Method for smelting ferro-nickel alloy

A method for smelting nickel-iron alloy through oxidative acid leaching and impurity removal processes efficiently converts nickel-iron alloy into battery-grade iron phosphate and nickel precursors, addressing the inefficiencies of existing energy-intensive conversion methods.

CN119082478AActive Publication Date: 2024-12-06GUANGDONG BRUNP RECYCLING TECH CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411256667.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-12-06
Estimated Expiration
2044-09-09

AI Technical Summary

Technical Problem

The existing process for converting nickel-iron alloy into nickel beans or nickel powder is energy-intensive and results in the burial of iron as waste slag, hindering the effective utilization of both nickel and iron resources.

Method used

A method involving oxidative acid leaching, followed by chromium and phosphorus removal steps, and subsequent impurity removal to produce battery-grade iron phosphate and nickel precursors, utilizing hydrogen peroxide, phosphoric acid, trivalent iron salts, and silicate solutions to achieve deep impurity removal without extraction.

Benefits of technology

The method achieves high comprehensive benefits by converting nickel-iron alloy into valuable products with low processing costs, making iron into battery-grade iron phosphate and nickel into a precursor.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082478A_ABST
    Figure CN119082478A_ABST
Patent Text Reader

Abstract

The invention relates to a method for smelting a nickel-iron alloy, which comprises the following steps: carrying out oxidation acid leaching on the nickel-iron alloy to obtain a leaching solution and leaching residues; removing chromium from the obtained leachate to obtain chromium-removed slag and chromium-removed filtrate; mixing a first oxidizing agent, phosphoric acid and the obtained chromium-removed filtrate to remove iron, so as to obtain iron phosphate and iron-removed liquid; ferric iron salt and the obtained iron removal liquid are mixed for phosphorus removal, and a phosphorus removal solution and iron phosphate slag are obtained; and performing impurity removal on the obtained phosphorus removal solution, and using the obtained impurity removal solution for preparing the ternary precursor. According to the method, extraction is not needed, the treatment cost of the nickel-iron alloy is reduced, iron in the nickel-iron alloy can be made into battery-grade iron phosphate, nickel can be used for preparing a precursor, and comprehensive benefits are high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of valuable metal recovery and relates to a method for alloy smelting, in particular to a method for smelting nickel-iron alloy. Background Art

[0002] As a key material for new energy power batteries, nickel is crucial to the development of new energy vehicles. According to statistics, the global production of mineral nickel will be about 3.6 million tons in 2023. The global nickel resources exceed 350 million tons, of which 54% are laterite nickel ore, 35% are magmatic sulfide ore, 10% are massive sulfide ore and 1% are tailings.

[0003] Nickel-iron alloy is an intermediate product in the smelting process of nickel sulfide ore. Since the iron content in nickel-iron alloy is high and the value of iron is low, nickel-iron alloy needs to be further smelted to enrich the nickel content in nickel-iron alloy into nickel beans or nickel powder with a nickel content of more than 90%. However, the process of converting nickel-iron alloy into nickel beans or nickel powder requires very high energy consumption, and the iron therein will also be buried as waste slag, which is not conducive to the effective utilization of the iron in nickel-iron alloy. As the demand for lithium iron phosphate batteries increases, the demand for iron resources is also gradually increasing. Therefore, it is necessary to develop a resource utilization method for nickel-iron alloy to realize the comprehensive utilization of nickel resources and iron resources in nickel-iron alloy. Summary of the invention

[0004] The object of the present invention is to provide a method for smelting nickel-iron alloy, which can achieve the purpose of deep impurity removal without extraction, and can not only make the iron in the nickel-iron alloy into battery-grade iron phosphate, but also make the nickel into a precursor, with high comprehensive benefits.

[0005] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0006] The present invention provides a method for smelting nickel-iron alloy, which comprises the following steps:

[0007] (1) the nickel-iron alloy is subjected to oxidative acid leaching to obtain a leaching solution and a leaching residue;

[0008] (2) removing chromium from the leaching solution obtained in step (1) to obtain chromium-removed slag and chromium-removed filtrate;

[0009] (3) mixing the first oxidant, phosphoric acid and the chromium removal filtrate obtained in step (2) to remove iron, thereby obtaining iron phosphate and an iron removal liquid;

[0010] (4) mixing the trivalent iron salt with the iron removal solution obtained in step (3) to remove phosphorus, thereby obtaining a phosphorus removal solution and iron phosphate slag;

[0011] (5) The dephosphorization solution obtained in step (4) is subjected to impurity removal, and the obtained impurity-removed solution is used to prepare a precursor.

[0012] The method provided by the present invention can achieve the purpose of deep impurity removal without extraction operation, has low processing cost, can make the iron in the nickel-iron alloy into battery-grade iron phosphate, and the nickel can be made into a precursor, so the overall benefit is high.

[0013] Preferably, the oxidative acid leaching in step (1) comprises: first mixing the nickel-iron alloy with an acid for acid leaching, and then adding hydrogen peroxide to a pH value of 1 to 2, for example, 1, 1.2, 1.5, 1.8 or 2, but not limited to the listed values, and other values ​​not listed in the numerical range are also applicable, preferably 1.5 to 2.

[0014] Preferably, the concentration of hydrogen peroxide used in the oxidative acid leaching process is 27.5wt% to 50wt%, for example, it can be 27.5wt%, 30wt%, 35wt%, 40wt%, 45wt% or 50wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0015] Preferably, the acid comprises any one of sulfuric acid, hydrochloric acid or nitric acid or a combination of at least two thereof, typical but non-limiting combinations include a combination of sulfuric acid and hydrochloric acid, a combination of hydrochloric acid and nitric acid, a combination of sulfuric acid and nitric acid, or a combination of sulfuric acid, hydrochloric acid and nitric acid, preferably sulfuric acid.

[0016] The concentration of sulfuric acid in the present invention is above 70wt%, for example, it can be 70wt%, 75wt%, 80wt%, 85wt%, 90wt%, 95wt% or 98wt%, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0017] Preferably, the amount of the acid is 0.8 times or more of the theoretical amount, for example, 0.8 times, 0.85 times, 0.9 times, 0.95 times or 1 times, but is not limited to the listed values, and the remaining values ​​not listed in the numerical range are also applicable. If less acid is used in the oxidative acid leaching process, the Ni and Fe contents in the leachate will be low, affecting the subsequent product quality.

