Method for treating complex tin sludge and comprehensively recovering various valuable metals
Through process steps such as roasting, leaching, extraction and replacement, the problem of recycling of various valuable metals in complex tin mud is solved, and the effective recycling of metals such as tin, copper, indium, bismuth, and silver is achieved, reducing costs and optimizing Process parameters solve the problem of high cost of process sewage treatment in the prior art.
Patent Information
- Application Number
- CN202411209509.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-06
AI Technical Summary
The prior art fails to effectively treat and recover a variety of valuable metals in complex tin mud, especially when the tin content is reduced, resulting in high cost of process wastewater treatment and failure to realize the pricing and recycling of copper metals.
Complex steps include roasting, sulfuric acid leaching, P204 extraction, displacement, reduction and smelting, oxidation and slag separation, continuous crystallization and electrolysis, and tin is achieved through the optimization of parameters such as calcining temperature, kiln tail negative pressure, extraction temperature and replacement conditions. Comprehensive recycling of valuable metals such as copper, indium, bismuth, and silver.
It realizes flexible recycling of various valuable metals in complex tin mud, reduces production costs, improves economic benefits, and reduces waste liquid disposal costs through the optimization of process parameters.
Smart Images

Figure CN119082460A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of tin smelting, and more specifically relates to a method for treating complex tin mud and comprehensively recovering multiple valuable metals. Background Art
[0002] Tin sludge is a tin-containing material with a wide range of sources and complex components. Some of it comes from electroplating tin stripping water after neutralization and precipitation, and some comes from SnCl 4 Catalyst production process, etc. Due to its high tin content, it is often used as a tin material for tin recovery. Usually, a rotary kiln is used for drying, and tin concentrate is put into an electric furnace for reduction smelting to produce crude tin. The crude tin is further refined by pyrometallurgy to produce refined tin. The copper slag (or sulfur slag) produced by the pyrometallurgy and sulfur removal process is directly sold according to the tin content; this treatment process fails to achieve the pricing and recycling of copper metal. Patent application number 202211723439.8 adds sulfuric acid and hydrogen peroxide to tin mud with a tin content of 30-40% to reduce the copper content and increase the tin content. The copper in the leachate is added with alkali to form a copper hydroxide product; this method is more suitable for tin mud with a higher tin content. If the tin content of the tin mud is reduced, a large amount of process wastewater will be generated while consuming a large amount of leaching agent, and the cost of wastewater treatment is high. Patent application No. 202210775040.8 discloses a process for preparing sodium stannate by direct roasting, alkali roasting, leaching, sulfidation to remove lead, and concentrated crystallization to treat tin-containing sludge, but does not specify the recovery of indium and copper valuable metals in complex tin sludge. There is no report on the comprehensive utilization and recovery of tin, copper, lead, indium, silver, antimony, and bismuth in complex tin sludge.
[0003] Therefore, how to provide a method for complex tin sludge treatment and comprehensive recovery of multiple valuable metals is a problem that technical personnel in this field urgently need to solve. Summary of the invention
[0004] In order to overcome the shortcomings and deficiencies in the prior art, the present invention provides a method for treating complex tin mud and comprehensively recovering multiple valuable metals. The present invention has strong versatility for various tin mud raw materials, and can comprehensively recover valuable metals such as copper, lead, antimony, indium, bismuth, and silver in the tin mud, effectively reducing production operation costs and achieving economic benefits.
[0005] In order to achieve the above object, the present invention adopts the following technical solution:
[0006] A method for treating complex tin sludge and comprehensively recovering multiple valuable metals, characterized in that it specifically comprises the following steps:
[0007] (1) calcining the complex tin mud in a rotary kiln at a calcination temperature of 300 to 900° C., a negative pressure of -10 to -50 Pa at the kiln tail, and a kiln rotation speed of 0.1 to 2.0 r / min to obtain calcined sand;
[0008] (2) leaching the roasted sand in sulfuric acid to obtain a leaching solution containing copper and indium and a leaching residue enriched with tin, lead, antimony, bismuth and silver;
[0009] (3) extracting indium from the leaching solution obtained in step (2) with P204 to obtain a raffinate and an indium-containing extract; stripping, neutralizing, and replacing the indium-containing extract to obtain a sponge indium product;
[0010] (4) the raffinate obtained in step (3) is replaced with iron powder at a temperature of 30 to 60° C. for 0.5 to 6 h to obtain a sponge copper product and a replaced liquid; the replaced liquid is pH adjusted to remove iron and then returned to step (2) and prepared with sulfuric acid for leaching;
[0011] (5) sending the leached slag obtained in step (2) to one of an electric furnace, an Ausmelt furnace or a side-blown furnace for reduction smelting to obtain a crude tin alloy and slag; the slag is sold as a fuming furnace material;
[0012] (6) subjecting the crude tin alloy to sulfidation in an oxidation pot to remove copper, and oxidation slag to separate high melting point copper and iron elements to obtain copper slag, iron slag and oxygen-refined tin; after the copper slag is screened, the undersize is returned to the rotary kiln for roasting, and the oversize and iron slag are returned for reduction smelting treatment;
[0013] (7) feeding the oxygen-refined tin into a continuous crystallizer for separation to obtain a tin ingot product and a crystallizer solder;
[0014] (8) If the crystallizer solder contains Ag>0.04%, solder electrolysis is used to obtain solder ingots that meet the GBT8012-2013 standard and anode mud rich in precious metals;
[0015] If the crystallizer solder contains Ag < 0.04%, a vacuum furnace is used for separation to obtain vacuum tin and lead-antimony-bismuth-silver alloy products.
