium, sodium, potassium, gallium, lithium, etc. in the solution reaches saturation, the corresponding chlorides are crystallized by cooling and solid-liquid separation is performed; iron chloride, aluminum chloride, calcium chloride, magnesium chloride, sodium chloride, potassium chloride, gallium chloride, lithium chloride, etc. can be crystallized and precipitated respectively;

[0167] e. Redissolve the chloride crystals separately: adjust the pH value of the chloride solution to pH=3.8 with calcium carbonate powder, precipitate iron hydroxide, filter, wash, and dry (to 500° C.) to produce iron oxide; adjust the pH value of the filtrate to pH=11 with sodium carbonate (or sodium hydroxide), and precipitate aluminum hydroxide;

[0168] f. The residue after hydrochloric acid dissolution is washed and dried. According to the aluminum and silicon (9-80%) contents of aluminum-silicon alloy, the aluminum oxide and silicon oxide contents of the raw material are adjusted with aluminum oxide and silica to meet the composition index requirements of the alloy, and then mixed with carbon (reducing agent) to form the alloy production raw material. The amount of carbon required for the complete reaction is calculated according to the reaction formula of Al2O3+1.5C=2Al+1.5CO2; SiO2+C=Si+CO2, and 10% is added to this amount. The smelting reaction is continued for 2 hours in a mineral heat reduction furnace with slag-free submerged arc high-temperature smelting technology at a temperature of 2300°C. The material is continuously added at the upper part and discharged from the lower outlet to cast the aluminum-silicon alloy.

[0169] Embodiment 12:

[0170] Follow these steps:

[0171] a. Use chemical analysis methods to analyze the content of the main components in fly ash: Al2O3, Fe2O3, TiO2, CaO, MgO, Na2O, K2O, etc.;

[0172] b. According to the weight of Fe2O3, CaO and MgO in fly ash material and the chemical reaction formula:

[0173] Fe2O3+6HCl=2FeCl3+3H2O; CaO+2HCl=CaCl2+H2O; MgO+2HCl=MgCl2+H2O, calculate the amount of hydrochloric acid required for complete reaction, and add 30% excess hydrochloric acid;

[0174] c. Solid content: 10-40%, reaction temperature: 100°C, pressure: 0.1MPa, react for 3h under stirring, and separate the solid and liquid;

[0175] d. The dissolving liquid can be recycled after supplementing with concentrated hydrochloric acid; when the concentration of chlorides of iron, aluminum, calcium, magnesium, sodium, potassium, gallium, lithium, etc. in the solution reaches saturation, the corresponding chlorides are crystallized by cooling and solid-liquid separation is performed; iron chloride, aluminum chloride, calcium chloride, magnesium chloride, sodium chloride, potassium chloride, gallium chloride, lithium chloride, etc. can be crystallized and precipitated respectively;

[0176] e. Redissolve the chloride crystals separately: adjust the pH value of the chloride solution to pH=3.8 with calcium carbonate powder, precipitate iron hydroxide, filter, wash, and dry (to 500° C.) to produce iron oxide; adjust the pH value of the filtrate to pH=11 with sodium carbonate (or sodium hydroxide), and precipitate aluminum hydroxide;

[0177] f. The residue after hydrochloric acid dissolution is washed and dried. According to the aluminum and silicon (9-80%) contents of aluminum-silicon alloy, the aluminum oxide and silicon oxide contents of the raw material are adjusted with aluminum oxide and silica to meet the composition index requirements of the alloy, and then mixed with carbon (reducing agent) to form the alloy production raw material. The amount of carbon required for the complete reaction is calculated according to the reaction formula of Al2O3+1.5C=2Al+1.5CO2; SiO2+C=Si+CO2, and 20% is added to this amount. The smelting reaction is continued for 2 hours in a mineral heat reduction furnace with slag-free submerged arc high-temperature smelting technology at a temperature of 2000°C. The material is continuously added at the upper part and discharged from the lower outlet to cast the aluminum-silicon alloy.

