Ni3Al reinforced medium-entropy alloy bonded tungsten alloy and preparation method thereof
By introducing Ni3Al reinforced phase into the medium-entropy alloy bonded tungsten alloy and adopting high-energy ball milling and discharge plasma sintering processes, the problems of high sintering temperature and coarse grains of tungsten alloy are solved, and the mechanical properties and density of tungsten alloy are significantly improved. Achieve 'double high' performance with high hardness and high strength.
Patent Information
- Application Number
- CN202411290343.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-12-06
AI Technical Summary
In terms of improving mechanical properties, existing medium-entropy alloys have problems such as excessive sintering temperature, coarse tungsten grains and low bending resistance, which is difficult to further improve the overall performance of the alloy.
Ni3Al is introduced as the reinforced phase of the bonded tungsten alloy of the medium-entropy alloy. Through high-energy ball milling and discharge plasma sintering processes, W-VCoNi-Ni3Al alloy is prepared, and the low melting point and good fluidity of the VCoNi medium-entropy alloy and the mechanical activation of Ni3Al are used. Achieve the superposition effect of multiple strengthening methods and improve the mechanical properties of tungsten alloys.
The comprehensive mechanical properties of tungsten alloys are significantly improved, including reduced sintering temperature, fine tungsten grains, high relative density, and increased hardness and strength, which solves the shortcomings in mechanical properties of tungsten alloys.
Smart Images

Figure CN119082579A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of tungsten alloy materials, and particularly relates to a Ni3Al reinforced medium entropy alloy bonded tungsten alloy and a preparation method thereof. Background Art
[0002] Tungsten heavy alloy, also commonly known as tungsten alloy, is a two-phase composite material composed of tungsten phase and binder phase. It is used in oil drilling, aerospace, medical, national defense and military industries due to its high density, high strength, high melting point, good wear resistance, good processability and high radiation absorption. The pursuit of higher comprehensive mechanical properties, especially higher strength, has always been one of the main research goals in the field of tungsten alloys. At present, the use of new binder phases and modification through alloying elements are important means to improve the mechanical properties of tungsten alloys.
[0003] In recent years, the research on multi-component alloys containing multiple elements has attracted increasing attention. Due to the existence of high mixing entropy effect, slow diffusion effect, lattice distortion effect, and multi-element harmonic effect, high entropy alloys and medium entropy alloys with excellent properties such as high strength, high hardness, high work hardening, high wear resistance, and high temperature stability have attracted much attention. Among them, medium entropy alloys are generally alloys formed by three metal elements in an equiatomic ratio or a near-equiatomic ratio, and their cost is lower than that of high entropy alloys. However, the performance of medium entropy alloys is similar to that of high entropy alloys. Therefore, the preparation of fine-grained tungsten alloys with excellent mechanical properties using medium entropy alloys as the bonding phase has attracted people's attention. At present, tungsten alloys with high entropy alloys / medium entropy alloys as the bonding phase show excellent compressive strength and hardness, but there are also problems such as too high alloy sintering temperature, coarse sintered alloy tungsten grains, and low bending resistance. At present, although tungsten alloys with medium entropy alloys as the bonding phase often show excellent strength and hardness, whether the mechanical properties of the alloy can be further improved on this basis is still a question.
[0004] Therefore, it is very important to introduce other strengthening phases (such as intermetallic compounds) into the medium-entropy alloy-bonded tungsten alloy, and then improve the comprehensive performance of the medium-entropy alloy-bonded tungsten alloy with excellent mechanical properties to a higher level through the synergistic coupling of multiple strengthening methods, so as to obtain a "double-high" mechanical property tungsten alloy with higher hardness and higher strength. Summary of the invention
[0005] In view of the shortcomings and deficiencies of the above prior art, the primary purpose of the present invention is to provide a Ni3Al-reinforced medium entropy alloy bonded tungsten alloy. In view of the problems existing in medium entropy alloy bonded tungsten alloy, the present invention proposes a new intermetallic compound-reinforced medium entropy alloy bonded tungsten alloy technology, that is, by introducing Ni3Al as a strengthening phase of medium entropy alloy bonded tungsten alloy, the comprehensive performance of medium entropy alloy bonded tungsten alloy with excellent mechanical properties is improved to a new level, and finally a "double high" mechanical property tungsten alloy with high hardness and high strength is obtained.