[0018] Preferably, the acid leaching temperature is 70°C to 90°C, for example, 70°C, 75°C, 80°C, 85°C or 90°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable, preferably 80°C to 90°C.

[0019] Preferably, the acid leaching time is 2.5 h to 5 h, for example, it can be 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h or 5 h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable, preferably 2.5 h to 4 h.

[0020] Preferably, the chromium removal in step (2) comprises: firstly mixing the second oxidant with the leaching solution obtained in step (1), and then adding phosphate to carry out chromium removal reaction, and performing solid-liquid separation after standing to obtain chromium removal slag and chromium removal filtrate.

[0021] The method provided by the invention aims at the characteristic that chromium in the acid leaching solution is difficult to remove. Phosphate is ionized into phosphate ions and hydroxide ions in the solution, and the conditions of the chromium removal reaction are controlled so that the phosphate ions, the hydroxide ions and the iron ions in the acid leaching solution are combined into amorphous iron phosphate and iron hydroxide. The amorphous iron phosphate can induce the generation of chromium phosphate, and the iron hydroxide can adsorb a part of the chromium ions. The purpose of deep chromium removal is achieved by combining the induction and adsorption method.

[0022] Exemplarily, the phosphate is configured into a solution with a concentration of 10wt% to 30wt% and then added, for example, it can be 10wt%, 15wt%, 20wt%, 25wt% or 30wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0023] Preferably, the second oxidant comprises any one of hydrogen peroxide, sodium persulfate or manganese dioxide or a combination of at least two thereof, and typical but non-limiting combinations include a combination of hydrogen peroxide and sodium persulfate, a combination of sodium persulfate and manganese dioxide, a combination of hydrogen peroxide and manganese dioxide, or a combination of hydrogen peroxide, sodium persulfate and manganese dioxide.

[0024] Preferably, the amount of the second oxidant added is such that the content of trivalent iron ions in the system is 0.5 g / L to 2 g / L, for example, 0.5 g / L, 1 g / L, 1.5 g / L or 2 g / L, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0025] Preferably, the phosphate comprises trisodium phosphate (Na 3 PO 4 ), sodium dihydrogen phosphate (NaH 2 PO 4 ) or sodium monohydrogen phosphate (Na 2 HPO 4 ), typical but non-limiting combinations include a combination of trisodium phosphate and sodium dihydrogen phosphate, a combination of sodium dihydrogen phosphate and sodium monohydrogen phosphate, a combination of trisodium phosphate and sodium monohydrogen phosphate, or a combination of trisodium phosphate, sodium dihydrogen phosphate and sodium monohydrogen phosphate.

[0026] Preferably, the amount of phosphate added is 1.1 to 3 times the theoretical amount of chromium reaction in the system, for example, it can be 1.1 times, 1.5 times, 2 times, 2.5 times or 3 times, but is not limited to the listed values. Other values ​​not listed in the numerical range are also applicable, preferably 1.8 to 2.5 times.

[0027] Preferably, the temperature of the chromium removal reaction is 25°C to 50°C, for example, 25°C, 30°C, 35°C, 40°C, 45°C or 50°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable, preferably 40°C to 50°C.

[0028] Preferably, the pH value of the chromium removal reaction is 3 to 5, for example, 3, 3.5, 4, 4.5 or 5, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable, preferably 3.5 to 4.

[0029] Exemplarily, the pH value of the chromium removal reaction of the present invention is adjusted by adding nickel hydroxide and / or nickel carbonate.

[0030] Preferably, the chromium removal reaction time is 1 h to 3 h, for example, 1 h, 1.5 h, 2 h, 2.5 h or 3 h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable, preferably 1.5 h to 2 h.

[0031] Preferably, the standing time is 5 h to 12 h, for example, 5 h, 6 h, 8 h, 10 h or 12 h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable, preferably 6 h to 10 h.

[0032] Preferably, in step (3), the first oxidant comprises any one of hydrogen peroxide, oxygen, ozone or sodium persulfate, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of hydrogen peroxide and oxygen, a combination of oxygen and ozone, a combination of ozone and sodium persulfate, a combination of hydrogen peroxide, oxygen and ozone, a combination of oxygen, ozone and sodium persulfate, or a combination of hydrogen peroxide, ozone, oxygen and sodium persulfate, preferably hydrogen peroxide.

[0033] Preferably, the concentration of the first oxidant is 27.5wt% to 50wt%, for example, 27.5wt%, 30wt%, 35wt%, 40wt%, 45wt% or 50wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0034] Preferably, the amount of the first oxidant added is 1 to 1.5 times the theoretical amount of ferrous ions in the system, for example, 1, 1.2, 1.3, 1.4 or 1.5 times, but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable, preferably 1.2 to 1.5 times.

[0035] Preferably, the amount of phosphoric acid added is 1 to 1.2 times the theoretical amount of iron reaction in the system, for example, it can be 1, 1.1 or 1.2 times, but is not limited to the listed values. Other values ​​not listed in the numerical range are also applicable, preferably 1.1 to 1.2 times.

[0036] Preferably, the iron removal in step (3) is carried out at a pH value of 1 to 2, for example, 1, 1.2, 1.5, 1.8 or 2, but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable, preferably 1.5 to 2.

[0037] Exemplarily, the pH value of the iron removal in step (3) of the present invention is adjusted using a sodium hydroxide solution with a concentration of 20wt% to 50wt%, for example, it can be 20wt%, 25wt%, 30wt%, 35wt%, 40wt%, 45wt% or 50wt%, but is not limited to the listed values, and the remaining unlisted values ​​within the numerical range are also applicable.

[0038] Preferably, the temperature for iron removal in step (3) is 80°C to 95°C, for example, 80°C, 82°C, 85°C, 90°C or 95°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0039] Preferably, the trivalent iron salt in step (4) comprises ferric sulfate.

[0040] Preferably, the amount of the trivalent iron salt added in step (4) is 1 to 2 times the theoretical amount used for the reaction with phosphorus, for example, it can be 1 time, 1.2 times, 1.5 times, 1.8 times or 2 times, but is not limited to the listed values, and the remaining values ​​not listed in the numerical range are also applicable.

