Method for recovering rare earth from fine-fraction sedimentary clay rock type rare earth ore
Through the pre-iron removal-roasting-leaching-rare earth mother liquor removal-precipitation-calcination process, the problems of low leaching rate and high impurity content of sedimentary clay rock-type rare earth ore are solved, efficient rare earth recovery and purity improvement are achieved, and the Process flow and reduce costs.
Patent Information
- Application Number
- CN202411255114.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-09
AI Technical Summary
In the prior art, the rare earth leaching rate of sedimentary clay rock-type rare earth ore has a low rare earth leaching rate and a high impurity content, and lacks a complete process flow from raw ore to rare earth oxides.
Using the pre-iron removal-roasting-leaching-rare earth mother liquor removal-precipitation-calcination process flow, rare earths are recovered from fine particle-grade sedimentary clay rock-type rare earth ore to obtain high purity rare earth oxides.
It has achieved efficient recycling of rare earths and improved purity, simplified the process flow, reduced costs, and is suitable for ores with different rare earth contents, with good economic benefits and strategic significance.
Smart Images

Figure CN119082512A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of rare earth processing, and in particular relates to a method for recovering rare earth from fine particle-grade sedimentary clay rock type rare earth ore. Background Art
[0002] Sedimentary clay rock type rare earth ores are widely distributed in the adjacent areas of Sichuan, Yunnan and Guizhou. The average grade of rare earth oxides is 0.39%, which exceeds the industrial grade of ion adsorption type rare earth deposits of 500μg / g. Rare earth resources are widely distributed and have great development potential. The main mineral composition of sedimentary clay rock type rare earth ores is kaolinite (the mineral content accounts for more than 89%), and the secondary minerals are cerium phosphate, anatase, mica, illite, chlorite, hematite, sericite and muscovite. Rare earths mainly exist in the form of ultra-microscopic cerium phosphate inclusions and independent minerals of cerium phosphate; a small amount of rare earth exists in kaolinite in the form of isomorphous. This rare earth mine is a weathering product of Emeishan basalt. The mineral particle size is relatively fine, mostly fine particle size (micron level), especially the particle size of rare earth minerals is mostly below 1μm. There are few reports on the comprehensive utilization of this rare earth resource.
[0003] Publication No. CN109266839A reports a method for selectively leaching sedimentary rare earth ores, wherein sedimentary rare earth ore powder is roasted with sulfuric acid at high temperature and then acid-leached to obtain a rare earth-rich liquid, but there is a lack of subsequent process flow.
[0004] Publication No. CN114134348A discloses a method for recovering sedimentary rare earths by a hot high-acid direct leaching process. The rare earth-rich leaching solution is crystallized from ammonium aluminum sulfate using ammonium sulfate, and then extracted and stripped to recover the rare earths. The process is complicated and the cost is high.
[0005] Publication No. CN104711424A discloses a method for recovering rare earths from the slag removed from the leachate of weathering crust elution type rare earth ore, wherein an aluminum product is obtained by precipitation with an alkaline solution, and a rare earth product is obtained by precipitation with an alkaline solution. The process aging time is relatively long and is suitable for solutions with high rare earth and aluminum contents.
[0006] Publication No. CN115058609A discloses a method for leaching rare earth from basalt weathering crust, which has a long roasting time and is suitable for basalt weathering crust with a relatively high degree of weathering.
[0007] Publication No. CN113621837A discloses a rare earth extraction method for low-grade fine-grained rare earth ores, which is mainly aimed at rare earth ores with a rare earth REEO content of no more than 0.113%, completes the rare earth roasting and leaching process, and finally obtains rare earth leaching solution and leaching residue.
[0008] At present, there are few reports on the complete process flow of sedimentary rare earth ores from raw ore to rare earth oxides. Summary of the invention
[0009] In order to solve the defects of low rare earth leaching rate and high impurity content of existing sedimentary clay rock type rare earth ores, the present invention provides a method for recovering rare earths from fine particle-level sedimentary clay rock type rare earth ores, thereby realizing green and efficient comprehensive utilization of valuable elements such as rare earths.