[0006] Another object of the present invention is to provide a method for preparing Ni3Al reinforced medium entropy alloy bonded tungsten alloy.
[0007] The purpose of the present invention is achieved through the following technical solutions:
[0008] A Ni3Al reinforced medium entropy alloy bonded tungsten alloy comprises a W matrix, a VCoNi medium entropy alloy bonding phase and a Ni3Al reinforcement phase, wherein the content of the W matrix is 85-95wt%, the content of the VCoNi medium entropy alloy bonding phase is 4-10wt%, the content of the Ni3Al reinforcement phase is 1-5wt%, and the element molar ratio of V, Co and Ni in the VCoNi medium entropy alloy bonding phase is 1:1:1.
[0009] Preferably, the relative density of the Ni3Al reinforced medium entropy alloy bonded tungsten alloy is greater than 95%, the macroscopic hardness is greater than 72HRA, and the bending strength is greater than or equal to 1500MPa.
[0010] Further preferably, the content of the W matrix is 90wt%, the content of the VCoNi medium entropy alloy bonding phase is 8wt%, and the content of the Ni3Al strengthening phase is 2wt%; the relative density of the Ni3Al reinforced medium entropy alloy bonded tungsten alloy is >98%, the macro hardness is >73HRA, and the bending strength is >1900MPa.
[0011] A method for preparing a Ni3Al reinforced medium entropy alloy bonded tungsten alloy comprises the following preparation steps:
[0012] (1) high-energy ball milling V, Co, and Ni single-element powders to obtain VCoNi medium-entropy alloy powder;
[0013] (2) high-energy ball milling the original Ni3Al powder to obtain activated Ni3Al powder;
[0014] (3) ball milling the VCoNi medium entropy alloy powder, activated Ni3Al powder and W powder to obtain a composite powder;
[0015] (4) The obtained composite powder is subjected to spark plasma sintering to obtain Ni3Al reinforced medium entropy alloy bonded tungsten alloy.
[0016] Furthermore, the average particle size of the V, Co, and Ni single-element powders in step (1) is ≤20 μm; the average particle size of the VCoNi entropy alloy powder is ≤30 μm; the average particle size of the Ni3Al powder in step (2) is ≤40 μm; and the average particle size of the W powder in step (3) is ≤5 μm.
[0017] Furthermore, in step (1), the molar ratio of the added V, Co and Ni single substance powders is 1:1:1.
[0018] Furthermore, in the composite powder in step (3), the content of VCoNi entropy alloy powder is 4-10wt%, the content of Ni3Al powder is 1-5wt%, and the content of W powder is 85-95wt%.
[0019] Furthermore, the high-energy ball milling in step (1) and step (2) is dry ball milling; the ball-to-material ratio of the high-energy ball milling is 10 to 20:1, the ball mill speed is 200 to 500 r / min, and the ball milling time is 20 to 30 h.
[0020] Further preferably, the high-energy ball milling in step (1) and step (2) is intermittent ball milling, wherein a single operation time is 30 to 60 minutes and a stop time is 5 to 20 minutes.
[0021] Furthermore, the ball milling mixing in step (3) is carried out with or without adding grinding balls; the mixing method with adding grinding balls is specifically as follows: VCoNi medium entropy alloy powder, Ni3Al powder, W powder and grinding balls are placed in a ball mill, and mixed for 10 to 30 hours at a ball-to-material ratio not exceeding 10:1 and a ball mill speed not exceeding 400 r / min; the mixing method without adding grinding balls is specifically as follows: VCoNi medium entropy alloy powder, Ni3Al powder and W powder are placed in a ball mill, and mixed for 10 to 30 hours at a ball mill speed not exceeding 400 r / min.
[0022] Furthermore, the spark plasma sintering in step (4) is a one-step sintering method; the air pressure in the furnace of the one-step sintering method is 10-50 Pa, the temperature is 1100-1300° C., the sintering pressure is 30-100 MPa, the heating rate is 100-400° C. / min, and the insulation time is 1-30 min.