[0041] Preferably, the impurity removal in step (5) comprises: first concentrating the dephosphorization solution, then mixing it with silicate and alkali solution, letting it stand after the reaction, and separating the solid from the liquid to obtain impurity removal residue and impurity removal liquid.

[0042] The phosphorus removal solution contains silicon, zinc and iron. By adding silicate as an inducer, the silicate is ionized into silicic acid and hydroxide ions in the solution. Silicic acid can induce the silicate and ions in the solution to become silicic acid, and the hydroxide ions combine with iron and nickel to form iron hydroxide and nickel hydroxide; iron hydroxide and nickel hydroxide can adsorb silicon, and the purpose of deep silicon removal is achieved by combining induction and adsorption.

[0043] Preferably, the concentration is concentrated to a Ni concentration in the solution of 100 g / L to 120 g / L, for example, 100 g / L, 105 g / L, 110 g / L, 115 g / L or 120 g / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable, preferably 110 g / L to 120 g / L.

[0044] Preferably, the added amount of the silicate is 0.1 g / L to 1.5 g / L, for example, it can be 0.1 g / L, 0.3 g / L, 0.5 g / L, 0.8 g / L, 1 g / L or 1.5 g / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0045] Preferably, the amount of the alkali solution added is sufficient to react with the nickel in the system to generate 3 g / L to 10 g / L of nickel hydroxide, for example, 3 g / L, 5 g / L, 6 g / L, 8 g / L or 10 g / L, but not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable, preferably 5 g / L to 8 g / L.

[0046] Exemplarily, the alkali solution includes a sodium hydroxide solution with a concentration of 20wt% to 32wt%, for example, it can be 20wt%, 24wt%, 25wt%, 28wt%, 30wt% or 32wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0047] Preferably, the reaction temperature is 50°C to 80°C, for example, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C or 80°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0048] Preferably, the reaction time is 1 h to 3 h, for example, 1 h, 1.5 h, 2 h, 2.5 h or 3 h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable, preferably 1 h to 2 h.

[0049] Preferably, the standing time is 12 h to 24 h, for example, 12 h, 15 h, 16 h, 18 h, 20 h or 24 h, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0050] As a preferred technical solution of the method for smelting nickel-iron alloy provided by the present invention, the method comprises the following steps:

[0051] (1) mixing the nickel-iron alloy with sulfuric acid, acid leaching at 70° C. to 90° C. for 2.5 h to 5 h, then adding hydrogen peroxide until the pH value is 1 to 2, and performing solid-liquid separation to obtain a leachate and a leach residue;

[0052] The amount of sulfuric acid used is more than 0.8 times the theoretical amount used for acid leaching;

[0053] (2) firstly mixing the second oxidant with the leaching solution obtained in step (1), and then adding phosphate, performing a chromium removal reaction at 25° C. to 50° C. and a pH value of 3 to 5 for 1 h to 3 h, standing for 5 h to 12 h, and then performing solid-liquid separation to obtain a chromium removal slag and a chromium removal filtrate;

[0054] The second oxidant includes any one of hydrogen peroxide, sodium persulfate or manganese dioxide or a combination of at least two thereof, and the amount of the second oxidant added is such that the content of trivalent iron ions in the system is 0.5 g / L to 2 g / L;

[0055] The phosphate includes any one of trisodium phosphate, sodium dihydrogen phosphate or sodium monohydrogen phosphate, or a combination of at least two thereof, and the amount of the phosphate added is 1.1 to 3 times the theoretical amount of chromium reaction in the system;

[0056] (3) mixing the first oxidant, phosphoric acid and the chromium removal filtrate obtained in step (2), adjusting the pH value to 1 to 2 using 20 wt % to 50 wt % of sodium hydroxide, and removing iron at 80° C. to 95° C. to obtain iron phosphate and an iron removal liquid;

[0057] The amount of the first oxidant added is 1 to 1.5 times the theoretical amount of the ferrous ions in the system; the amount of the phosphoric acid added is 1 to 1.2 times the theoretical amount of the iron in the system;

[0058] (4) mixing the trivalent iron salt with the iron removal solution obtained in step (3) to remove phosphorus, thereby obtaining a phosphorus removal solution and iron phosphate slag;

[0059] The amount of the trivalent iron salt added is 1 to 2 times the theoretical amount used for the reaction with phosphorus;

[0060] (5) The dephosphorization solution is first concentrated to a Ni concentration of 100 g / L to 120 g / L, then mixed with silicate and alkali solution, reacted at 50° C. to 80° C. for 1 h to 3 h, allowed to stand for 12 h to 24 h, and solid-liquid separated to obtain dephosphorization slag and dephosphorization liquid; the dephosphorization liquid obtained is used to prepare a precursor;

[0061] The silicate is added in an amount of 0.1 g / L to 1.5 g / L; the alkali solution is added in an amount sufficient to react with nickel in the system to generate 3 g / L to 10 g / L of nickel hydroxide.

[0062] Compared with the prior art, the present invention has the following beneficial effects:

[0063] The method provided by the present invention can achieve the purpose of deep impurity removal without extraction operation, has low processing cost, can make the iron in the nickel-iron alloy into battery-grade iron phosphate, and the nickel can be made into a precursor, so the overall benefit is high. BRIEF DESCRIPTION OF THE DRAWINGS

[0064] Figure 1 A process flow chart of the method is provided for Example 1. DETAILED DESCRIPTION

[0065] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only used to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0066] Example 1

[0067] The present embodiment provides a method for smelting nickel-iron alloy. In terms of mass percentage, the main components in the nickel-iron alloy include 25.6wt% Ni, 0.25wt% Co, 0.12wt% Mn, 72.5wt% Fe, 0.09wt% Cr, 0.23wt% Si, 0.012wt% Zn, 0.002wt% Ca and 0.001wt% Mg. The process flow chart of the method is as follows: Figure 1 As shown, the following steps are included:

[0068] (1) a nickel-iron alloy having an average particle size of 5 mm was mixed with water at a solid-liquid ratio (g / mL) of 1:5 for slurrying, and after stirring, mixed with sulfuric acid having a concentration of 98 wt%, acid-leached at 80° C. for 4 h, and then hydrogen peroxide having a concentration of 27.5 wt% was added to a pH value of 1.5, and solid-liquid separation was performed to obtain a leachate and a leach residue;

[0069] The amount of sulfuric acid used is 0.8 times the theoretical amount of acid leaching;