[0010] The technical solution of the present invention is as follows:
[0011] The present invention provides a method for recovering rare earth from fine particle-grade sedimentary clay rock type rare earth ore, comprising the following steps:
[0012] (1) Calcination: crushing and grinding the fine-particle sedimentary clay rock type rare earth ore, mixing it with a calcining agent, and calcining it to obtain a calcined rare earth ore;
[0013] (2) Leaching: Leaching rare earths from the roasted rare earth ore using a leaching agent to obtain a rare earth-rich mother liquor;
[0014] (3) precipitation and impurity removal: the rare earth-rich mother liquor is impurity-removed by using an impurity-removing agent to obtain an aluminum-rich precipitate and a rare earth-rich mother liquor after impurity removal;
[0015] (4) Precipitating rare earths: using a precipitant to precipitate rare earths from the rare earth-rich mother liquor after impurities removal to obtain a rare earth-rich precipitate;
[0016] (5) Calcination: Calcinate the rare earth-rich precipitate to obtain mixed rare earth oxides.
[0017] In a specific embodiment, the rare earth content of the fine particle-grade sedimentary clay rock type rare earth ore is 0.05% to 2.50%.
[0018] The present invention is also applicable to fine-particle sedimentary clay rock type rare earth ores with a rare earth content greater than 2.5% or less than 0.05%.
[0019] In a specific embodiment, in step (1), the particle size after crushing and grinding is -160 μm to -75 μm.
[0020] In a specific embodiment, when the iron content in the fine-particle sedimentary clay rock type rare earth ore is higher than 1.5%, an acidic reagent is required to remove iron before mixing with the roasting reagent; the acidic reagent is at least one of hydrochloric acid, nitric acid and sulfuric acid; the concentration of the acidic reagent is 0.5-4 mol / L; during the process of removing iron with the acidic reagent, the acidification temperature is 40-90°C, the acidification time is 0.5-2h, and the ratio of the acidic reagent to the ore sample is 10-40mL / g.
[0021] Removing iron before roasting can not only effectively reduce the consumption of roasting reagents and reduce the aluminum-iron separation process, but also reduce the impact of iron impurity ions on the product quality of rare earth precipitation crystallization and improve the recovery rate of rare earths.
[0022] In a specific embodiment, in step (1), the roasting agent is at least one of sulfuric acid, ammonium sulfate, sodium sulfate, sodium oxalate, ammonium chloride, magnesium chloride, sodium chloride and ammonium citrate. Preferably, the roasting agent is sulfuric acid or ammonium sulfate with a volume concentration of 60-98%; the ratio of the roasting agent sulfuric acid to the rare earth ore is 0.4-2 mL / g, and the mass ratio of the remaining roasting agents to the rare earth ore is 3:1-1:3; the roasting temperature is 300-800°C, and the roasting time is 5-55 min.
[0023] In a specific embodiment, in step (2), the leaching agent is an aqueous solution of at least one of sodium chloride, sodium citrate and ammonium chloride; the mass concentration of the leaching agent is 1 to 20%; the leaching temperature is 50 to 90° C., and the leaching time is 3 to 6 hours; the ratio of the leaching agent to the rare earth ore is 10 to 30 mL / g.
[0024] In a specific embodiment, in step (3), the impurity remover is at least one of sodium carbonate, sodium bicarbonate, sodium hydroxide, ammonia water and sodium sulfide; the mass concentration of the impurity remover is 7.8-49.7%; the temperature during the impurity removal process is 5-40°C, the pH value is 4.5-5.5, the impurity removal process is continuously stirred, and the filtration is completed 0-30 minutes after the precipitation is completed.
[0025] In a specific embodiment, the aluminum-rich precipitate in step (3) is calcined to obtain aluminum-rich oxide; the calcination temperature is 700 to 900° C., and the calcination time is 0.5 to 2 hours.
[0026] In a specific embodiment, in step (4), the precipitant is at least one of oxalic acid, ammonium oxalate and sodium oxalate, and the mass concentration of the precipitant solution is 6 to 12.5%.
[0027] In a specific embodiment, in step (5), the calcination temperature is 500-900° C., and the calcination time is 0.5-1 h.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] 1. The present invention aims at the comprehensive utilization of rare earths in fine-particle sedimentary clay rock-type rare earth ores. In view of the fact that the rare earths mainly exist in the form of ultra-microscopic cerium phosphate inclusions and independent mineral forms of cerium phosphate, a process flow of pre-iron removal-roasting-leaching-rare earth mother liquor impurity removal-precipitation-calcination is proposed to realize the process flow from rare earth ore to rare earth oxide products, and the obtained rare earth oxide products have high purity.
[0030] 2. The present invention belongs to the development and utilization process of potential rare earth resources, has simple equipment, easy operation, good product stability and high added value, provides a new way for the comprehensive utilization of fine particle sedimentary clay rock type rare earth ores, and has good economic benefits and strategic significance. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 It is a schematic diagram of the process flow of the present invention;
[0032] Figure 2 This is the XRD spectrum of the rare earth oxide of Example 3. DETAILED DESCRIPTION
[0033] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0034] The process flow chart of the embodiment is shown in Figure 1 shown.