[0016] Preferably, the mass percentage of water in the complex tin mud is 20-65%; the mass percentage of each component in the tin mud on a dry basis is: Sn 10-80%, Cu 0.1-30%, Pb 0.1-50%, Sb 0.1-10%, Bi 0.1-5.0%, In0.01-1.0%, Ag 0.001-0.5%, and the rest are impurities.
[0017] Preferably, if the tin mud contains less than 2.0% Cu or less than 0.2% In on a dry basis, steps (2) to (4) can be omitted, and the roasted sand from step (1) can be directly sent to step (5) for reduction smelting.
[0018] The beneficial effect of the above technical solution is: according to the content of each valuable metal in the complex tin mud, an economical recovery method can be flexibly selected to achieve the purpose of reducing unit consumption cost.
[0019] Preferably, the liquid-to-solid ratio of the leaching in step (2) is 3 to 10:1, the initial concentration of sulfuric acid is 10 to 300 g / L, the temperature is 25 to 90° C., and the time is 0.5 to 4 h.
[0020] The beneficial effect of the above technical solution is to determine feasible and economical process parameters for the leaching step.
[0021] Preferably, the reaction temperature of the extraction in step (3) is 25-60°C, and the oil (O) / (W) is 1 / 5-1 / 2.
[0022] Preferably, the sulfidation copper removal in step (6) is controlled at a temperature of 240-280°C, and the sulfur-copper weight ratio is 1:2-3; the covering material added to the oxidized slag is sawdust, the amount is 1-100 kg / t crude tin alloy, the temperature is 260-320°C, and the reaction time is 1-4 hours.
[0023] The beneficial effect of the above technical solution is to determine feasible and economical process parameters for sulfidation copper removal.
[0024] Preferably, if the oxygen-refined tin in step (6) contains Sb>1.5%, the oxygen-refined tin can omit step (7) and directly enter step (8) for vacuum furnace separation.
[0025] Preferably, if the oxygen-refined tin in step (6) contains Ag>0.04%, the oxygen-refined tin can omit step (7) and directly proceed to step (8) for solder electrolysis.
[0026] The beneficial effect of the above technical solution is: according to the content of each valuable metal in the complex tin mud, an economical recovery method can be flexibly selected to achieve the purpose of reducing unit consumption cost.
[0027] Preferably, the solder electrolysis in step (8) is carried out using fluorinated silicic acid as the electrolyte, and is produced by controlling the cell voltage to 0.1-0.25 V, the current intensity to 1300-2200 A, and the electrolyte temperature to 20-40° C.
[0028] The beneficial effect of the above technical solution is to determine feasible and economical process parameters for silicofluoric acid solder electrolysis.
[0029] Preferably, the specific operation of the vacuum separation in step (8) is: performing 2 to 3 levels of vacuum separation in a vacuum furnace, controlling the vacuum degree to 1 to 50 Pa and the temperature to 900 to 1500° C., so that lead, antimony and bismuth are volatilized to form a lead-antimony-bismuth alloy product.
[0030] The beneficial effect of the above technical solution is: determining feasible and economical process parameters for vacuum separation.
[0031] It can be seen from the above technical solutions that, compared with the prior art, the present invention provides a method for treating complex tin sludge and comprehensively recovering multiple valuable metals, which has the following beneficial effects:
[0032] (1) The present invention can specifically process various types of complex tin muds of different sources and components, showing the advantage of strong raw material adaptability.