[0070] (2) firstly mixing the second oxidant with the leaching solution obtained in step (1) for 0.5 h, then adding trisodium phosphate, carrying out chromium removal reaction at 40° C. and pH 3.5 (adjusted by nickel hydroxide) for 2 h, standing for 6 h, and then carrying out solid-liquid separation to obtain chromium removal slag and chromium removal filtrate;

[0071] The second oxidant is 27.5 wt% hydrogen peroxide, and the amount of the second oxidant added is such that the content of trivalent iron ions in the system is 0.5 g / L;

[0072] Trisodium phosphate is added in the form of a 20 wt% solution, the amount added being 1.8 times the theoretical amount of chromium reaction in the system;

[0073] (3) mixing the first oxidant, phosphoric acid and the chromium removal filtrate obtained in step (2), controlling the pH value to 2 using 32 wt % sodium hydroxide, and removing iron at 95° C. for 4 h to obtain iron phosphate and an iron removal liquid;

[0074] The first oxidant is 27.5wt% hydrogen peroxide, and the amount of the first oxidant added is 1.2 times the theoretical amount of the reaction with the ferrous ions in the system; the amount of the phosphoric acid added is 1.1 times the theoretical amount of the reaction with the iron in the system;

[0075] (4) mixing ferric sulfate with the iron removal solution obtained in step (3) to remove phosphorus, thereby obtaining a phosphorus removal solution and iron phosphate slag;

[0076] The amount of ferric sulfate added is 1.2 times the theoretical amount required for reaction with phosphorus;

[0077] (5) The dephosphorization solution is first concentrated to a Ni concentration of 120 g / L in the concentrated solution, and then stirred and mixed with sodium silicate and a 32 wt% sodium hydroxide solution, reacted at 70° C. for 1 h, and allowed to stand for 12 h, and solid-liquid separation was performed to obtain a dephosphorization slag and a dephosphorization liquid;

[0078] The amount of sodium silicate added is 0.2 g / L; the amount of sodium hydroxide solution added is sufficient to react with nickel in the system to generate 5 g / L of nickel hydroxide;

[0079] Cobalt sulfate and manganese sulfate are added to the obtained impurity removal liquid for batching, and a ternary precursor is obtained through a coprecipitation reaction.

[0080] In this embodiment, the compositions of the leaching solution, the chromium removal filtrate, the concentrated solution and the impurity removal solution are shown in Table 1.

[0081] Table 1

[0082]

[0083] Example 2

[0084] The present embodiment provides a method for smelting a nickel-iron alloy. In terms of mass percentage, the main components of the nickel-iron alloy include 32.1wt% Ni, 0.32wt% Co, 0.15wt% Mn, 65.6wt% Fe, 0.07wt% Cr, 0.18wt% Si, 0.02wt% Zn, 0.002wt% Ca and 0.001wt% Mg. The method comprises the following steps:

[0085] (1) a nickel-iron alloy having an average particle size of 5 mm was mixed with water at a solid-liquid ratio (g / mL) of 1:2 for slurrying, and after stirring, mixed with sulfuric acid having a concentration of 98 wt%, acid-leached at 85° C. for 3 h, and then hydrogen peroxide having a concentration of 27.5 wt% was added until the pH value was 2, and solid-liquid separation was performed to obtain a leachate and a leach residue;

[0086] The amount of sulfuric acid used is 0.9 times the theoretical amount of acid leaching;

[0087] (2) firstly mixing the second oxidant with the leaching solution obtained in step (1) for 0.5 h, then adding sodium dihydrogen phosphate, carrying out chromium removal reaction at 50° C. and pH 4 (adjusted by nickel hydroxide) for 1.5 h, standing for 10 h, and then carrying out solid-liquid separation to obtain chromium removal slag and chromium removal filtrate;

[0088] The second oxidant is 27.5 wt% hydrogen peroxide, and the amount of the second oxidant added is such that the content of trivalent iron ions in the system is 1 g / L;

[0089] Sodium dihydrogen phosphate is added in the form of a 20 wt% solution, the amount added being 2.5 times the theoretical amount of chromium reaction in the system;

[0090] (3) mixing the first oxidant, phosphoric acid and the chromium removal filtrate obtained in step (2), controlling the pH value to 1.5 using 32 wt % sodium hydroxide, and removing iron at 95° C. for 3 h to obtain iron phosphate and an iron removal liquid;

[0091] The first oxidant is 27.5wt% hydrogen peroxide, and the amount of the first oxidant added is 1.5 times the theoretical amount of the reaction with the ferrous ions in the system; the amount of the phosphoric acid added is 1.2 times the theoretical amount of the reaction with the iron in the system;

[0092] (4) mixing ferric sulfate with the iron removal solution obtained in step (3) to remove phosphorus, thereby obtaining a phosphorus removal solution and iron phosphate slag;

[0093] The amount of ferric sulfate added is 1.1 times the theoretical amount for reaction with phosphorus;

[0094] (5) The dephosphorization solution is first concentrated to a Ni concentration of 110 g / L in the concentrated solution, and then stirred and mixed with sodium silicate and a 32 wt% sodium hydroxide solution, reacted at 70° C. for 2 h, and allowed to stand for 24 h, followed by solid-liquid separation to obtain a dephosphorization slag and a dephosphorization liquid;

[0095] The amount of sodium silicate added is 1 g / L; the amount of sodium hydroxide solution added is sufficient to react with nickel in the system to generate 8 g / L of nickel hydroxide;

[0096] Cobalt sulfate and manganese sulfate are added to the obtained impurity removal liquid for batching, and a ternary precursor is obtained through a coprecipitation reaction.

[0097] In this embodiment, the compositions of the leaching solution, the chromium removal filtrate, the concentrated solution and the impurity removal solution are shown in Table 2.

