Method for preparing cobalt-free single crystal positive electrode material by lithium source echelon roasting process
Through the lithium source caulking process and the regulation of baking conditions, the problems of low lithium source utilization and poor battery performance of cobalt-free single crystal cathode material are solved, and higher lithium source utilization and electrochemical performance are achieved.
Patent Information
- Application Number
- CN202311305396.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-10
- Publication Date
- 2024-12-06
AI Technical Summary
The traditional single-firing process of existing cobalt-free single-crystal cathode materials leads to low utilization of lithium sources, residual alkaline substances, affecting battery performance, and high cost.
The lithium source step-firing process is adopted, and the first calcination is cooled and the airflow is broken. Then the second lithium source is added for secondary calcination. The use of the lithium source and material structure are optimized by regulating the calcination conditions such as the heating rate and time.
It improves the utilization rate of lithium sources, improves electrochemical performance and cycle stability, reduces material costs, and optimizes the single crystal morphology and battery capacity.
Smart Images

Figure HDA0004486001610000011 
Figure HDA0004486001610000012 
Figure HDA0004486001610000021
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of positive electrode materials for photolithium ion batteries, in particular to the field of IPC H01M4, and more specifically to a method for preparing a cobalt-free single crystal positive electrode material by a lithium source stepwise roasting process. Background Art
[0002] In the context of the deepening energy crisis, electric vehicles and energy storage equipment powered by lithium-ion batteries and other batteries have developed rapidly. Vigorously developing electric vehicles and clean energy can accelerate the process of fuel substitution and reduce tail gas emissions, which is of great significance to ensuring energy security, promoting energy conservation and emission reduction, and preventing and controlling air pollution. Positive electrode materials, as a key part affecting the performance of lithium-ion batteries, are the focus of current technical research. In order to further control the cost of positive electrode materials and improve the cost performance, the utilization rate of lithium is increased in the cobalt-free binary components, and the use of high-cost lithium carbonate is reduced, so as to achieve the effect of reducing costs and increasing efficiency. The traditional process of cobalt-free single crystal positive electrode materials adopts a one-time roasting lithiation process, which not only has poor consistency in single crystal morphology, but also has a low utilization rate of lithium source, resulting in a large amount of alkaline substances remaining on the surface, which not only affects the processing performance, but also ultimately leads to deterioration of battery performance.
[0003] CN109616663B discloses a method for preparing a nickel-cobalt-aluminum ternary positive electrode material, comprising the following steps: preparing a nano-alumina solution, a nickel-cobalt salt solution and a complexing alkali solution; performing liquid phase precipitation synthesis to obtain a ternary positive electrode material precursor; drying the ternary positive electrode material precursor and grinding it into a precursor powder; mixing a lithium salt with the precursor powder and performing heat treatment to obtain the nickel-cobalt-aluminum ternary positive electrode material. The preparation method has the characteristics of simple and convenient process. However, the invention adopts a one-time calcination lithiation process, which not only has a low degree of lithiation but also has a severe reaction temperature that will greatly lose the lithium source, resulting in excessive lithium source being added during the calcination of the ternary material and not being fully utilized, thereby increasing the material cost.
[0004] CN115974172A discloses a method and application of a low-cobalt and cobalt-free positive electrode material prepared by a pre-burning lithium-poor process. By designing the pre-burning process, especially controlling the conditions of the pre-burning process: heating to 300-750°C at a heating rate of 4-6°C / min, and pre-burning time of 3-24h; the precursor has enough time to absorb oxygen and react more easily with the lithium source, and the ternary positive electrode material is easier to achieve lithiation, but the lithium source of the invention is added at one time, which affects the electrochemical performance to a certain extent. Summary of the invention
[0005] The first aspect of the present invention provides a method for preparing a cobalt-free single crystal positive electrode material by a lithium source stepwise roasting process, comprising the following steps:
[0006] Step 1: Mixing a cobalt-free precursor with a first lithium source and performing a calcination;
[0007] Step 2: After the primary calcination is completed, the material is cooled, subjected to air flow crushing, and a second lithium source is added for secondary calcination;
[0008] Step 3: After the secondary roasting process is completed, air flow crushing is performed again to obtain the product.