[0033] (2) The present invention adopts pyrometallurgy as the main method and hydrometallurgy as the auxiliary method, and the pyrometallurgy + hydrometallurgy process is linked, fully exploring and giving play to the complementary advantages of different processes such as oxidative roasting, reduction smelting, fuming volatilization, pyrometallurgy, electrolytic refining, leaching, etc., to achieve comprehensive recovery of valuable metals such as tin, copper, lead, antimony, indium, bismuth, and silver in tin mud, reflecting the superiority and economy of the process.
[0034] (3) The present invention uses roasting, leaching and replacement methods to recover copper, which can be applied not only to the treatment of complex tin mud, but also to the treatment of copper slag produced by tin smelting, thus forming a circulation and recovery of copper in the production system and improving economic benefits.
[0035] (4) The present invention uses leaching, extraction, replacement and other methods to recover indium at the front end. Compared with the method of recovering indium from the electrolyte after reduction smelting of the indium element and electrolytic refining, the process is short and the operating cost can be effectively reduced.
[0036] (5) The replaced liquid of the present invention can be returned to the leaching solution after adjusting the pH value to remove iron, thereby reducing the cost of waste liquid disposal. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0038] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION
[0039] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0040] Example 1
[0041] A method for treating complex tin sludge and comprehensively recovering multiple valuable metals, specifically comprising the following steps:
[0042] 5000kg of complex tin mud, of which the mass percentage of water is 54.44%. The dry basis composition of the tin mud contains Sn55.54%, Cu 4.08%, Pb 0.33%, Sb 0.27%, Bi 0.27%, In 0.86% and Ag 0.002%, and the rest are impurities. It can be seen that the complex tin mud contains high copper and indium. The complex tin mud is put into a rotary kiln, the roasting temperature is 500-600℃, the negative pressure at the kiln tail is -10--20Pa, the kiln speed is 0.7-0.9r / min, and 2227.2kg of roasted sand is obtained, with the composition of Sn 56.37%, Cu 4.16%, Pb 0.34%, Sb 0.27%, Bi 0.28%, In 0.88%, Ag0.002%, and the rest are impurities.
[0043] The obtained roasted sand was leached under the conditions of liquid-to-solid ratio of 3:1, initial sulfuric acid concentration of 150 g / L, temperature of 70 °C, and time of 2.0 h to obtain 7.126 m3 of leaching solution containing 12.88 g / L Cu and 2.71 g / L In. 3 And 2064.2kg of leached residue.
[0044] The leaching solution was extracted with P204 at a temperature of 40°C and O / W=1 / 4, with an indium extraction rate of 98.5%, and the raffinate contained 0.04g / L In and 12.90g / L Cu. The raffinate was replaced with iron powder at a temperature of 40°C and a time of 2.5h to obtain 91.79kg of sponge copper product, containing 95.31% Cu. The extracted indium-containing extract was stripped with 1.06g / mL dilute hydrochloric acid at a temperature of 40°C and O / W=5 / 1, with an indium stripping rate of 99.3%, and the stripping solution contained 55.60g / L In; the stripping solution was finally neutralized and replaced to obtain 19.65kg of sponge indium product, containing 91.50% indium.
[0045] 2064.2 kg of leached slag was reduced and smelted in an electric furnace to produce 606.99 kg of slag and 1171.37 kg of crude tin alloy. The crude tin alloy composition was Sn 96.68%, Cu 0.08%, Pb 0.64%, Sb 0.46%, Bi 0.52%, and the rest were impurities.
[0046] The crude tin alloy was put into an oxidation pot, and sulfur was added at a sulfur-copper weight ratio of 1:2.8 at a temperature of 280°C to remove copper, obtaining 5.83kg of copper slag, followed by adding 30kg of sawdust, and reacting at 285°C for 1.0h to obtain 8.8kg of iron slag and 1133.32kg of oxygen-refined tin. The oxygen-refined tin was put into a continuous crystallizer to obtain 1110.36kg of tin ingot products.
[0047] Example 2
[0048] A method for treating complex tin sludge and comprehensively recovering multiple valuable metals, specifically comprising the following steps:
[0049] 63.59t of complex tin mud, of which the mass percentage of water is 25.63%. The dry basis composition of the tin mud contains Sn50.81%, Cu 0.45%, Pb 1.59%, Sb 4.46%, Bi 0.30%, In 0.01% and Ag 0.003%, and the rest are impurities. It can be seen that the complex tin mud contains low levels of copper, indium and silver. The complex tin mud is put into a rotary kiln, the roasting temperature is 700-800℃, the negative pressure at the kiln tail is -10--30Pa, and the kiln speed is 0.3-0.4r / min. 46.35t of roasted sand is obtained, with the composition of Sn 51.84%, Cu 0.46%, Pb 1.61%, Sb 4.50%, Bi 0.30%, In 0.003%, Ag0.01%, and the rest are impurities.
