Method and device for preparing high-purity gallium through magnetron directional crystallization

By using a magnetron directional crystallization device in gallium liquid and using stirring technology with different magnetic field strengths, the problems of low purity and high operation difficulty in the existing technology are solved, and efficient high-purity gallium preparation is achieved, which is suitable for industrial production.

CN119082509APending Publication Date: 2024-12-06SHANGHAI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411193065.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In the prior art, the high-purity preparation device of gallium is difficult to operate and has low crystallization efficiency, resulting in low purity of gallium, which limits the feasibility of industrial production.

Method used

Design a magnetron directional crystallization device, using an annular crystal trough, a constant temperature tank, a first magnetic field generator and a second magnetic field generator, through stirring with different magnetic field strengths, the uniform temperature distribution and impurity removal of gallium liquid are achieved, and the purity of gallium.

Benefits of technology

It achieves efficient temperature uniformity of gallium liquid and impurity removal, improves the purity of gallium, simplifies operation, and is suitable for industrial production of high-purity gallium 8N and above.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082509A_ABST
    Figure CN119082509A_ABST
Patent Text Reader

Abstract

The invention relates to a method and device for preparing high-purity gallium through magnetron directional crystallization, and the device comprises an annular crystallization tank, a constant-temperature tank disposed on the side wall of the outer ring of the crystallization tank, a first magnetic field generator disposed on the periphery of the outer ring of the crystallization tank, and a plurality of second magnetic field generators disposed on the side wall of the inner ring of the crystallization tank. The magnetic field intensity of the first magnetic field generator is larger than that of the second magnetic field generator, and the magnetic field directions of the first magnetic field generator and the second magnetic field generator face the crystallizer. Compared with the prior art, stirring with different magnetic field intensities is applied to the two sides of the liquid crude gallium, so that the internal temperature of the gallium liquid is more uniform, the thickness of a boundary layer at a liquid-solid interface is reduced, the impurity removal efficiency is improved, the extraction process of the high-purity gallium is more efficient and uniform, a higher purity standard can be achieved, and the yield of the high-purity gallium is improved. The method is suitable for industrial production of 8N and above high-purity gallium.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal purification, and in particular to a method and a device for preparing high-purity gallium by magnetron directional crystallization. Background Art

[0002] Gallium is a rare metal with a low melting point and a high boiling point. Its compounds are widely used in cutting-edge technology fields such as semiconductor materials, optoelectronic materials, and medical devices, and are known as the "backbone of the electronics industry." China currently has the capacity to mass-produce high-purity gallium, but due to the limitations of technical stability, most companies have low output and mainly produce low-level products (below 6N). This means that the output of high-level products such as 7N and 8N in my country cannot meet the domestic market demand at this stage, and it still needs to rely on imports. Therefore, it is urgent to develop new, efficient, stable, and ultra-high-purity gallium preparation technologies.

[0003] Gallium is present in very low concentrations in the earth's crust. It is usually associated with metals such as aluminum and zinc and is recovered as a by-product of smelting. The extraction process includes acid or alkali leaching, enrichment through ion exchange, graded precipitation and solvent extraction, and finally obtaining 99.99% crude gallium through electrolysis. Crude gallium contains a variety of impurities such as Cu, Al, Fe, Pb, Cd, Hg, Zn, Sn, etc., which greatly limits its application. At present, the preparation of high-purity gallium in industry usually uses 4N grade gallium as raw material, and impurities are removed by electrolytic refining, crystallization, zone melting, vacuum distillation and other methods. Among them, the directional crystallization method is widely used in industrial production due to its high efficiency and high economic benefits.

[0004] The existing devices for preparing high-purity gallium by crystallization method all have the problems of complex equipment operation and low crystallization efficiency. CN108588449A discloses a device for preparing high-purity gallium, but the device is extremely difficult to operate in order to accurately control the temperature and stirring speed of the device, and the entire crystallization process is time-consuming, which is not conducive to rapid production. CN115786743A discloses that high-purity gallium can be produced through an effective cooling and crystallization process. However, this process requires precise temperature control and special equipment, which makes it have certain limitations in large-scale production and operational complexity. These factors limit the feasibility of this technology in large-scale industrial applications. CN 219784718U discloses a rough gallium impurity removal structure, in which a magnet is provided at the bottom of the impurity removal tank to stir the liquid gallium without contact, causing the stirring and flow of the liquid gallium to be concentrated at the bottom, while the influence on the upper liquid is small, thereby affecting the impurity removal effect.