[0009] The applicant has found that the mass ratio of the first lithium source to the second lithium source is (50-90): (10-50). On the basis of obtaining excellent electrochemical performance, the use of lithium source can be reduced, which may reduce the degree of lithium-nickel mixing and improve the utilization rate of lithium source. However, if the first lithium source is too little, it is easy to make the lithium insertion prematurely fixed, resulting in lithium vacancies in the material structure. Most of these vacancies are occupied by Ni. 2+ Occupancy will reduce the electrochemical properties and structural stability of the material. Too much of the first lithium source will cause residual lithium on the surface of the material, hindering the insertion and extraction of lithium ions, and will also increase the alkalinity of the material surface, affecting the electrochemical properties of the material.
[0010] Further research found that the process conditions for primary calcination were: heating at a rate of 2-10°C / min to 700-950°C and then maintaining the temperature for 4-10 hours, which could further improve the battery's gram capacity and cycle performance. This may be due to the reduction of the diffusion path of lithium ions, the slowing of the stress caused by phase change, the reduction of microcracks, and the enhancement of the material's cycle stability. Too low a temperature will cause Ni 2+ It is difficult to be oxidized to Ni 3+ , increasing the degree of lithium-nickel mixing and reducing the electrochemical performance. Too high a temperature will lead to the precipitation of lattice oxygen in the material, destroying the layered structure. 2+ It is difficult to oxidize and the ions diffuse slowly in the solid phase, and too long a time will lead to particle agglomeration, volatilization of lithium salts and energy waste.
[0011] The mass ratio of the first lithium source to the second lithium source is (50-90):(10-50).
[0012] Preferably, the mass ratio of the first lithium source to the second lithium source is (80-90):(10-20).
[0013] The cobalt-free precursor is a metal compound containing at least one of nickel and manganese, and the metal compound includes at least one of metal hydroxide, metal carbonate, metal oxide and metal sulfate.
[0014] Preferably, the cobalt-free precursor comprises Ni x Mn y (OH)2、Ni x Mn yCO3、Ni x Mn y O and Ni x Mn y At least one of SO4, wherein 0≤x≤1, 0≤y≤1.
[0015] The first lithium source includes at least one of alkyl lithium alkoxide, organic lithium acid and inorganic lithium acid.
[0016] Preferably, the alkyl lithium alkoxide includes at least one of lithium ethoxide, lithium methoxide, lithium isopropoxide and lithium butoxide.
[0017] Preferably, the organic acid lithium includes at least one of lithium acetate and lithium formate.
[0018] Preferably, the inorganic acid lithium includes at least one of LiNO3, LiNO2, Li2CO3, Li2SO4, Li2SO3, LiClO4 and LiMnO4.
[0019] Further preferably, the first lithium source includes Li2CO3.
[0020] Preferably, the second lithium source and the first lithium source are of the same material.
[0021] The process conditions of the primary calcination are: heating to 700-950° C. at a heating rate of 2-10° C. / min and then maintaining the constant temperature for 4-10 hours.
[0022] Preferably, the process conditions of the primary calcination are: heating to 750-950° C. at a heating rate of 4-6° C. / min and then maintaining the constant temperature for 4-10 hours.
[0023] The process conditions of the secondary calcination are: heating to 800-1000° C. at a heating rate of 2-10° C. / min and then maintaining the constant temperature for 4-10 hours.
[0024] Preferably, the process conditions of the secondary calcination are: heating to 850-1000° C. at a heating rate of 4-6° C. / min and then maintaining the constant temperature for 4-8 hours.
[0025] The cobalt-free precursor contains all metal elements Me, the first lithium source and the second lithium source contain Li, and the molar ratio of the sum of Li in the first lithium source and the second lithium source to Me is (1.01-1.10):1.