[0098] Table 2

[0099]

[0100] Example 3

[0101] The present embodiment provides a method for smelting a nickel-iron alloy. In terms of mass percentage, the main components of the nickel-iron alloy include 30.1wt% Ni, 0.45wt% Co, 0.21wt% Mn, 68.3wt% Fe, 0.06wt% Cr, 0.27wt% Si, 0.018wt% Zn, 0.002wt% Ca and 0.001wt% Mg. The method comprises the following steps:

[0102] (1) a nickel-iron alloy having an average particle size of 5 mm was mixed with water at a solid-liquid ratio (g / mL) of 1:3 for slurrying, and after stirring, mixed with sulfuric acid having a concentration of 98 wt%, acid-leached at 90° C. for 2.5 h, and then hydrogen peroxide having a concentration of 27.5 wt% was added to a pH value of 2, and solid-liquid separation was performed to obtain a leachate and a leach residue;

[0103] The amount of sulfuric acid used is 0.8 times the theoretical amount of acid leaching;

[0104] (2) firstly mixing the second oxidant with the leaching solution obtained in step (1) for 1 hour, then adding trisodium phosphate, carrying out chromium removal reaction at 45° C. and pH 4 (adjusted by nickel carbonate) for 2 hours, standing for 10 hours, and then carrying out solid-liquid separation to obtain chromium removal slag and chromium removal filtrate;

[0105] The second oxidant is manganese dioxide, and the amount of the second oxidant added is such that the content of trivalent iron ions in the system is 2 g / L;

[0106] Trisodium phosphate is added in the form of a 20 wt% solution, the amount added being twice the theoretical amount of chromium reaction in the system;

[0107] (3) mixing the first oxidant, phosphoric acid and the chromium removal filtrate obtained in step (2), controlling the pH value to 2 using 32 wt % sodium hydroxide, and removing iron at 90° C. for 5 h to obtain iron phosphate and an iron removal liquid;

[0108] The first oxidant is 27.5wt% hydrogen peroxide, and the amount of the first oxidant added is 1.5 times the theoretical amount of the reaction with the ferrous ions in the system; the amount of the phosphoric acid added is 1.1 times the theoretical amount of the reaction with the iron in the system;

[0109] (4) mixing ferric sulfate with the iron removal solution obtained in step (3) to remove phosphorus, thereby obtaining a phosphorus removal solution and iron phosphate slag;

[0110] The amount of ferric sulfate added is 1.1 times the theoretical amount for reaction with phosphorus;

[0111] (5) The dephosphorization solution is first concentrated to a Ni concentration of 115 g / L in the concentrated solution, and then stirred and mixed with sodium silicate and a 32 wt% sodium hydroxide solution, reacted at 70° C. for 2 h, and allowed to stand for 16 h, followed by solid-liquid separation to obtain a dephosphorization slag and a dephosphorization liquid;

[0112] The amount of sodium silicate added is 1.5 g / L; the amount of sodium hydroxide solution added is sufficient to react with nickel in the system to generate 6 g / L of nickel hydroxide;

[0113] Cobalt sulfate and manganese sulfate are added to the obtained impurity removal liquid for batching, and a ternary precursor is obtained through a coprecipitation reaction.

[0114] In this embodiment, the compositions of the leaching solution, the chromium removal filtrate, the concentrated solution and the impurity removal solution are shown in Table 3.

[0115] Table 3

[0116]

[0117]

[0118] Example 4

[0119] The present embodiment provides a method for smelting a nickel-iron alloy. In terms of mass percentage, the main components in the nickel-iron alloy include 25.6wt% Ni, 0.25wt% Co, 0.12wt% Mn, 72.5wt% Fe, 0.09wt% Cr, 0.23wt% Si, 0.012wt% Zn, 0.002wt% Ca and 0.001wt% Mg. The method comprises the following steps:

[0120] (1) a nickel-iron alloy having an average particle size of 5 mm was mixed with water at a solid-liquid ratio (g / mL) of 1:5 for slurrying, and after stirring, mixed with sulfuric acid having a concentration of 98 wt%, acid-leached at 70° C. for 5 h, and then added with hydrogen peroxide having a concentration of 27.5 wt% until the pH value was 1, and solid-liquid separation was performed to obtain a leachate and a leach residue;

[0121] The amount of sulfuric acid used is 0.8 times the theoretical amount of acid leaching;

[0122] (2) firstly mixing the second oxidant with the leaching solution obtained in step (1) for 0.5 h, then adding trisodium phosphate, carrying out chromium removal reaction at 25° C. and pH 5 (adjusted by nickel hydroxide) for 1 h, standing for 5 h, and then carrying out solid-liquid separation to obtain chromium removal slag and chromium removal filtrate;

[0123] The second oxidant is 27.5 wt% hydrogen peroxide, and the amount of the second oxidant added is such that the content of trivalent iron ions in the system is 0.5 g / L;

[0124] Trisodium phosphate was added in the form of a 20 wt% solution, the amount of which was 1.1 times the theoretical amount of chromium reaction in the system;

[0125] (3) mixing the first oxidant, phosphoric acid and the chromium removal filtrate obtained in step (2), controlling the pH value to 2 using 32 wt % sodium hydroxide, and removing iron at 80° C. for 4 h to obtain iron phosphate and an iron removal liquid;

[0126] The first oxidant is 27.5wt% hydrogen peroxide, and the amount of the first oxidant added is 1 times the theoretical amount of the reaction with the ferrous ions in the system; the amount of the phosphoric acid added is 1 times the theoretical amount of the reaction with the iron in the system;

[0127] (4) mixing ferric sulfate with the iron removal solution obtained in step (3) to remove phosphorus, thereby obtaining a phosphorus removal solution and iron phosphate slag;

[0128] The amount of ferric sulfate added is 1.2 times the theoretical amount required for reaction with phosphorus;

[0129] (5) The dephosphorization solution is first concentrated to a Ni concentration of 100 g / L in the concentrated solution, and then stirred and mixed with sodium silicate and a 32 wt% sodium hydroxide solution, reacted at 50° C. for 3 h, and allowed to stand for 12 h. The dephosphorization solution is then solid-liquid separated to obtain a dephosphorization slag and a dephosphorization liquid;

[0130] The amount of sodium silicate added is 0.1 g / L; the amount of sodium hydroxide solution added is sufficient to react with nickel in the system to generate 3 g / L of nickel hydroxide;

[0131] Cobalt sulfate and manganese sulfate are added to the obtained impurity removal liquid for batching, and a ternary precursor is obtained through a coprecipitation reaction.

[0132] In this embodiment, the compositions of the leaching solution, the chromium removal filtrate, the concentrated solution and the impurity removal solution are shown in Table 4.