[0005] Therefore, from the perspective of industrialization, we focused on issues such as the difficulty of operation and the low purity of the prepared gallium, and designed a new device and method for magnetron directional crystallization of high-purity gallium. Summary of the invention

[0006] The purpose of the present invention is to provide a method and device for preparing high-purity gallium through magnetron directional crystallization in order to overcome the problems of the prior art such as great difficulty in operation and low purity of prepared gallium.

[0007] The purpose of the present invention can be achieved by the following technical solutions:

[0008] One of the technical solutions of the present invention is to provide a device for preparing high-purity gallium by magnetron directional crystallization, comprising a circular crystallization tank, a constant temperature tank arranged on the outer ring side wall of the crystallization tank, a first magnetic field generator arranged around the outer ring of the crystallization tank, and a plurality of second magnetic field generators arranged on the inner ring side wall of the crystallization tank, wherein the magnetic field strength of the first magnetic field generator is greater than the magnetic field strength of the second magnetic field generator, and the magnetic field directions of the first magnetic field generator and the second magnetic field generator are both toward the crystallizer.

[0009] In some specific embodiments, a funnel for conveying raw materials is provided at the top inlet of the crystallization tank, a conveying pipeline is provided at the bottom outlet, and a first valve is provided on the conveying pipeline.

[0010] In some specific embodiments, a water inlet pipe is provided at the bottom inlet of the thermostatic bath, a drainage pipe is provided at the top outlet, a second valve is provided on the water inlet pipe, and a third valve is provided on the drainage pipe.

[0011] In some specific embodiments, a polytetrafluoroethylene coating is provided on the inner side wall of the crystallization tank.

[0012] In some specific embodiments, the magnetic field strength of the first magnetic field generator is 50-500 mT, and the magnetic field strength of the second magnetic field generator is 5-30 mT.

[0013] In some specific embodiments, the first magnetic field generator is an electromagnetic stirrer.

[0014] In some specific embodiments, the second magnetic field generator is a permanent magnet stirrer.

[0015] The second technical solution of the present invention is to provide a method for preparing high-purity gallium by magnetron directional crystallization. The device for preparing high-purity gallium by magnetron directional crystallization according to one of the above technical solutions comprises the following steps:

[0016] S1, washing the liquid crude gallium with acid to remove impurities, and collecting the liquid gallium after the acid is removed;

[0017] S2, placing the liquid gallium obtained in step S1 and the high-purity gallium seed crystal in a crystallization tank, adjusting the constant temperature tank to allow them to co-crystallize at a low temperature, and turning on the first magnetic field generator around the outer ring of the crystallization tank and a plurality of second magnetic field generators at the inner ring side wall, so that the magnetic field strength of the first magnetic field generator is greater than the magnetic field strength of the second magnetic field generator, discharging the uncrystallized liquid gallium, and melting the crystallized gallium;

[0018] S3. After repeating step S2 for multiple times, high-purity gallium is obtained.

[0019] In some specific embodiments, in step S1, the purity of the liquid crude gallium is in the range of 2N-4N.

[0020] In some specific embodiments, in step S1, when pickling and removing impurities, hydrochloric acid is first added to the liquid crude gallium and stirred once, and then nitric acid is added and stirred for a second time.

[0021] In some specific embodiments, the concentration of hydrochloric acid is 3-10 mol / L, the mass ratio of hydrochloric acid to liquid crude gallium is 1:3 to 1:8, and the stirring time is 3-8 hours;

[0022] In some specific embodiments, the concentration of nitric acid is 3-10 mol / L, the mass ratio of nitric acid to liquid gallium is 1:3 to 1:8, and the secondary stirring time is 3-8 h.

[0023] In some specific embodiments, in step S2, the number of high-purity gallium seed crystals added is 0-8.

[0024] In some specific embodiments, in step S2, the diameter of the high purity gallium seed crystal is 0.5 cm.