[0023] The principle of the present invention is: first, the single powders of vanadium, cobalt and nickel are converted into VCoNi medium entropy alloy powder and mechanically activated Ni3Al powder by high-energy ball milling, and then they are evenly mixed with tungsten powder, and finally high-performance W-VCoNi-Ni3Al alloy is obtained by spark plasma sintering. The present invention adopts a specific VCoNi medium entropy alloy powder as a bonding phase, which has a low melting point, good fluidity in the molten state, and good adaptability with tungsten powder, and can achieve low-temperature sintering and promote low-temperature densification of the alloy. In addition, the introduction of mechanically activated Ni3Al powder as a reinforcing phase can produce more strengthening methods. Through the superposition effect of multiple strengthening methods, a fine-grained tungsten alloy with better comprehensive mechanical properties than a single medium entropy alloy bonded tungsten alloy can be prepared.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] (1) The present invention selects VCoNi medium entropy alloy with good mechanical properties and relatively low price as the bonding phase, which can reduce the preparation cost of high entropy alloy bonding tungsten alloy, and has the same effect as high entropy alloy bonding tungsten alloy. The obtained Ni3Al reinforced medium entropy alloy bonding tungsten alloy has the characteristics of low sintering temperature, fine tungsten grains, high relative density, high hardness / strength, etc., and the comprehensive mechanical properties have been significantly improved compared with previous studies.
[0026] (2) The formation of face-centered cubic (Ni, Co) solid solution during the high-energy ball milling process of the present invention and the diffusion of W and V atoms into the solid solution during the sintering process lead to solid solution strengthening, which is beneficial to improving the mechanical properties of the alloy. At the same time, due to the addition of mechanically activated Ni3Al powder, a (W, Al) solid solution is formed during the sintering process, and the resulting solid solution strengthening is also beneficial to further improving the mechanical properties of the tungsten alloy.
[0027] (3) The surface oxidation of the metal V powder during the ball milling and sintering process of the present invention can form a vanadium oxide phase inside and between the tungsten grains, and the formation of an aluminum oxide phase during the sintering process can hinder the dissolution-precipitation process of tungsten, thereby inhibiting the growth of tungsten grains and causing fine grain strengthening. It can also pin and hinder dislocation movement and slow down crack propagation, thereby helping to improve the comprehensive mechanical properties of tungsten alloys. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 The XRD pattern of the VCoNi medium entropy alloy powder prepared by high energy ball milling in Example 1;
[0029] Figure 2 The DSC graph of the VCoNi medium entropy alloy powder prepared by high energy ball milling in Example 1;
[0030] Figure 3 is the XRD pattern of Ni3Al activated powder milled by high energy ball milling in Example 1;
[0031] Figure 4 The BSE image and EDS Mapping image of the W-VCoNi-Ni3Al alloy prepared in Example 1;
[0032] Figure 5 TEM image and EDS Mapping image of the W-VCoNi-Ni3Al alloy prepared in Example 1. DETAILED DESCRIPTION
[0033] The present invention is further described in detail below in conjunction with embodiments and drawings, but the embodiments of the present invention are not limited thereto.
[0034] Example 1
[0035] 1. Raw materials:
[0036] The purity of W powder is greater than 99.9%, the purity of V powder is greater than 99.9%, the purity of Co powder is greater than 99.9%, the purity of Ni powder is greater than 99.9%, and the purity of Ni3Al powder is greater than 99.9%. The average particle size of W powder is 3μm. The average particle size of V powder, Co powder, and Ni powder is ≤20μm. The average particle size of Ni3Al powder is ≤40μm.
[0037] 2. Preparation:
[0038] (1) V powder, Co powder, and Ni powder (corresponding mass fractions of 30.22 wt%, 34.96 wt%, and 34.82 wt%, respectively) with an element molar ratio of 1:1:1 were loaded into a ball mill and dry-milled on a high-energy ball mill with a ball-to-material ratio of 10:1, a single running time of 1 h, and an intermittent time of 10 min. After ball milling at a speed of 300 r / min for 24 h, VCoNi medium-entropy alloy powder was obtained.