[0026] The cooling temperature is 100-200°C.
[0027] Preferably, the cooling temperature is 120-200°C.
[0028] Beneficial effects:
[0029] 1. The mass ratio of the first lithium source to the second lithium source is (50-90): (10-50), which can reduce the use of lithium sources and improve the utilization rate of lithium sources while obtaining excellent electrochemical performance.
[0030] 2. The mass ratio of the first lithium source to the second lithium source is (80-90): (10-20). The prepared battery has a significantly improved cycle stability while having a relatively low decrease in gram capacity.
[0031] 3. The process conditions of the primary calcination are regulated as follows: heating to 700-950°C at a heating rate of 2-10°C / min and maintaining the constant temperature for 4-10 hours, which can further improve the battery's gram capacity and cycle performance at the same time.
[0032] 4. The molar ratio of the sum of Li and Me in the first lithium source and the second lithium source is (1.01-1.10):1. By combining the primary calcination and secondary calcination processes, a better single crystal morphology can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is the surface morphology (SEM) of the positive electrode material of Example 1.
[0034] Figure 2 This is the surface morphology (SEM) of the positive electrode material of Example 2.
[0035] Figure 3 This is the surface morphology (SEM) of the positive electrode material of Comparative Example 1.
[0036] Figure 4 This is the surface morphology (SEM) of the positive electrode material of Comparative Example 2.
[0037] Figure 5 This is the surface morphology (SEM) of the positive electrode material of Comparative Example 3.
[0038] Figure 6 1 and 2 are the first charge and discharge curves of Example 1 and Comparative Example 1, wherein the light-colored line corresponds to Example 1 and the dark-colored line corresponds to Comparative Example 1.
[0039] Figure 7 1 and 2 are cycle curves of Example 1 and Comparative Example 1, wherein the light-colored dot graph corresponds to Example 1, and the dark-colored dot graph corresponds to Comparative Example 1.
[0040] Figure 8 1 are the first charge and discharge curves of Example 2 and Comparative Example 2, wherein the light-colored line corresponds to Example 2 and the dark-colored line corresponds to Comparative Example 2.
[0041] Fig. 9 1 and 2 are cycle curves of Example 2 and Comparative Example 2, wherein the light-colored dot diagram corresponds to Example 2, and the dark-colored dot diagram corresponds to Comparative Example 2.
[0042] Fig.10 This is the first charge and discharge curve of Comparative Example 3.
[0043] Fig.11 This is the cycle curve of Comparative Example 3. DETAILED DESCRIPTION
[0044] Example 1
[0045] 3.00 kg of cobalt-free precursor (NM6040, produced by our company) and 0.9830 kg of Li2CO3 are mixed at high speed, then all are put into a bowl and placed in an air atmosphere, heated to 850°C at a heating rate of 5°C / min, and then kept at a constant temperature for 6 hours. After the material is naturally cooled to 150°C, it is subjected to air flow crushing (crusher model: ceramic machinery, air flow mill two-in-one equipment / MQW03+CSM120; crushing parameters: classification 100-180), and the D50 particle size is 3.0-6.0 μm; then the crushed sample is again mixed with 0.2458 kg of Li2CO3 at high speed and put into a bowl in an air atmosphere, heated to 930°C at a heating rate of 5°C / min, and then kept at a constant temperature for 6 hours. After naturally cooling to 150°C, it is subjected to air flow crushing to obtain the product.
[0046] The molar ratio of Me in the cobalt-free precursor to Li in the total Li2CO3 is 1:1.015.
[0047] Example 2
[0048] 3.00 kg of cobalt-free precursor (NM5545, produced by our company) and 1.1042 kg of Li2CO3 are mixed at high speed, then all are put into a bowl and placed in an air atmosphere, heated to 880°C at a heating rate of 5°C / min, and then kept at a constant temperature for 6 hours. After the material is naturally cooled to 150°C, it is subjected to air flow crushing; then the crushed sample is again mixed with 0.1227 kg of Li2CO3 at high speed and put into a bowl in an air atmosphere, heated to 960°C at a heating rate of 5°C / min, and then kept at a constant temperature for 6 hours. After naturally cooling to 150°C, it is subjected to air flow crushing to obtain the product.