[0050] The roasted sand was reduced and smelted in an Ausmelt furnace to produce 16.22 tons of slag and 26.17 tons of crude tin alloy. The composition of the crude tin alloy was Sn 84.47%, Cu 0.81%, Pb 2.87%, Sb 8.06%, Bi 0.54%, In 0.018%, Ag 0.016%, and the rest were impurities.
[0051] The crude tin alloy is put into an oxidation pot, and at a temperature of 260°C, 85kg of sulfur is added according to the weight ratio of sulfur to copper = 1:2.2 for sulfidation and copper removal, and 1.36t of copper slag is fished out, containing 15.60% Cu and 58.30% Sn. After the copper slag is screened, the screened material and iron slag are returned for reduction smelting treatment, and the screened material is returned to the rotary kiln. The roasting temperature is controlled at 700-800°C, the negative pressure at the kiln tail is -10--30Pa, and the kiln speed is 0.5-1.2r / min to obtain copper-containing roasted sand; the copper-containing roasted sand is leached with an initial concentration of 200g / L sulfuric acid at a liquid-solid ratio of 5:1, a temperature of 60°C, and a time of 1.0h to obtain a copper-containing leachate; the leachate is replaced with iron powder at a temperature of 60°C and a time of 3h to obtain a sponge copper product of 0.20t, containing 96.70% Cu.
[0052] After the copper is removed from the crude tin alloy in the oxidation pot, 50kg of sawdust is added and reacted at 270℃ for 1.5h to obtain 1.54t of iron slag and 23.15t of oxygen-refined tin containing 8.11% Sb. The oxygen-refined tin is put into a vacuum furnace and subjected to two-stage vacuum separation under the conditions of vacuum degree 4-10Pa and temperature 1000-1500℃ to obtain 3.20t of lead-antimony-bismuth alloy products, and the vacuum tin is cast to obtain 19.90t of tin ingot products.
[0053] Example 3
[0054] A method for treating complex tin sludge and comprehensively recovering multiple valuable metals, specifically comprising the following steps:
[0055] 32.59t of complex tin mud, of which the mass percentage of water is 21.21%. The dry basis of tin mud contains 31.26% Sn, 0.08% Cu, 31.07% Pb, 0.24% Sb, 0.17% Bi, 0.01% In and 0.03% Ag, and the rest are impurities. It can be seen that the complex tin mud contains low copper and indium, and high silver. The complex tin mud is put into a rotary kiln, the roasting temperature is 300-500℃, the negative pressure at the kiln tail is -30-50Pa, the kiln speed is 1.0-1.5r / min, and 25.16t of roasted sand is obtained. The roasted sand was reduced and smelted in a side-blown furnace to produce 8.81 tons of slag and 16.03 tons of crude tin alloy. The composition of the crude tin alloy was Sn 46.57%, Cu 0.13%, Pb 49.77%, Sb 0.38%, Bi 0.27%, In 0.016%, Ag 0.048%, and the rest were impurities.
[0056] The crude tin alloy was put into the oxidation pot, and 50kg of sawdust was added by oxidation slag removal. After reacting at 280℃ for 0.5h, 0.96t of iron slag and 15.08t of oxygen-refined tin containing 0.048% Ag were separated. The oxygen-refined tin was electrolyzed by silicic acid system solder, and the cell voltage was controlled at 0.22V, the current intensity was 1700A, and the electrolyte temperature was 36℃. Under the conditions, 14.58t of solder ingots meeting the GBT8012-2013 standard and 0.62t of anode mud rich in precious metals were obtained. The anode mud contained 42.65% Sn, 3.51% Cu, 2.50% Pb, 8.50% Sb, 6.92% Bi, 0.016% In, 1.10% Ag, and the rest were impurities.
[0057] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the embodiments can be referred to each other. For the scheme disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part.