[0025] In some specific embodiments, in step S2, the preparation process of high-purity gallium seed crystal is: obtaining liquid high-purity gallium by low-temperature crystallization.

[0026] In some specific embodiments, liquid high-purity gallium is obtained by melting high-purity gallium of 5N or above.

[0027] In some specific embodiments, in step S2, the magnetic field strength of the first magnetic field generator located around the outer ring of the crystallization tank is 50-500 mT, and the magnetic field strength of the plurality of second magnetic field generators located at the side wall of the inner ring of the crystallization tank is 5-30 mT.

[0028] In some specific embodiments, in step S2, the temperature of low temperature crystallization is -10 to 25°C.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] (1) The present invention can make the temperature of the gallium liquid more uniform by applying different magnetic field strengths on both sides of the liquid crude gallium without blind spots, making the extraction process of high-purity gallium more efficient, and helping to achieve higher purity standards. Stirring with a larger magnetic field strength on the outside of the liquid crude gallium generates Lorentz force in the liquid crude gallium, thereby causing the liquid gallium to flow, which helps to make the temperature inside the gallium liquid more uniform, thereby effectively reducing the boundary layer thickness at the liquid-solid interface and improving the purification effect. Stirring with a smaller magnetic field strength on the inside of the liquid crude gallium can drive the flow of the gallium liquid, helping to reduce the boundary layer thickness at the liquid-solid interface, thereby improving the removal efficiency of impurities.

[0031] (2) The device provided by the present invention is easy to operate and simple to use, and can achieve a high crystallization efficiency, and is suitable for the industrial production of 8N and above high-purity gallium. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 It is a schematic diagram of the structure of the device of the present invention.

[0033] Figure 2 is the residual impurity content of gallium under different processing conditions.

[0034] Figure 1 The identifiers in are as follows:

[0035] 1 is a funnel, 2 is a constant temperature bath, 3 is a second valve, 4 is a second magnetic field generator, 5 is a first valve, 6 is a crystallization bath, 7 is a polytetrafluoroethylene coating, 8 is a first magnetic field generator, 9 is a water inlet pipe, 10 is a drainage pipe, and 11 is a third valve. DETAILED DESCRIPTION

[0036] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.

[0037] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.

[0038] In conjunction with the accompanying drawings, some embodiments of the present invention are described in detail below. In the absence of conflict, the following embodiments and features in the embodiments may be combined with each other.

[0039] In the following embodiments and comparative examples, if there is no special description of functional components or structures, it indicates that they are all conventional components or conventional structures used in the art to achieve corresponding functions. If there is no special description of raw materials or processing techniques, it indicates that they are all conventional commercially available raw materials or conventional processing techniques in the art.

[0040] Embodiment 1:

[0041] The present embodiment provides a device for preparing high-purity gallium by magnetron directional crystallization, comprising a circular crystallization tank 6, a constant temperature tank 2 arranged on the outer ring side wall of the crystallization tank 6, a first magnetic field generator 8 arranged around the outer ring of the crystallization tank 6, and a plurality of second magnetic field generators 4 arranged at the inner ring side wall of the crystallization tank 6, wherein the magnetic field strength of the first magnetic field generator 8 is greater than the magnetic field strength of the second magnetic field generator 4, and the magnetic field directions of the first magnetic field generator 8 and the second magnetic field generator 4 are both toward the crystallizer 6.

[0042] The technical solution is to set magnetic field generators with different magnetic field strengths on both sides of the crystallization tank 6 without dead angles. The outer ring side of the crystallization tank 6 is a magnetic field generator with a larger magnetic field strength, which can effectively adjust the overall flow of liquid gallium in the crystallization tank 6, make the temperature distribution of liquid gallium more uniform, and effectively reduce the boundary layer thickness at the liquid-solid interface; the inner ring side of the crystallization tank 6 is a magnetic field generator with a smaller magnetic field strength, which can accurately control the local flow of liquid gallium in the crystallization tank 6, reduce the accumulation of impurities, and help reduce the boundary layer thickness at the liquid-solid interface. The magnetic field stirring on both sides of the crystallization tank 6 can achieve a more comprehensive and uniform stirring effect, which can not only affect the internal flow of liquid gallium, but also control the boundary layer thickness of the entire liquid and the distribution of impurities.