[0049] The molar ratio of Me in the cobalt-free precursor to Li in the total Li2CO3 is 1:1.01.
[0050] Comparative Example 1
[0051] 3.00 kg of cobalt-free precursor (NM6040, produced by our company) and 1.3136 kg of Li2CO3 are mixed at high speed, then all are put into a pot and heated to 930°C at a heating rate of 5°C / min in an air atmosphere, and then kept at a constant temperature for 12 hours. After the material is naturally cooled to 150°C, it is obtained.
[0052] The molar ratio of Me in the cobalt-free precursor to Li in the total Li2CO3 is 1:1.085.
[0053] Comparative Example 2
[0054] 3.00 kg of cobalt-free precursor (NM5545, produced by our company) and 1.2269 kg of Li2CO3 are mixed at high speed, then all are put into a pot and heated to 960°C at a heating rate of 5°C / min in an air atmosphere, and then kept at a constant temperature for 10 hours. After the material is naturally cooled to 150°C, it is obtained.
[0055] The molar ratio of Me in the cobalt-free precursor to Li in the total Li2CO3 is 1:1.065.
[0056] Comparative Example 3
[0057] 3.00 kg of cobalt-free precursor (NM5545, produced by our company) and 0.203 kg of Li2CO3 are mixed at high speed, then all are put into a bowl and placed in an air atmosphere, heated to 880°C at a heating rate of 5°C / min, and then kept at a constant temperature for 6 hours. After the material is naturally cooled to 150°C, it is subjected to air flow crushing; then the crushed sample is again mixed with 0.812 kg of Li2CO3 at high speed and put into a bowl in an air atmosphere, heated to 960°C at a heating rate of 5°C / min, and then kept at a constant temperature for 6 hours. After naturally cooling to 150°C, it is subjected to air flow crushing to obtain the product.
[0058] The molar ratio of Me in the cobalt-free precursor to Li in the total Li2CO3 is 1:1.01.
[0059] Comparative Example 4
[0060] 3.00 kg of cobalt-free precursor (NM5545, produced by our company) and 1.227 kg of Li2CO3 are mixed at high speed, then all are put into a bowl and placed in an air atmosphere, heated to 880°C at a heating rate of 5°C / min, and then kept at a constant temperature for 6 hours. After the material is naturally cooled to 150°C, it is subjected to air flow crushing; then the crushed samples are mixed at high speed and put into a bowl in an air atmosphere, heated to 960°C at a heating rate of 5°C / min, and then kept at a constant temperature for 6 hours. After naturally cooling to 150°C, it is subjected to air flow crushing to obtain the product.
[0061] The molar ratio of Me in the cobalt-free precursor to Li in the total Li2CO3 is 1:1.01.
[0062] Performance Testing Methods
[0063] 1. Observe the morphology of the cathode material under a scanning electron microscope (SEM), such as Figure 1-5 shown.
[0064] 2. Assemble the positive electrode materials in the embodiments and comparative examples into batteries: weigh 9.5 g of positive electrode material, add 0.3 g of acetylene black (SP) as a conductive agent and 0.2 g of PVDF (HSV-900) as a binder, mix thoroughly, add N-methyl-pyrrolidone (NMP) solvent to a solid content of 70% for dispersion, and slurry evenly on a 16 μm thick aluminum foil to form a positive electrode sheet. In an anaerobic glove box, a metal lithium sheet is used as the negative electrode, a 12+4 μm ceramic diaphragm is used as the diaphragm, and a mixture of 1 mol / L LiPF6 of ethyl carbonate (EC), dimethyl carbonate (DMC) and diethyl carbonate (EMC) (volume ratio of 1:1:1) is used as the electrolyte. A standard half-cell configuration is adopted, and a (CR2032) button cell is used as the battery shell, and the half-cell is assembled for subsequent battery testing.