[0178] Embodiment 13:

[0179] Follow these steps:

[0180] a. Use chemical analysis methods to analyze the main components in fly ash: Al2O3, Fe2O3, TiO2, CaO, MgO, Na2O, K2O, etc.;

[0181] b. According to the weight of Fe2O3, CaO and MgO in fly ash material and the chemical reaction formula:

[0182] Fe2O3+6HCl=2FeCl3+3H2O; CaO+2HCl=CaCl2+H2O; MgO+2HCl=MgCl2+H2O, calculate the amount of hydrochloric acid required for complete reaction, and add 30% excess hydrochloric acid;

[0183] c. Solid content: 10-40%, reaction temperature: 130°C, pressure: 0.3MPa, react for 2h under stirring, and separate the solid and liquid;

[0184] d. The dissolving liquid can be recycled after supplementing with concentrated hydrochloric acid; when the concentration of chlorides of iron, aluminum, calcium, magnesium, sodium, potassium, gallium, lithium, etc. in the solution reaches saturation, the corresponding chlorides are crystallized by cooling and solid-liquid separation is performed; iron chloride, aluminum chloride, calcium chloride, magnesium chloride, sodium chloride, potassium chloride, gallium chloride, lithium chloride, etc. can be crystallized and precipitated respectively;

[0185] e. Redissolve the chloride crystals separately: adjust the pH value of the chloride solution to pH=3.8 with calcium carbonate powder, precipitate iron hydroxide, filter, wash, and dry (to 500° C.) to produce iron oxide; adjust the pH value of the filtrate to pH=11 with sodium carbonate (or sodium hydroxide), and precipitate aluminum hydroxide;

[0186] f. The residue after hydrochloric acid dissolution is washed and dried. According to the aluminum and silicon (9-80%) contents of aluminum-silicon alloy, the aluminum oxide and silicon oxide contents of the raw material are adjusted with aluminum oxide and silica to meet the composition index requirements of the alloy, and then mixed with carbon (reducing agent) to form the alloy production raw material. The amount of carbon required for the complete reaction is calculated according to the reaction formula of Al2O3+1.5C=2Al+1.5CO2; SiO2+C=Si+CO2, and 5% is added to this amount. The smelting reaction is continued for 2 hours in a mineral heat reduction furnace with slag-free submerged arc high-temperature smelting technology at a temperature of 2200°C. The material is continuously added at the upper part and discharged from the lower outlet to be cast into aluminum-silicon alloy.

[0187] Embodiment 14:

[0188] Follow these steps:

[0189] a. Use chemical analysis methods to analyze the main components in fly ash: Al2O3, Fe2O3, TiO2, CaO, MgO, Na2O, K2O, etc.;

[0190] b. According to the weight of Fe2O3, CaO and MgO in fly ash material and the chemical reaction formula:

[0191] Fe2O3+6HCl=2FeCl3+3H2O; CaO+2HCl=CaCl2+H2O; MgO+2HCl=MgCl2+H2O, calculate the amount of hydrochloric acid required for complete reaction, and add 20% excess hydrochloric acid;

[0192] c. Solid content: 10-40%, reaction temperature: 140°C, pressure: 0.4MPa, react for 2h under stirring, and separate the solid and liquid;

[0193] d. The dissolving liquid can be recycled after supplementing with concentrated hydrochloric acid; when the concentration of chlorides of iron, aluminum, calcium, magnesium, sodium, potassium, gallium, lithium, etc. in the solution reaches saturation, the corresponding chlorides are crystallized by cooling and solid-liquid separation is performed; iron chloride, aluminum chloride, calcium chloride, magnesium chloride, sodium chloride, potassium chloride, gallium chloride, lithium chloride, etc. can be crystallized and precipitated respectively;

[0194] e. Redissolve the chloride crystals separately: adjust the pH value of the chloride solution to pH=3.8 with calcium carbonate powder, precipitate iron hydroxide, filter, wash, and dry (to 500° C.) to produce iron oxide; adjust the pH value of the filtrate to pH=11 with sodium carbonate (or sodium hydroxide), and precipitate aluminum hydroxide;

[0195] f. The residue after hydrochloric acid dissolution is washed and dried. According to the aluminum and silicon (9-80%) contents of aluminum-silicon alloy, the aluminum oxide and silicon oxide contents of the raw material are adjusted with aluminum oxide and silica to meet the composition index requirements of the alloy, and then mixed with carbon (reducing agent) to form the alloy production raw material. The amount of carbon required for the complete reaction is calculated according to the reaction formula of Al2O3+1.5C=2Al+1.5CO2; SiO2+C=Si+CO2, and 10% is added to this amount. The smelting reaction is continued for 2 hours in a mineral heat reduction furnace with slag-free submerged arc high-temperature smelting technology at a temperature of 1900°C. The material is continuously added at the upper part and discharged from the lower outlet to cast the aluminum-silicon alloy.