[0043] During the directional crystallization process of liquid gallium, a boundary layer is formed on the liquid-solid interface. This boundary layer is a relatively static part of the fluid, and its thickness directly affects the mass transfer process. A thicker boundary layer will cause impurities to accumulate near the liquid-solid interface, affecting the purity of the crystallization. Therefore, by stirring the liquid gallium with magnetic fields of different magnetic field strengths, the flow speed and direction of the liquid gallium are changed, so that the substances in the boundary layer can flow and mix quickly, thereby reducing the thickness of the boundary layer. When the boundary layer becomes thinner, impurities are more likely to diffuse outward from the liquid-solid interface, reducing their doping in the crystal. At the same time, when the boundary layer becomes thinner, the diffusion rate of impurities in the liquid gallium will be accelerated, thereby improving the efficiency of impurity removal, and ultimately helping to produce higher purity gallium.

[0044] In order to facilitate the transportation of raw materials and products, a funnel 1 for conveying raw materials is provided at the top inlet of the crystallization tank 6, and a conveying pipeline 8 is provided at the bottom outlet. A first valve 5 is provided on the conveying pipeline, and a polytetrafluoroethylene coating 7 is provided on the inner wall of the crystallization tank 6. Exemplarily, the first valve 5 is a polytetrafluoroethylene ball valve, the funnel 1 is a polytetrafluoroethylene funnel, and the crystallization tank 6 is welded with 306 stainless steel. The polytetrafluoroethylene used makes the crystallization tank 6 and the first valve 5 have excellent corrosion resistance, temperature resistance, low friction coefficient, non-stickiness, and good insulation.

[0045] A water inlet pipe 9 is provided at the bottom inlet of the constant temperature bath 2, and a drainage pipe 10 is provided at the top outlet. A second valve 3 is provided on the water inlet pipe 9, and a third valve 11 is provided on the drainage pipe 10. Exemplarily, the second valve 3 and the third valve 11 are stainless steel ball valves with excellent corrosion resistance, high temperature resistance and good sealing performance.

[0046] The magnetic field strength of the first magnetic field generator 8 is 50-500mT, and the magnetic field strength of the second magnetic field generator 4 is 5-30mT. Exemplarily, the first magnetic field generator 8 is an electromagnetic stirrer, which can provide a larger magnetic field strength. The second magnetic field generator 4 is a permanent magnet stirrer, which can provide a smaller magnetic field strength, wherein the permanent magnet can be selected from aluminum nickel cobalt (AlNiCo) permanent magnets, ferrite permanent magnets, samarium iron boron (SmCo) permanent magnets, neodymium iron boron (NdFeB) permanent magnets, strontium ferrite (SrFeO3) permanent magnets, preferably neodymium iron boron (NdFeB) permanent magnets. Exemplarily, 6 neodymium iron boron permanent magnets are evenly arranged along the inner ring side wall of the crystallization groove 6.

[0047] Embodiment 2:

[0048] This embodiment is based on the device for preparing high-purity gallium by magnetron directional crystallization provided in the above embodiment 1 to prepare high-purity gallium. The preparation method includes the following steps:

[0049] (1) Crude gallium with a purity of 4N is melted at 50°C to obtain liquid crude gallium. 9 kg of liquid crude gallium is accurately weighed and placed in a polytetrafluoroethylene beaker with a volume of 3 L.

[0050] (2) Prepare 3 mol / L hydrochloric acid solution and 3 mol / L nitric acid solution. First, add 1.8 kg of 3 mol / L hydrochloric acid solution to the polytetrafluoroethylene beaker of step (1), mix with the liquid crude gallium, and place the polytetrafluoroethylene beaker on a precision electric stirrer to stir the liquid crude gallium containing the acid solution for 3 hours, and then add 1.8 kg of 3 mol / L nitric acid solution, and continue stirring for 3 hours to complete the pickling and remove impurities such as Zn, Al, Fe, Ca, etc. in the liquid gallium. After the acid solution is sucked out, pour the liquid gallium into the crystallization tank 6.