[0035] In the embodiment, the fine particle sedimentary clay rock type rare earth ore is taken from the basalt weathering crust in a certain place in northwest Guizhou, wherein the rare earth (REE) content is between 0.05 and 2.50%. According to the rare earth content and the lithology difference of the ore, the rare earth ore is divided into a rare earth ore with a higher iron content (a mixture of rare earth ore samples with an iron oxide content greater than 1.50%, the rare earth content of the mixed sample is 0.247%, and the iron oxide content is 13.8%) and a rare earth ore with a lower iron content (a mixture of rare earth ore samples with an iron oxide content less than 1.50%, the rare earth content of the mixed representative sample is 2.20%, and the iron oxide content is 1.2%).
[0036] Example 1
[0037] Sampling was performed according to the particle size of the ore sample of -124μm. 30g of rare earth ore with low iron content (iron oxide content of 1.2%) was taken and directly mixed with sulfuric acid with a volume concentration of 90%. The ratio of roasting agent to mixed rare earth ore was 1.35mL / g, the roasting temperature was 700℃, and the roasting time was 15min to obtain the roasted rare earth ore. The roasted rare earth ore was mixed with a sodium citrate solution with a mass concentration of 5% for leaching, the leaching temperature was 90℃, the leaching time was 4h, the ratio of leaching agent to ore sample was 10mL / g, and a rare earth-rich mother liquor was obtained, and the rare earth leaching rate was 89.30%. A sodium carbonate solution with a mass concentration of 49.7% is used as a precipitant for precipitation and impurity removal, the precipitation temperature is 30°C, the precipitation pH value is 5.0, and the precipitation is directly filtered after the precipitation is completed to obtain a pure rare earth-rich mother liquor, and then a sodium oxalate solution with a mass concentration of 12.5% is used to precipitate rare earth to obtain a rare earth oxalate precipitate, which is calcined at 500°C for 1h to obtain a mixed rare earth oxide, and the product purity is 97.59%. The comprehensive recovery rate of rare earth is 79.03%.
[0038] Example 2
[0039] Sampling was performed according to the particle size of the ore sample of -75μm. 30g of rare earth ore with high iron content (iron oxide content of 13.8%) was taken, and 1mol / L hydrochloric acid was used, the acidification temperature was 90℃, the ratio of the acidic reagent to the ore sample was 30mL / g, and the acidification time was 2h to obtain the iron-free rare earth ore. The iron-free rare earth ore and the rare earth ore with low iron content (iron oxide content of 1.2%) were sampled at a mass ratio of 1:1 to obtain 30g of mixed rare earth ore, which was directly mixed with sulfuric acid with a volume concentration of 98%, the ratio of roasting agent to mixed rare earth ore was 1.35mL / g, the roasting temperature was 700℃, and the roasting time was 20min to obtain the roasted rare earth ore. The calcined rare earth ore was mixed with a sodium chloride solution with a mass concentration of 5% for leaching, the leaching temperature was 90°C, the leaching time was 4h, the ratio of leaching agent to ore sample was 20mL / g, and a rare earth-rich mother liquor was obtained, and the leaching rate of rare earth was 89.09%. A sodium carbonate solution with a mass concentration of 49.7% was used as a precipitant for precipitation and impurity removal, the precipitation temperature was 30°C, the precipitation pH value was 5.0, and the precipitation was directly filtered after the precipitation was completed to obtain a pure rare earth-rich mother liquor, and then a sodium oxalate solution with a mass concentration of 12.5% was used to precipitate rare earth to obtain a rare earth oxalate precipitate, which was calcined at 500°C for 1h to obtain a mixed rare earth oxide, and the product purity was 97.90%. The comprehensive recovery rate of rare earth was 76.13%.