[0196] Embodiment 15:

[0197] Follow these steps:

[0198] a. Use chemical analysis methods to analyze the content of the main components in fly ash: Al2O3, Fe2O3, TiO2, CaO, MgO, Na2O, K2O, etc.;

[0199] b. According to the weight of Fe2O3, CaO and MgO in fly ash material and the chemical reaction formula:

[0200] Fe2O3+6HCl=2FeCl3+3H2O; CaO+2HCl=CaCl2+H2O; MgO+2HCl=MgCl2+H2O, calculate the amount of hydrochloric acid required for complete reaction, and add 20% excess hydrochloric acid;

[0201] c. Solid content: 10-40%, reaction temperature: 110°C, pressure: 0.1MPa, react for 3h under stirring, and separate the solid and liquid;

[0202] d. The dissolving liquid can be recycled after supplementing with concentrated hydrochloric acid; when the concentration of chlorides of iron, aluminum, calcium, magnesium, sodium, potassium, gallium, lithium, etc. in the solution reaches saturation, the corresponding chlorides are crystallized by cooling and solid-liquid separation is performed; iron chloride, aluminum chloride, calcium chloride, magnesium chloride, sodium chloride, potassium chloride, gallium chloride, lithium chloride, etc. can be crystallized and precipitated respectively;

[0203] e. Redissolve the chloride crystals separately: adjust the pH value of the chloride solution to pH=3.8 with calcium carbonate powder, precipitate iron hydroxide, filter, wash, and dry (to 500° C.) to produce iron oxide; adjust the pH value of the filtrate to pH=11 with sodium carbonate (or sodium hydroxide), and precipitate aluminum hydroxide;

[0204] f. The residue after hydrochloric acid dissolution is washed and dried. According to the aluminum and silicon (9-80%) contents of aluminum-silicon alloy, the aluminum oxide and silicon oxide contents of the raw material are adjusted with aluminum oxide and silica to meet the composition index requirements of the alloy, and then mixed with carbon (reducing agent) to form the alloy production raw material. The amount of carbon required for the complete reaction is calculated according to the reaction formula of Al2O3+1.5C=2Al+1.5CO2; SiO2+C=Si+CO2, and 10% is added to this amount. The smelting reaction is continued for 2 hours in a mineral heat reduction furnace with slag-free submerged arc high-temperature smelting technology at a temperature of 2400°C. The material is continuously added at the upper part and discharged from the lower outlet to be cast into aluminum-silicon alloy.

[0205] Embodiment 16:

[0206] Follow these steps:

[0207] a. Use chemical analysis methods to analyze the content of the main components in fly ash: Al2O3, Fe2O3, TiO2, CaO, MgO, Na2O, K2O, etc.;

[0208] b. According to the weight of Fe2O3, CaO and MgO in fly ash material and the chemical reaction formula:

[0209] Fe2O3+6HCl=2FeCl3+3H2O; CaO+2HCl=CaCl2+H2O; MgO+2HCl=MgCl2+H2O, calculate the amount of hydrochloric acid required for complete reaction, and add 20% excess hydrochloric acid;

[0210] c. Solid content: 10-40%, reaction temperature: 110°C, pressure: 0.1MPa, reaction for 1h under stirring, solid-liquid separation;

[0211] d. The dissolving liquid can be recycled after supplementing with concentrated hydrochloric acid; when the concentration of chlorides of iron, aluminum, calcium, magnesium, sodium, potassium, gallium, lithium, etc. in the solution reaches saturation, the corresponding chlorides are crystallized by cooling and solid-liquid separation is performed; iron chloride, aluminum chloride, calcium chloride, magnesium chloride, sodium chloride, potassium chloride, gallium chloride, lithium chloride, etc. can be crystallized and precipitated respectively;

[0212] e. Redissolve the chloride crystals separately: adjust the pH value of the chloride solution to pH=3.8 with calcium carbonate powder, precipitate iron hydroxide, filter, wash, and dry (to 500° C.) to produce iron oxide; adjust the pH value of the filtrate to pH=11 with sodium carbonate (or sodium hydroxide), and precipitate aluminum hydroxide;