[0133] Table 4

[0134]

[0135] Example 5

[0136] The present embodiment provides a method for smelting a nickel-iron alloy. In terms of mass percentage, the main components in the nickel-iron alloy include 25.6wt% Ni, 0.25wt% Co, 0.12wt% Mn, 72.5wt% Fe, 0.09wt% Cr, 0.23wt% Si, 0.012wt% Zn, 0.002wt% Ca and 0.001wt% Mg. The method comprises the following steps:

[0137] (1) a nickel-iron alloy having an average particle size of 5 mm was mixed with water at a solid-liquid ratio (g / mL) of 1:5 for slurrying, and after stirring, mixed with sulfuric acid having a concentration of 98 wt%, acid-leached at 80° C. for 4 h, and then hydrogen peroxide having a concentration of 27.5 wt% was added to a pH value of 1.5, and solid-liquid separation was performed to obtain a leachate and a leach residue;

[0138] The amount of sulfuric acid used is 0.8 times the theoretical amount of acid leaching;

[0139] (2) firstly mixing the second oxidant with the leaching solution obtained in step (1) for 0.5 h, then adding trisodium phosphate, carrying out chromium removal reaction at 40° C. and pH 3 (adjusted by nickel hydroxide) for 3 h, standing for 12 h, and then carrying out solid-liquid separation to obtain chromium removal slag and chromium removal filtrate;

[0140] The second oxidant is 27.5 wt% hydrogen peroxide, and the amount of the second oxidant added is such that the content of trivalent iron ions in the system is 0.5 g / L;

[0141] Trisodium phosphate is added in the form of a 20 wt% solution, the amount added being three times the theoretical amount of chromium reaction in the system;

[0142] (3) mixing the first oxidant, phosphoric acid and the chromium removal filtrate obtained in step (2), controlling the pH value to 2 using 32 wt % sodium hydroxide, and removing iron at 95° C. for 4 h to obtain iron phosphate and an iron removal liquid;

[0143] The first oxidant is 27.5wt% hydrogen peroxide, and the amount of the first oxidant added is 1.2 times the theoretical amount of the reaction with the ferrous ions in the system; the amount of the phosphoric acid added is 1.1 times the theoretical amount of the reaction with the iron in the system;

[0144] (4) mixing ferric sulfate with the iron removal solution obtained in step (3) to remove phosphorus, thereby obtaining a phosphorus removal solution and iron phosphate slag;

[0145] The amount of ferric sulfate added is 1.2 times the theoretical amount required for reaction with phosphorus;

[0146] (5) The dephosphorization solution is first concentrated to a Ni concentration of 120 g / L in the concentrated solution, and then stirred and mixed with sodium silicate and a 32 wt% sodium hydroxide solution, reacted at 80° C. for 1 h, and allowed to stand for 12 h, and solid-liquid separation was performed to obtain a dephosphorization slag and a dephosphorization liquid;

[0147] The amount of sodium silicate added is 0.2 g / L; the amount of sodium hydroxide solution added is sufficient to react with nickel in the system to generate 10 g / L of nickel hydroxide;

[0148] Cobalt sulfate and manganese sulfate are added to the obtained impurity removal liquid for batching, and a ternary precursor is obtained through a coprecipitation reaction.

[0149] In this embodiment, the compositions of the leaching solution, the chromium removal filtrate, the concentrated solution and the impurity removal solution are shown in Table 5.

[0150] Table 5

[0151]

[0152] Example 6

[0153] The present embodiment provides a method for smelting a nickel-iron alloy. In terms of mass percentage, the main components in the nickel-iron alloy include 25.6wt% Ni, 0.25wt% Co, 0.12wt% Mn, 72.5wt% Fe, 0.09wt% Cr, 0.23wt% Si, 0.012wt% Zn, 0.002wt% Ca and 0.001wt% Mg. The method comprises the following steps:

[0154] (1) a nickel-iron alloy having an average particle size of 5 mm was mixed with water at a solid-liquid ratio (g / mL) of 1:5 for slurrying, and after stirring, mixed with sulfuric acid having a concentration of 98 wt%, acid-leached at 80° C. for 4 h, and then hydrogen peroxide having a concentration of 27.5 wt% was added to a pH value of 1.5, and solid-liquid separation was performed to obtain a leachate and a leach residue;

[0155] The amount of sulfuric acid used is 0.8 times the theoretical amount of acid leaching;

[0156] (2) mixing the leaching solution obtained in step (1) with trisodium phosphate, performing a chromium removal reaction at 40° C. for 2 h, standing for 6 h, and then performing solid-liquid separation to obtain a chromium removal slag and a chromium removal filtrate;

[0157] During the chromium removal reaction, a sodium hydroxide solution with a concentration of 32 wt% was introduced to maintain a pH value of 5;

[0158] Trisodium phosphate is added in the form of a 20 wt% solution, the amount added being 1.8 times the theoretical amount of chromium reaction in the system;

[0159] (3) mixing the first oxidant, phosphoric acid and the chromium removal filtrate obtained in step (2), controlling the pH value to 2 using 32 wt % sodium hydroxide, and removing iron at 95° C. for 4 h to obtain iron phosphate and an iron removal liquid;

[0160] The first oxidant is 27.5wt% hydrogen peroxide, and the amount of the first oxidant added is 1.2 times the theoretical amount of the reaction with the ferrous ions in the system; the amount of the phosphoric acid added is 1.1 times the theoretical amount of the reaction with the iron in the system;

[0161] (4) mixing ferric sulfate with the iron removal solution obtained in step (3) to remove phosphorus, thereby obtaining a phosphorus removal solution and iron phosphate slag;

[0162] The amount of ferric sulfate added is 1.2 times the theoretical amount required for reaction with phosphorus;

[0163] (5) The dephosphorization solution is first concentrated to a Ni concentration of 120 g / L in the concentrated solution, and then stirred and mixed with a 32 wt% sodium hydroxide solution, reacted at 70° C. for 1 h, and allowed to stand for 12 h, and solid-liquid separation was performed to obtain a dephosphorization slag and a dephosphorization liquid;

[0164] The amount of sodium hydroxide solution added is sufficient to react with nickel in the system to generate 5 g / L of nickel hydroxide.

[0165] In this embodiment, the compositions of the leaching solution, the chromium removal filtrate, the concentrated solution and the impurity removal solution are shown in Table 6.