[0040] Example 3
[0041] Sampling was performed according to the particle size of the ore sample of -124μm. 30g of rare earth ore with high iron content (iron oxide content of 13.8%) was taken, 3mol / L hydrochloric acid was used, the acidification temperature was 90℃, the ratio of the acidic reagent to the ore sample was 30mL / g, and the acidification time was 1h to obtain the iron-free rare earth ore. The iron-free rare earth ore and the rare earth ore with low iron content (iron oxide content of 1.2%) were sampled at a mass ratio of 2.5:1 to obtain 28g of mixed rare earth ore, which was directly mixed with sulfuric acid with a volume concentration of 80%, the mixed roasting agent sulfuric acid and rare earth ore ratio was 1.35mL / g, the roasting temperature was 700℃, and the roasting time was 15min to obtain the roasted rare earth ore. The roasted rare earth ore was mixed with an ammonium chloride solution with a mass concentration of 5% for leaching, the leaching temperature was 90°C, the leaching time was 4.5h, the leaching agent and the ore sample ratio was 20mL / g, and a rare earth-rich mother liquor was obtained, and the rare earth leaching rate was 88.02%. A sodium carbonate solution with a mass concentration of 49.7% was used as a precipitant for precipitation and impurity removal, the precipitation temperature was 30°C, the precipitation pH value was 5.0, and the precipitation was directly filtered after the precipitation was completed to obtain a pure rare earth-rich mother liquor, and then a sodium oxalate solution with a mass concentration of 12.5% was used to precipitate rare earths to obtain rare earth oxalate precipitates, which were calcined at 500°C for 1h to obtain mixed rare earth oxides, and the product purity was 98.51%. The process from rare earth ore to rare earth oxide products was realized, and the comprehensive recovery rate of rare earth was 75.22%.
[0042] The mixed rare earth oxide prepared in this example was subjected to X-ray diffraction analysis, and the XRD pattern is shown in Figure 2 As shown in Figure 2, mixed rare earth oxides are mainly light rare earth oxides, such as NdO2 and Ce 0.5 Nd 0.5 O 1.75 .
[0043] Comparative Example 1
[0044] Sampling was performed according to the particle size of the ore sample of -124μm. 30g of rare earth ore with a high iron content (iron oxide content of 13.8%) was taken and directly mixed with sulfuric acid with a volume concentration of 90%. The ratio of roasting agent to mixed rare earth ore was 0.8mL / g, the roasting temperature was 700℃, and the roasting time was 45min to obtain the roasted rare earth ore. The roasted rare earth ore was mixed with a sodium citrate solution with a mass concentration of 5% for leaching, the leaching temperature was 90℃, the leaching time was 3h, the leaching agent was 20mL / g to obtain a rare earth-rich mother liquor, and the leaching rate of rare earth was 81.66%. Sodium carbonate with a mass concentration of 49.7% is used as a precipitant for precipitation and impurity removal. The precipitation temperature is 30°C and the precipitation pH value is 5.0. After the precipitation is completed, the pure rare earth-rich mother liquor is directly filtered, and then a sodium oxalate solution with a mass concentration of 12.5% is used to precipitate rare earth to obtain rare earth oxalate precipitate, which is calcined at 500°C for 1h to obtain mixed rare earth oxides with a product purity of 80.41%. The comprehensive recovery rate of rare earth is 50.59%.
[0045] Comparative Example 2
[0046] Sampling was performed according to the particle size of the ore sample of -124μm. 30g of rare earth ore with low iron content (iron oxide content of 1.2%) was taken and directly mixed with sulfuric acid with a volume concentration of 90%. The ratio of roasting agent to mixed rare earth ore was 0.8mL / g, the roasting temperature was 700℃, and the roasting time was 30min to obtain the roasted rare earth ore. The roasted rare earth ore was mixed with distilled water for leaching, the leaching temperature was 90℃, the leaching time was 4h, the ratio of leaching agent to ore sample was 50mL / g, and a rare earth-rich mother liquor was obtained, and the rare earth leaching rate was 75.11%.
[0047] Comparative Example 3
[0048] Sampling was performed according to the particle size of the ore sample of -124μm. 30g of rare earth ore with high iron content (iron oxide content of 13.8%) was taken and directly mixed with ammonium sulfate, sodium sulfate, sodium oxalate, ammonium chloride, magnesium chloride, sodium chloride or ammonium citrate, the ratio of roasting agent to mixed rare earth ore was 1:1, the roasting temperature was 700℃, the roasting time was 30min, and the roasted rare earth ore was obtained. The roasted rare earth ore was mixed with a sodium citrate solution with a mass concentration of 5% for leaching, the leaching temperature was 90℃, the leaching time was 3h, the ratio of leaching agent to ore sample was 20mL / g, and a rare earth-rich mother liquor was obtained. The rare earth leaching rate of ammonium sulfate roasting was about 50%; the rare earth leaching rates of the other reagents were all less than 30%.