[0213] f. The residue after hydrochloric acid dissolution is washed and dried. According to the aluminum and silicon (9-80%) contents of aluminum-silicon alloy, the aluminum oxide and silicon oxide contents of the raw material are adjusted with aluminum oxide and silica to meet the composition index requirements of the alloy, and then mixed with carbon (reducing agent) to form the alloy production raw material. The amount of carbon required for the complete reaction is calculated according to the reaction formula of Al2O3+1.5C=2Al+1.5CO2; SiO2+C=Si+CO2, and 20% is added to this amount. The smelting reaction is continued for 2 hours in a mineral heat reduction furnace with slag-free submerged arc high-temperature smelting technology at a temperature of 2000°C. The material is continuously added at the upper part and discharged from the lower outlet to cast the aluminum-silicon alloy.

[0214] Embodiment 17:

[0215] Follow these steps:

[0216] a. Use chemical analysis methods to analyze the main components in fly ash: Al2O3, Fe2O3, TiO2, CaO, MgO, Na2O, K2O, etc.;

[0217] b. According to the weight of Fe2O3, CaO and MgO in fly ash material and the chemical reaction formula:

[0218] Fe2O3+6HCl=2FeCl3+3H2O; CaO+2HCl=CaCl2+H2O; MgO+2HCl=MgCl2+H2O, calculate the amount of hydrochloric acid required for complete reaction, and add 30% excess hydrochloric acid;

[0219] c. Solid content: 10-40%, reaction temperature: 110°C, pressure: 0.1MPa, react for 2h under stirring, and separate the solid and liquid;

[0220] d. The dissolving liquid can be recycled after supplementing with concentrated hydrochloric acid; when the concentration of chlorides of iron, aluminum, calcium, magnesium, sodium, potassium, gallium, lithium, etc. in the solution reaches saturation, the corresponding chlorides are crystallized by cooling and solid-liquid separation is performed; iron chloride, aluminum chloride, calcium chloride, magnesium chloride, sodium chloride, potassium chloride, gallium chloride, lithium chloride, etc. can be crystallized and precipitated respectively;

[0221] e. Redissolve the chloride crystals separately: adjust the pH value of the chloride solution to pH=3.8 with calcium carbonate powder, precipitate iron hydroxide, filter, wash, and dry (to 500° C.) to produce iron oxide; adjust the pH value of the filtrate to pH=11 with sodium carbonate (or sodium hydroxide), and precipitate aluminum hydroxide;

[0222] f. The residue after hydrochloric acid dissolution is washed and dried. According to the aluminum and silicon (9-80%) contents of aluminum-silicon alloy, the aluminum oxide and silicon oxide contents of the raw material are adjusted with aluminum oxide and silica to meet the composition index requirements of the alloy, and then mixed with carbon (reducing agent) to form the alloy production raw material. The amount of carbon required for the complete reaction is calculated according to the reaction formula of Al2O3+1.5C=2Al+1.5CO2; SiO2+C=Si+CO2, and 5% is added to this amount. The smelting reaction is continued for 2 hours in a mineral heat reduction furnace with slag-free submerged arc high-temperature smelting technology at a temperature of 1800°C. The material is continuously added at the upper part and discharged from the lower outlet to be cast into aluminum-silicon alloy.