[0166] Table 6

[0167]

[0168]

[0169] Example 7

[0170] The present embodiment provides a method for smelting a nickel-iron alloy. In terms of mass percentage, the main components in the nickel-iron alloy include 25.6wt% Ni, 0.25wt% Co, 0.12wt% Mn, 72.5wt% Fe, 0.09wt% Cr, 0.23wt% Si, 0.012wt% Zn, 0.002wt% Ca and 0.001wt% Mg. The method comprises the following steps:

[0171] (1) a nickel-iron alloy having an average particle size of 5 mm was mixed with water at a solid-liquid ratio (g / mL) of 1:5 for slurrying, and after stirring, mixed with sulfuric acid having a concentration of 98 wt%, acid-leached at 80° C. for 4 h, and then hydrogen peroxide having a concentration of 27.5 wt% was added to a pH value of 1.5, and solid-liquid separation was performed to obtain a leachate and a leach residue;

[0172] The amount of sulfuric acid used is 0.8 times the theoretical amount of acid leaching;

[0173] (2) mixing the leaching solution obtained in step (1) with sodium carbonate, performing a chromium removal reaction at 40° C. for 2 h, standing for 6 h, and then performing solid-liquid separation to obtain a chromium removal slag and a chromium removal filtrate;

[0174] During the chromium removal reaction, a sodium hydroxide solution with a concentration of 32 wt% was introduced to maintain a pH value of 5;

[0175] Sodium carbonate was added in the form of a 15 wt% solution, the amount of which was 1.8 times the theoretical amount of chromium reaction in the system;

[0176] (3) mixing the first oxidant, phosphoric acid and the chromium removal filtrate obtained in step (2), controlling the pH value to 2 using 32 wt % sodium hydroxide, and removing iron at 95° C. for 4 h to obtain iron phosphate and an iron removal liquid;

[0177] The first oxidant is 27.5wt% hydrogen peroxide, and the amount of the first oxidant added is 1.2 times the theoretical amount of the reaction with the ferrous ions in the system; the amount of the phosphoric acid added is 1.1 times the theoretical amount of the reaction with the iron in the system;

[0178] (4) mixing ferric sulfate with the iron removal solution obtained in step (3) to remove phosphorus, thereby obtaining a phosphorus removal solution and iron phosphate slag;

[0179] The amount of ferric sulfate added is 1.2 times the theoretical amount required for reaction with phosphorus;

[0180] (5) The dephosphorization solution was first concentrated to a Ni concentration of 120 g / L in the concentrated solution. After stirring, nickel hydroxide was added (nickel hydroxide was added at a concentration of 5 g / L). The solution was reacted at 70° C. for 1 h, allowed to stand for 12 h, and solid-liquid separation was performed to obtain dephosphorization slag and dephosphorization liquid.

[0181] In this embodiment, the compositions of the leaching solution, the chromium removal filtrate, the concentrated solution and the impurity removal solution are shown in Table 7.

[0182] Table 7

[0183]

[0184] Example 8

[0185] The present embodiment provides a method for smelting a nickel-iron alloy. In terms of mass percentage, the main components in the nickel-iron alloy include 25.6wt% Ni, 0.25wt% Co, 0.12wt% Mn, 72.5wt% Fe, 0.09wt% Cr, 0.23wt% Si, 0.012wt% Zn, 0.002wt% Ca and 0.001wt% Mg. The method comprises the following steps:

[0186] (1) a nickel-iron alloy having an average particle size of 5 mm was mixed with water at a solid-liquid ratio (g / mL) of 1:5 for slurrying, and after stirring, mixed with sulfuric acid having a concentration of 98 wt%, acid-leached at 80° C. for 4 h, and then hydrogen peroxide having a concentration of 27.5 wt% was added to a pH value of 1.5, and solid-liquid separation was performed to obtain a leachate and a leach residue;

[0187] The amount of sulfuric acid used is 0.8 times the theoretical amount of acid leaching;

[0188] (2) firstly mixing the second oxidant with the leaching solution obtained in step (1) for 0.5 h, then adding trisodium phosphate, carrying out chromium removal reaction at 40° C. and pH 3.5 (adjusted by nickel hydroxide) for 2 h, standing for 6 h, and then carrying out solid-liquid separation to obtain chromium removal slag and chromium removal filtrate;

[0189] The second oxidant is 27.5 wt% hydrogen peroxide, and the amount of the second oxidant added is such that the content of trivalent iron ions in the system is 0.5 g / L;

[0190] Trisodium phosphate is added in the form of a 20 wt% solution, the amount added being 1.8 times the theoretical amount of chromium reaction in the system;

[0191] (3) mixing the first oxidant, phosphoric acid and the chromium removal filtrate obtained in step (2), controlling the pH value to 2 using 32 wt % sodium hydroxide, and removing iron at 95° C. for 4 h to obtain iron phosphate and an iron removal liquid;

[0192] The first oxidant is 27.5wt% hydrogen peroxide, and the amount of the first oxidant added is 1.2 times the theoretical amount of the reaction with the ferrous ions in the system; the amount of the phosphoric acid added is 1.1 times the theoretical amount of the reaction with the iron in the system;

[0193] (4) mixing ferric sulfate with the iron removal solution obtained in step (3) to remove phosphorus, thereby obtaining a phosphorus removal solution and iron phosphate slag;

[0194] The amount of ferric sulfate added is 1.2 times the theoretical amount required for reaction with phosphorus;

[0195] (5) The dephosphorization solution is first concentrated to a Ni concentration of 120 g / L in the concentrated solution, and then stirred and mixed with aluminum sulfate 18hydrate and a 32 wt% sodium hydroxide solution, reacted at 70° C. for 1 h, and allowed to stand for 12 h, and solid-liquid separation was performed to obtain a dephosphorization residue and a dephosphorization liquid;

[0196] The amount of sodium hydroxide solution added is sufficient to make the pH value of the system 5.5;

[0197] Cobalt sulfate and manganese sulfate are added to the obtained impurity removal liquid for batching, and a ternary precursor is obtained through a coprecipitation reaction.

[0198] In this embodiment, the compositions of the leaching solution, the chromium removal filtrate, the concentrated solution and the impurity removal solution are shown in Table 8.