[0051] (3) Place 7N grade liquid high-purity gallium in a polytetrafluoroethylene beaker, place the polytetrafluoroethylene beaker in a constant temperature bath at 0°C, and stir with a polytetrafluoroethylene rod for 20 minutes to produce seed crystals with a diameter of 0.5 cm. Collect the seed crystals with uniform shapes, which can be used as the nucleation core of the liquid gallium, and select 4 seed crystals to be poured into the crystallization tank 6.

[0052] (4) The temperature of the thermostatic bath 2 was set to 5°C, the flow rate was 10L / min, and the electromagnetic stirrer and the permanent magnet stirrer were turned on at the same time. The magnetic field strength of the electromagnetic stirrer was set to 400mT, and the magnetic field strength of the permanent magnet stirrer was set to 10mT. It can be found that the liquid crude gallium was driven to stir. After crystallization for 2h, the first valve 5 on the conveying pipe 8 at the bottom of the crystallization tank 6 was opened to discharge the uncrystallized liquid gallium, and then the temperature of the thermostatic bath 2 was set to 50°C to melt the crystallized gallium in the crystallization tank 6. After repeating the above operation 7 times, 10g of liquid gallium in the crystallization tank 6 was sucked into a polytetrafluoroethylene centrifuge tube with a polytetrafluoroethylene pipette for GDMS detection.

[0053] The purity of the final product is about 8N. The test results are shown in Table 1. Figure 2 shown.

[0054] Table 1 The original impurity content of crude gallium and the impurity content of gallium after magnetron oriented crystallization

[0055]

[0056]

[0057] Comparative Example 1:

[0058] Compared with Example 2, most of them are the same, and the only difference is that the stirring effect of the electromagnetic stirrer and the permanent magnet stirrer on the gallium liquid is omitted.

[0059] The purity of the product is about 6N5. The specific test results are shown in Table 2. Figure 2 shown.

[0060] Table 2 Impurity content after 7 times of non-stirring directional crystallization

[0061]

[0062] Comparative Example 2:

[0063] Compared with Example 2, most of the steps are the same, with the only difference being that only the electromagnetic stirrer is turned on.

[0064] The purity of the product is about 6N8. The specific test results are shown in Table 3. Figure 2 shown.

[0065] Table 3 Impurity content after 7 times of magnetron oriented crystallization

[0066]

[0067] Comparative Example 3:

[0068] Compared with Example 2, most of them are the same, the only difference is that only the permanent magnet stirrer is turned on. The permanent magnet stirrer located on the inner ring side of the crystallization tank 6 can directly act on the boundary layer, effectively reduce the thickness of the boundary layer, better control the migration and distribution of impurities, and improve the removal efficiency of impurities. Although the electromagnetic stirrer located on the outer ring side of the crystallization tank 6 can drive the overall rotation of the liquid crude gallium and improve the uniformity of the macroscopic temperature field, this macroscopic stirring may not directly affect the solid-liquid interface at the microscopic level.

[0069] The purity of the product is about 7N, and the test results are shown in Table 4. Figure 2 shown.

[0070] Table 4 Impurity content after 7 times of magnetron oriented crystallization

[0071]

[0072] Comparative Example 4:

[0073] Compared with Example 1, most of them are the same, and the only difference is that a first magnetic field generator 8 is provided on both the inner ring side and the outer ring side of the crystallization tank 6. Exemplarily, the first magnetic field generator 8 is an electromagnetic stirrer.

[0074] When preparing high-purity gallium, the electromagnetic stirrer was turned on at the same time, and the final product purity was 6N9. The test results are shown in Table 5. Figure 2 As shown:

[0075] Table 5 Impurity content after 7 times of magnetron oriented crystallization

[0076]

[0077] Comparative Example 5:

[0078] Compared with Example 1, most of them are the same, the only difference is that a second magnetic field generator 4 is provided on both the inner ring and the outer ring of the crystallization tank 6. Exemplarily, the first magnetic field generator 4 is a permanent magnet stirrer, and the permanent magnet is preferably a neodymium iron boron (NdFeB) permanent magnet.