[0065] 1. Measure the first discharge capacity (mAh / g) of the battery at a voltage range of 4.35-2.8V and a charge / discharge rate of 0.2C. Figure 6 , Figure 8 , Fig.10 shown.
[0066] 2. Test at 1.0C current density and 4.35V voltage. After 50 cycles, the capacity retention rate is as follows: Figure 7 , Fig. 9 , Fig.11 shown.
[0067] The test data are listed in Table 1.
[0068] Performance test data
[0069] Table 1
[0070] Gram capacity (mAh / g) Capacity retention rate (%) SEM morphology Example 1 175.5 87.7 Single crystal distribution Example 2 183.6 51.6 Single crystal distribution Comparative Example 1 178.2 83.2 Polycrystalline agglomerate distribution Comparative Example 2 184.2 48.9 Polycrystalline agglomerate distribution Comparative Example 3 187.6 45.7 Polycrystalline agglomerate distribution Comparative Example 4 163.5 52.6 Polycrystalline agglomerate distribution
Claims
1. A method for preparing a cobalt-free single crystal positive electrode material by a lithium source stepwise roasting process, characterized in that: The following steps are involved: Step 1: Mixing a cobalt-free precursor with a first lithium source and performing a calcination; Step 2: After the primary calcination is completed, the material is cooled, subjected to air flow crushing, and a second lithium source is added for secondary calcination; Step 3: After the secondary roasting process is completed, air flow crushing is performed again to obtain the product.
2. The method for preparing a cobalt-free single crystal positive electrode material by a lithium source stepwise roasting process according to claim 1, characterized in that: The mass ratio of the first lithium source to the second lithium source is (50-90):(10-50).
3. The method for preparing a cobalt-free single crystal positive electrode material by a lithium source stepwise roasting process according to claim 2, characterized in that: The mass ratio of the first lithium source to the second lithium source is (80-90):(10-20).
4. The method for preparing a cobalt-free single crystal positive electrode material by a lithium source stepwise roasting process according to claim 3, characterized in that: The cobalt-free precursor is a metal compound containing at least one of nickel and manganese; preferably, the metal compound includes at least one of metal hydroxide, metal carbonate, metal oxide and metal sulfate.
5. The method for preparing a cobalt-free single crystal positive electrode material by a lithium source stepwise roasting process according to claim 1 or 4, characterized in that: The cobalt-free precursor includes Ni x Mn y (OH)2、Ni x Mn y CO3、Ni x Mn y O and Ni x Mn y At least one of SO4, wherein 0≤x≤1, 0≤y≤1.
6. The method for preparing a cobalt-free single crystal positive electrode material by a lithium source stepwise roasting process according to claim 5, characterized in that: The first lithium source includes at least one of alkyl lithium alkoxide, organic lithium acid and inorganic lithium acid.
7. The method for preparing a cobalt-free single crystal positive electrode material by a lithium source stepwise roasting process according to claim 6, characterized in that: The process conditions of the primary calcination are: heating to 700-950° C. at a heating rate of 2-10° C. / min and then maintaining the constant temperature for 4-10 hours.
8. The method for preparing a cobalt-free single crystal positive electrode material by a lithium source stepwise roasting process according to claim 7, characterized in that: The process conditions of the secondary calcination are: heating to 800-1000° C. at a heating rate of 2-10° C. / min and then maintaining the constant temperature for 4-10 hours.
9. The method for preparing a cobalt-free single crystal positive electrode material by a lithium source stepwise roasting process according to claim 8, characterized in that: The cobalt-free precursor contains all metal elements Me, the first lithium source and the second lithium source contain Li, and the molar ratio of the sum of Li in the first lithium source and the second lithium source to Me is (1.01-1.10):
1.
10. The method for preparing a cobalt-free single crystal positive electrode material by a lithium source stepwise roasting process according to claim 9, characterized in that: The cooling temperature is 100-200°C.