[0049] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for recovering rare earths from fine-particle sedimentary clay rock type rare earth ore, characterized in that: The steps include: (1) Calcination: crushing and grinding the fine-particle sedimentary clay rock type rare earth ore, mixing it with a calcining agent, and calcining it to obtain a calcined rare earth ore; (2) Leaching: Leaching rare earths from the roasted rare earth ore using a leaching agent to obtain a rare earth-rich mother liquor; (3) precipitation and impurity removal: the rare earth-rich mother liquor is impurity-removed by using an impurity-removing agent to obtain an aluminum-rich precipitate and a rare earth-rich mother liquor after impurity removal; (4) Precipitating rare earths: using a precipitant to precipitate rare earths from the rare earth-rich mother liquor after impurities removal to obtain a rare earth-rich precipitate; (5) Calcination: Calcinate the rare earth-rich precipitate to obtain mixed rare earth oxides.
2. The method for recovering rare earths from fine-particle sedimentary clay rock type rare earth ore according to claim 1, characterized in that: The rare earth content of the fine particle-grade sedimentary clay rock type rare earth ore is 0.05% to 2.50%.
3. The method for recovering rare earths from fine-particle sedimentary clay rock type rare earth ore according to claim 1, characterized in that: In step (1), the particle size of the rare earth ore after crushing and grinding is -160 μm to -75 μm.
4. The method for recovering rare earths from fine-particle sedimentary clay rock type rare earth ore according to claim 1, characterized in that: When the iron content of the fine-particle sedimentary clay rock type rare earth ore is higher than 1.5%, an acidic reagent is required to remove the iron before mixing with the roasting reagent; the acidic reagent is at least one of hydrochloric acid, nitric acid and sulfuric acid; the concentration of the acidic reagent is 0.5-4 mol / L; during the process of removing iron with the acidic reagent, the acidification temperature is 40-90°C, the acidification time is 0.5-2h, and the ratio of the acidic reagent to the ore sample is 10-40mL / g.
5. The method for recovering rare earths from fine-particle sedimentary clay rock type rare earth ore according to claim 1, characterized in that: In step (1), the roasting agent is at least one of sulfuric acid, ammonium sulfate, sodium sulfate, sodium oxalate, ammonium chloride, magnesium chloride, sodium chloride and ammonium citrate. Preferably, the roasting agent is sulfuric acid or ammonium sulfate with a volume concentration of 60 to 98%; the ratio of the roasting agent sulfuric acid to the rare earth ore is 0.4 to 2 mL / g, and the mass ratio of the remaining roasting agents to the rare earth ore is 3:1 to 1:3; the roasting temperature is 300 to 800°C, and the roasting time is 5 to 55 min.
6. The method for recovering rare earth from fine-particle sedimentary clay rock type rare earth ore according to claim 1, characterized in that: In step (2), the leaching agent is an aqueous solution of at least one of sodium chloride, sodium citrate and ammonium chloride; the mass concentration of the leaching agent is 1 to 20%; the leaching temperature is 50 to 90° C., the leaching time is 3 to 6 hours; and the ratio of the leaching agent to the rare earth ore is 10 to 30 mL / g.
7. The method for recovering rare earth from fine-particle sedimentary clay rock type rare earth ore according to claim 1, characterized in that: In step (3), the impurity remover is at least one of sodium carbonate, sodium bicarbonate, sodium hydroxide, ammonia water and sodium sulfide; the mass concentration of the impurity remover is 7.8-49.7%; the temperature during the impurity removal process is 5-40° C., the pH value is 4.5-5.5, the impurity removal process is continuously stirred, and the filtration is completed 0-30 minutes after the precipitation is completed.
8. The method for recovering rare earths from fine-particle sedimentary clay rock type rare earth ore according to claim 1, characterized in that: The aluminum-rich precipitate of step (3) is calcined to obtain aluminum-rich oxide; the calcination temperature is 700-900° C., and the calcination time is 0.5-2 h.
9. The method for recovering rare earths from fine-particle sedimentary clay rock type rare earth ore according to claim 1, characterized in that: In step (4), the precipitant is at least one of oxalic acid, ammonium oxalate and sodium oxalate, and the mass concentration of the precipitant is 6 to 12.5%.
10. The method for recovering rare earths from fine-particle sedimentary clay rock type rare earth ore according to claim 1, characterized in that: In step (5), the calcination temperature is 500-900° C. and the calcination time is 0.5-1 h.
Citation Information
Patent Citations
Method for selectively leaching sedimentary type rare earths
CN109266839A
Method for recovering sedimentary rare earth through hot high acid direct leaching process
CN114134348A
Method for leaching rare earth from basalt weathered crust
CN115058609A
Smelting method of iron rich mengite rare-earth mine
CN101363079A
Method for removing iron and enriching nickel cobalt through precipitation of laterite type nickel ores