[0079] When preparing high-purity gallium, the permanent magnet stirrer was turned on at the same time, and the final product purity was 7N2. The test results are shown in Table 6. Figure 2 As shown:

[0080] Table 6 Impurity content after 7 times of magnetron oriented crystallization

[0081]

[0082]

[0083] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A device for preparing high-purity gallium by magnetron directional crystallization, It is characterized in that The invention comprises a ring-shaped crystallization tank (6), a constant temperature tank (2) arranged on the outer ring side wall of the crystallization tank (6), a first magnetic field generator (8) arranged around the outer ring of the crystallization tank (6), and a plurality of second magnetic field generators (4) arranged on the inner ring side wall of the crystallization tank (6), wherein the magnetic field strength of the first magnetic field generator (8) is greater than the magnetic field strength of the second magnetic field generator (4), and the magnetic field directions of the first magnetic field generator (8) and the second magnetic field generator (4) are both toward the crystallizer (6).

2. The device for preparing high-purity gallium by magnetron directional crystallization according to claim 1, It is characterized in that A funnel (1) for conveying raw materials is provided at the top inlet of the crystallization tank (6), and a conveying pipeline is provided at the bottom outlet, and a first valve (5) is provided on the conveying pipeline; A water inlet pipe (9) is provided at the bottom inlet of the thermostatic bath (2), and a drainage pipe (10) is provided at the top outlet. A second valve (3) is provided on the water inlet pipe (9), and a third valve (11) is provided on the drainage pipe (10).

3. The device for preparing high-purity gallium by magnetron directional crystallization according to claim 1, It is characterized in that A polytetrafluoroethylene coating (7) is provided on the inner side wall of the crystallization tank (6).

4. The device for preparing high-purity gallium by magnetron directional crystallization according to claim 1, It is characterized in that The first magnetic field generator (8) is an electromagnetic stirrer, and the magnetic field strength is 50-500mT; The second magnetic field generator (4) is a permanent magnet stirrer, and the magnetic field strength is 5-30 mT.

5. A method for preparing high-purity gallium by magnetron directional crystallization, It is characterized in that The device for preparing high-purity gallium by magnetron directional crystallization according to claims 1-4 comprises the following steps: S1, washing the liquid crude gallium with acid to remove impurities, and collecting the liquid gallium after the acid is removed; S2, placing the liquid gallium obtained in step S1 and the high-purity gallium seed crystal in a crystallization tank (6), adjusting the constant temperature tank (2) to allow them to co-crystallize at a low temperature, and turning on the first magnetic field generator (8) around the outer ring of the crystallization tank (6) and a plurality of second magnetic field generators (4) at the inner ring side wall, so that the magnetic field strength of the first magnetic field generator (8) is greater than the magnetic field strength of the second magnetic field generator (4), discharging the uncrystallized liquid gallium, and melting the crystallized gallium; S3. After repeating step S2 for multiple times, high-purity gallium is obtained.

6. The method for preparing high-purity gallium by magnetron oriented crystallization according to claim 5, It is characterized in that In step S1, the purity of the liquid crude gallium ranges from 2N to 4N; When pickling and removing impurities, first add hydrochloric acid to the liquid crude gallium and stir once, then add nitric acid and stir a second time.

7. The method for preparing high-purity gallium by magnetron oriented crystallization according to claim 6, It is characterized in that The concentration of hydrochloric acid is 3-10 mol / L, the mass ratio of hydrochloric acid to liquid crude gallium is 1:3 to 1:8, and the stirring time is 3-8 hours; The concentration of nitric acid is 3-10 mol / L, the mass ratio of nitric acid to liquid gallium is 1:3 to 1:8, and the secondary stirring time is 3-8 hours.

8. The method for preparing high-purity gallium by magnetron oriented crystallization according to claim 5, It is characterized in that In step S2, the preparation process of high-purity gallium seed crystal is as follows: high-purity gallium above 5N is melted to obtain liquid high-purity gallium, and the liquid high-purity gallium is crystallized at low temperature to obtain high-purity gallium seed crystal, and the diameter of the obtained high-purity gallium seed crystal is 0.5 cm.

9. The method for preparing high-purity gallium by magnetron oriented crystallization according to claim 5, It is characterized in that The number of high-purity gallium seed crystals added is 0-8.

10. The method for preparing high-purity gallium by magnetron oriented crystallization according to claim 5, It is characterized in that In step S2, the temperature of the low temperature crystallization is -10 to 25°C.