[0199] Table 8

[0200]

[0201] It can be seen from the above-mentioned Examples 1 to 5 that, as the preferred technical solution of the present invention, the purpose of deep impurity removal can be achieved, that is, the Cr in the chromium removal filtrate can be reduced to below 5ppm, and the Si in the impurity removal liquid can be reduced to below 10ppm. The methods in Examples 6 to 8 adopt a chemical precipitation method, which can reduce the Cr in the chromium removal filtrate to 10ppm to 20ppm, and reduce the Si to 10ppm to 30ppm.

[0202] In summary, the method provided by the present invention can achieve the purpose of deep impurity removal without extraction operation, has low processing cost, can make the iron in the nickel-iron alloy into battery-grade iron phosphate, and nickel can be made into a precursor, so the comprehensive benefit is high; the method provided by the present invention aims at the characteristic that chromium in the acid leaching solution is difficult to remove, phosphate is ionized into phosphate ions and hydroxide ions in the solution, and the conditions of the chromium removal reaction are controlled, so that the phosphate ions, hydroxide ions and iron ions in the acid leaching solution are combined into amorphous iron phosphate and iron hydroxide; amorphous iron phosphate can induce the formation of chromium phosphate, and iron hydroxide can adsorb a part of chromium ions, and the purpose of deep chromium removal is achieved by a method combining induction and adsorption; the phosphorus removal solution contains silicon, zinc and iron, and silicate is added as an inducer to ionize silicate in the solution into silicic acid and hydroxide ions, and silicate can induce silicate ions in the solution to become silicate, and hydroxide ions are combined with iron and nickel to form iron hydroxide and nickel hydroxide; iron hydroxide and nickel hydroxide can adsorb silicon, and the purpose of deep silicon removal is achieved by a method combining induction and adsorption.

[0203] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.

Claims

1. A method for smelting nickel-iron alloy, characterized in that: The method comprises the following steps: (1) the nickel-iron alloy is subjected to oxidative acid leaching to obtain a leaching solution and a leaching residue; (2) removing chromium from the leaching solution obtained in step (1) to obtain chromium-removed slag and chromium-removed filtrate; (3) mixing the first oxidant, phosphoric acid and the chromium removal filtrate obtained in step (2) to remove iron, thereby obtaining iron phosphate and an iron removal liquid; (4) mixing the trivalent iron salt with the iron removal solution obtained in step (3) to remove phosphorus, thereby obtaining a phosphorus removal solution and iron phosphate slag; (5) The dephosphorization solution obtained in step (4) is subjected to impurity removal, and the obtained impurity-removed solution is used to prepare a precursor.

2. The method according to claim 1, characterized in that The oxidative acid leaching of step (1) comprises: firstly mixing the nickel-iron alloy with an acid for acid leaching, and then adding hydrogen peroxide until the pH value is 1 to 2; Preferably, the acid comprises any one of sulfuric acid, hydrochloric acid or nitric acid or a combination of at least two thereof, preferably sulfuric acid; Preferably, the amount of the acid used is 0.8 times or more of the theoretical amount; Preferably, the acid leaching temperature is 70°C to 90°C; Preferably, the acid leaching time is 2.5 h to 5 h.

3. The method according to claim 1 or 2, characterized in that: The chromium removal in step (2) comprises: firstly mixing the second oxidant with the leaching solution obtained in step (1), then adding phosphate to carry out chromium removal reaction, and performing solid-liquid separation after standing to obtain chromium removal slag and chromium removal filtrate.

4. The method according to claim 3, characterized in that The second oxidant includes any one of hydrogen peroxide, sodium persulfate or manganese dioxide or a combination of at least two thereof; Preferably, the amount of the second oxidant added is such that the content of trivalent iron ions in the system is 0.5 g / L to 2 g / L; Preferably, the phosphate includes any one of trisodium phosphate, sodium dihydrogen phosphate or sodium monohydrogen phosphate, or a combination of at least two thereof; Preferably, the amount of the phosphate added is 1.1 to 3 times the theoretical amount of chromium reaction in the system.

5. The method according to claim 3 or 4, characterized in that: The temperature of the chromium removal reaction is 25°C to 50°C; Preferably, the pH value of the chromium removal reaction is 3 to 5; Preferably, the chromium removal reaction time is 1h to 3h; Preferably, the standing time is 5 h to 12 h.

6. The method according to any one of claims 1 to 5, characterized in that: Step (3) the first oxidant comprises any one of hydrogen peroxide, oxygen, ozone or sodium persulfate or a combination of at least two thereof, preferably hydrogen peroxide; Preferably, the amount of the first oxidant added is 1 to 1.5 times the theoretical amount for reacting with ferrous ions in the system; Preferably, the amount of phosphoric acid added is 1 to 1.2 times the theoretical amount required for reacting with iron in the system; Preferably, the iron removal in step (3) is carried out at a pH value of 1 to 2; Preferably, the temperature for removing iron in step (3) is 80°C to 95°C.

7. The method according to any one of claims 1 to 6, characterized in that: The trivalent iron salt in step (4) includes ferric sulfate; Preferably, the amount of the trivalent iron salt added in step (4) is 1 to 2 times the theoretical amount required for reaction with phosphorus.

8. The method according to any one of claims 1 to 7, characterized in that: The impurity removal in step (5) comprises: firstly concentrating the dephosphorization solution, then mixing it with silicate and alkali solution, letting it stand after the reaction, and separating the solid and liquid to obtain impurity removal residue and impurity removal liquid.

9. The method according to claim 8, characterized in that The concentration is concentrated to a Ni concentration in the solution of 100 g / L to 120 g / L; Preferably, the silicate is added in an amount of 0.1 g / L to 1.5 g / L; Preferably, the alkali solution is added in an amount sufficient to react with nickel in the system to generate 3 g / L to 10 g / L of nickel hydroxide.

10. The method according to claim 8 or 9, characterized in that: The reaction temperature is 50°C to 80°C; Preferably, the reaction time is 1 h to 3 h; Preferably, the standing time is 12 h to 24 h.

Citation Information

Patent Citations

  • Method for removing silicon from nickel solution through deep purification

    CN106191442A

  • Method for preparing battery material by using ferro-nickel alloy

    CN116409762A

  • Method for removing silicon in nickel sulfate production process

    CN117069166A

  • Method and device for removing chromium from ferronickel leachate

    CN118139996A

  • A process for the simultaneous production of salts of hexavalent chromium and other valuable oxygen compounds

    GB416624A