[0039] (2) The Ni3Al powder was loaded into a ball mill and dry-milled on a high-energy ball mill, wherein the ball-to-material ratio was 10:1, the single operation time was 1 h, the intermittent time was 10 min, and after ball milling at a speed of 300 r / min for 24 h, activated Ni3Al powder was obtained.
[0040] (3) The obtained VCoNi medium entropy alloy powder, activated Ni3Al powder and W powder were mixed in a ball mill according to a certain mass fraction (W powder: 90wt%, VCoNi: 8wt%, Ni3Al: 2wt%), with a ball-to-material ratio of 5:1, a ball mill speed of 300r / min, and a ball milling time of 24h to obtain a uniform tungsten alloy composite powder.
[0041] (4) After the composite powder is loaded into a graphite mold, it is placed in a spark plasma sintering system heating chamber, and after vacuuming, spark plasma one-step liquid phase sintering is performed; the sintering process conditions are: sintering vacuum degree <30Pa, sintering pressure is 40MPa, heating rate is 100℃ / min, sintering temperature is 1275℃, and holding time is 5min; pulse voltage is 4.5V, single power-on time of pulse voltage is 300ms, and single interruption time is 20ms. After the above sintering, a W-VCoNi-Ni3Al alloy with uniform structure is obtained.
[0042] The W-VCoNi-Ni3Al alloy obtained in this embodiment has an average tungsten grain size of less than 5 μm, a relative density of greater than 98%, a macroscopic hardness of 73.10 HRA, and a bending strength of 1990.19 MPa.
[0043] The phase analysis of the obtained VCoNi medium entropy alloy powder was carried out using an X-ray diffractometer (XRD, smartlab, RIGAKU, Japan). Figure 1 As shown in the figure, after 24 hours of high-energy ball milling, VCoNi medium-entropy alloy powder with face-centered cubic (fcc) (Ni, Co) solid solution and V-σ-rich phase was obtained. Differential scanning calorimetry (TGA / DSC3 + , Mettler Toledo Switzerland) analyzed the thermal effect of VCoNi medium entropy alloy powder during heating. The results are as follows Figure 2 As shown in the figure, the melting point of the medium entropy alloy powder is 1246°C, which is much lower than the melting points of single metals V, Co and Ni. The XRD pattern of the Ni3Al activated powder prepared by high-energy ball milling in step (2) is shown in Figure 3 shown.
[0044] The surface of the sintered tungsten alloy was characterized by scanning electron microscopy (FE-SEM, Verios G4 UC, Thermo Scientific, USA). The BSE images and their corresponding EDS element distribution results are shown in Figure 4 As can be seen from the figure, the W grains in the alloy are evenly distributed, and the grains are obviously spheroidized. From the element distribution diagram, it can be seen that V and Al oxides are generated in the alloy. The fine structure of the tungsten alloy was characterized by transmission electron microscopy (TEM, FEI, Talos, F200X, USA). The results are shown in Figure 5 It was found that the Al atoms of Ni3Al in the sintered alloy diffused into W to form an (Al, W) solid solution, and the Ni atoms and Co atoms dissolved in each other to form a (Ni, Co) solid solution.
[0045] Example 2
[0046] 1. Raw materials:
[0047] The purity of W powder is greater than 99.9%, the purity of V powder is greater than 99.9%, the purity of Co powder is greater than 99.9%, the purity of Ni powder is greater than 99.9%, and the purity of Ni3Al powder is greater than 99.9%. The average particle size of W powder is 3μm. The average particle size of V powder, Co powder, and Ni powder is ≤20μm. The average particle size of Ni3Al powder is ≤40μm.
[0048] 2. Preparation:
[0049] (1) V powder, Co powder, and Ni powder (corresponding mass fractions of 30.22 wt%, 34.96 wt%, and 34.82 wt%, respectively) with an element molar ratio of 1:1:1 were loaded into a ball mill and dry-milled on a high-energy ball mill with a ball-to-material ratio of 10:1, a single running time of 1 h, and an intermittent time of 10 min. After ball milling at a speed of 300 r / min for 24 h, VCoNi medium-entropy alloy powder was obtained.