Claims

1. The present invention relates to a method for comprehensive utilization of fly ash, characterized in that The following steps are involved: a. Use chemical analysis methods to analyze the main components in fly ash: Al2O3, Fe2O3, TiO2, CaO, MgO, Na2O, K2O, etc.; b. According to the content of Fe2O3, CaO and MgO in fly ash materials and the chemical reaction formula: Fe2O3+6HCl=2FeCl3+3H2O; CaO+2HCl=CaCl2+H2O; MgO+2HCl=MgCl2+H2O, calculate the amount of hydrochloric acid required for complete reaction, and add 10-50% excess hydrochloric acid; c. Solid content: 10-40%, reaction temperature: 100-150°C, pressure: 0.1-0.8MPa, react for 1-5h under stirring, and separate the solid and liquid; d. The solution in which the chloride salts have not reached the saturated concentration can be used to decompose fly ash after adding concentrated hydrochloric acid; when the concentration of a certain chloride of iron, aluminum, calcium, magnesium, sodium, potassium, gallium, lithium, etc. in the solution reaches the saturated concentration, the temperature is lowered to precipitate crystals, and the solid-liquid separation can be carried out; iron chloride, aluminum chloride, calcium chloride, magnesium chloride, sodium chloride, potassium chloride, gallium chloride, lithium chloride, etc. can be crystallized and precipitated respectively; e. Redissolve the chloride crystals separately: adjust the pH value of the chloride solution to pH=3.8 with calcium carbonate powder (or calcium hydroxide), precipitate iron hydroxide, filter, wash, and dry (to 500° C.) to make iron oxide; adjust the pH value of the solution to pH=11 with sodium carbonate (or sodium hydroxide), precipitate aluminum hydroxide; the pH value of other chloride solutions can also be adjusted with sodium carbonate (or sodium hydroxide) until the hydroxide precipitates; f. After the filter residue is dissolved with hydrochloric acid, it is washed and dried. According to the aluminum and silicon (9-80%) contents of aluminum-silicon alloy, the aluminum oxide and silicon oxide contents of the raw material are adjusted with aluminum oxide and silica to meet the composition index requirements of the alloy, and then it is mixed with carbon (reducing agent) to form the alloy production raw material. The amount of carbon required for the complete reaction is calculated according to the reaction formula of Al2O3+1.5C=2Al+1.5CO2; SiO2+C=Si+CO2, and 0-20% is added to this amount. The smelting reaction is continued for 30min-3h at a temperature of 1800-2400℃ using a mineral heat reduction furnace and slag-free submerged arc high-temperature smelting technology. The material is continuously added at the upper part and discharged from the lower outlet to cast the aluminum-silicon alloy.

2. According to claim 1, it is characterized in that: Use chemical analysis methods to analyze the content of the main components in fly ash: Al2O3, Fe2O3, TiO2, CaO, MgO, Na2O, K2O, etc.; according to the content of Fe2O3, CaO, and MgO in the fly ash material, and the chemical reaction formula: Fe2O3+6HCl=2FeCl3+3H2O; CaO+2HCl=CaCl2+H2O; MgO+2HCl=MgCl2+H2O, calculate the amount of hydrochloric acid required for the complete reaction, and add 10-30% excess hydrochloric acid.

3. According to claim 1, it is characterized in that: The reaction conditions for decomposing fly ash with hydrochloric acid are: solid content: 10-40%, temperature: 100-140°C, pressure: 0.1-0.4MPa, reaction time 1-3h, and then solid-liquid separation of the slurry.

4. According to claim 1, it is characterized in that: The dissolving liquid whose chloride salts have not reached the saturated concentration can be used to decompose fly ash after adding hydrochloric acid; when the concentration of a certain chloride of iron, aluminum, calcium, magnesium, sodium, potassium, gallium, lithium, etc. in the solution reaches the saturated concentration, the temperature is lowered to precipitate crystals and the solid-liquid is separated; iron chloride, aluminum chloride, calcium chloride, magnesium chloride, sodium chloride, potassium chloride, gallium chloride, lithium chloride, etc. can be crystallized and precipitated respectively.

5. According to claim 1, it is characterized in that: Redissolve the chloride crystals separately: adjust the pH value of the chloride solution to pH = 3.8 with calcium carbonate powder (or calcium hydroxide), precipitate iron hydroxide, filter, wash, and dry (to 500°C) to make iron oxide; adjust the pH value of the solution to pH = 11 with sodium carbonate (or sodium hydroxide), precipitate aluminum hydroxide; other chloride solutions can also be adjusted to pH with sodium carbonate (or sodium hydroxide) until the hydroxide is precipitated.

6. According to claim 1, it is characterized in that: The filter residue after hydrochloric acid dissolution is washed and dried, and then, according to the aluminum and silicon (9-80%) contents of the aluminum-silicon alloy, the aluminum oxide and silicon oxide contents of the raw material are adjusted with alumina and silica to meet the composition index requirements of the alloy, and then mixed with carbon (reducing agent) to form the alloy production raw material, and the amount of carbon required for the complete reaction is calculated according to the reaction formula of Al2O3+1.5C=2Al+1.5CO2; SiO2+C=Si+CO2, and 0-20% is added to this amount. A mineral heat reduction furnace is used, and slag-free submerged arc high-temperature smelting technology is adopted. At a temperature of 1800-2400°C, the smelting reaction is continued for 30min-3h, and the material is continuously added at the upper part and discharged from the lower outlet to cast the aluminum-silicon alloy.