[0058] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for treating complex tin sludge and comprehensively recovering multiple valuable metals, characterized in that: The specific steps include: (1) calcining the complex tin mud in a rotary kiln at a calcination temperature of 300 to 900° C., a negative pressure of -10 to -50 Pa at the kiln tail, and a kiln rotation speed of 0.1 to 2.0 r / min to obtain calcined sand; (2) leaching the roasted sand in sulfuric acid to obtain a leaching solution containing copper and indium and a leaching residue enriched with tin, lead, antimony, bismuth and silver; (3) extracting indium from the leaching solution obtained in step (2) with P204 to obtain a raffinate and an indium-containing extract; stripping, neutralizing, and replacing the indium-containing extract to obtain a sponge indium product; (4) the raffinate obtained in step (3) is replaced with iron powder at a temperature of 30 to 60° C. for 0.5 to 6 h to obtain a sponge copper product and a replaced liquid; the replaced liquid is pH adjusted to remove iron and then returned to step (2) and prepared with sulfuric acid for leaching; (5) sending the leached slag obtained in step (2) to one of an electric furnace, an Ausmelt furnace or a side-blown furnace for reduction smelting to obtain a crude tin alloy and slag; the slag is sold as a fuming furnace material; (6) subjecting the crude tin alloy to sulfidation in an oxidation pot to remove copper, and oxidation slag to separate high melting point copper and iron elements to obtain copper slag, iron slag and oxygen-refined tin; after the copper slag is screened, the undersize is returned to the rotary kiln for roasting, and the oversize and iron slag are returned for reduction smelting treatment; (7) feeding the oxygen-refined tin into a continuous crystallizer for separation to obtain a tin ingot product and a crystallizer solder; (8) If the crystallizer solder contains Ag>0.04%, solder ingots and anode mud rich in precious metals are obtained by solder electrolysis; If the crystallizer solder contains Ag < 0.04%, a vacuum furnace is used for separation to obtain vacuum tin and lead-antimony-bismuth-silver alloy products.
2. The method for treating complex tin sludge and comprehensively recovering multiple valuable metals according to claim 1, characterized in that: The mass percentage of water in the complex tin mud is 20-65%; the mass percentage of each component in the dry basis of the tin mud is: Sn 10-80%, Cu 0.1-30%, Pb 0.1-50%, Sb 0.1-10%, Bi 0.1-5.0%, In 0.01-1.0%, Ag 0.001-0.5%, and the rest are impurities.
3. The method for treating complex tin sludge and comprehensively recovering multiple valuable metals according to claim 1, characterized in that: If the tin mud contains less than 2.0% Cu or less than 0.2% In on a dry basis, steps (2) to (4) can be omitted, and the roasted sand from step (1) can be directly sent to step (5) for reduction smelting.
4. The method for treating complex tin sludge and comprehensively recovering multiple valuable metals according to claim 1, characterized in that: The liquid-to-solid ratio of the leaching in step (2) is 3 to 10:1, the initial concentration of sulfuric acid is 10 to 300 g / L, the temperature is 25 to 90° C., and the time is 0.5 to 4 h.
5. The method for treating complex tin sludge and comprehensively recovering multiple valuable metals according to claim 1, characterized in that: The reaction temperature of the extraction in step (3) is 25-60°C, and the oil (O) / (W) ratio is 1 / 5-1 / 2.
6. The method for treating complex tin sludge and comprehensively recovering multiple valuable metals according to claim 1, characterized in that: The sulfidation copper removal in step (6) is controlled at a temperature of 240-280°C, with a sulfur-copper weight ratio of 1:2-3; the covering material added to the oxidized slag is sawdust, with an amount of 1-100 kg / t crude tin alloy, a temperature of 260-320°C, and a reaction time of 1-4 hours.
7. The method for treating complex tin sludge and comprehensively recovering multiple valuable metals according to claim 1, characterized in that: If the oxygen-refined tin in step (6) contains Sb>1.5%, the oxygen-refined tin can omit step (7) and directly enter step (8) for vacuum furnace separation.
8. The method for treating complex tin sludge and comprehensively recovering multiple valuable metals according to claim 1, characterized in that: If the oxygen-refined tin in step (6) contains Ag>0.04%, the oxygen-refined tin can omit step (7) and directly proceed to step (8) for solder electrolysis.
9. The method for treating complex tin sludge and comprehensively recovering multiple valuable metals according to claim 1, characterized in that: The solder electrolysis in step (8) is carried out using silicofluoric acid as the electrolyte, and is produced by controlling the cell voltage to 0.1-0.25V, the current intensity to 1300-2200A, and the electrolyte temperature to 20-40°C.
10. The method for treating complex tin sludge and comprehensively recovering multiple valuable metals according to claim 1, characterized in that: The specific operation of the vacuum separation in step (8) is: performing 2-3 levels of vacuum separation in a vacuum furnace, controlling the vacuum degree to 1-50 Pa and the temperature to 900-1500° C., so that lead, antimony and bismuth are volatilized to form a lead-antimony-bismuth alloy product.