[0050] (2) The Ni3Al powder was loaded into a ball mill and dry-milled on a high-energy ball mill, wherein the ball-to-material ratio was 10:1, the single operation time was 1 h, the intermittent time was 10 min, and after ball milling at a speed of 300 r / min for 24 h, activated Ni3Al powder was obtained.
[0051] (3) The obtained VCoNi medium entropy alloy powder, activated Ni3Al powder and W powder were mixed in a ball mill according to a certain mass fraction (W powder: 90wt%, VCoNi: 8wt%, Ni3Al: 2wt%), with a ball-to-material ratio of 5:1, a ball mill speed of 300r / min, and a ball milling time of 24h to obtain a uniform tungsten alloy composite powder.
[0052] (4) After the composite powder is loaded into a graphite mold, it is placed in a spark plasma sintering system heating chamber, and after vacuuming, spark plasma one-step liquid phase sintering is performed; the sintering process conditions are: sintering vacuum degree <30Pa, sintering pressure is 40MPa, heating rate is 100℃ / min, sintering temperature is 1150℃, and holding time is 5min; pulse voltage is 4.5V, single power-on time of pulse voltage is 300ms, and single interruption time is 20ms. After the above sintering, a W-VCoNi-Ni3Al alloy with uniform structure is obtained.
[0053] The W-VCoNi-Ni3Al alloy obtained in this embodiment has a relative density greater than 96%, a macroscopic hardness of 78.30HRA, and a bending strength of 1125.22MPa.
[0054] Example 3
[0055] 1. Raw materials:
[0056] The purity of W powder is greater than 99.9%, the purity of V powder is greater than 99.9%, the purity of Co powder is greater than 99.9%, the purity of Ni powder is greater than 99.9%, and the purity of Ni3Al powder is greater than 99.9%. The average particle size of W powder is 3μm. The average particle size of V powder, Co powder, and Ni powder is ≤20μm. The average particle size of Ni3Al powder is ≤40μm.
[0057] 2. Preparation:
[0058] (1) V powder, Co powder, and Ni powder (corresponding mass fractions of 30.22 wt%, 34.96 wt%, and 34.82 wt%, respectively) with an element molar ratio of 1:1:1 were loaded into a ball mill and dry-milled on a high-energy ball mill with a ball-to-material ratio of 10:1, a single running time of 1 h, and an intermittent time of 10 min. After ball milling at a speed of 300 r / min for 24 h, VCoNi medium-entropy alloy powder was obtained.
[0059] (2) The Ni3Al powder was loaded into a ball mill and dry-milled on a high-energy ball mill, wherein the ball-to-material ratio was 10:1, the single operation time was 1 h, the intermittent time was 10 min, and after ball milling at a speed of 300 r / min for 24 h, activated Ni3Al powder was obtained.
[0060] (3) The obtained VCoNi medium entropy alloy powder, activated Ni3Al powder and W powder were mixed in a ball mill according to a certain mass fraction (W powder: 90wt%, VCoNi: 8wt%, Ni3Al: 2wt%), with a ball-to-material ratio of 5:1, a ball mill speed of 300r / min, and a ball milling time of 24h to obtain a uniform tungsten alloy composite powder.
[0061] (4) After the composite powder is loaded into a graphite mold, it is placed in a spark plasma sintering system heating chamber, and after vacuuming, spark plasma one-step liquid phase sintering is performed; the sintering process conditions are: sintering vacuum degree <30Pa, sintering pressure is 40MPa, heating rate is 100℃ / min, sintering temperature is 1200℃, and holding time is 5min; pulse voltage is 4.5V, single power-on time of pulse voltage is 300ms, and single interruption time is 20ms. After the above sintering, a W-VCoNi-Ni3Al alloy with uniform structure is obtained.
[0062] The W-VCoNi-Ni3Al alloy obtained in this embodiment has a relative density greater than 97%, a macroscopic hardness of 77.10HRA, and a bending strength of 1281.78MPa.
[0063] Example 4
[0064] 1. Raw materials:
[0065] The purity of W powder is greater than 99.9%, the purity of V powder is greater than 99.9%, the purity of Co powder is greater than 99.9%, the purity of Ni powder is greater than 99.9%, and the purity of Ni3Al powder is greater than 99.9%. The average particle size of W powder is 3μm. The average particle size of V powder, Co powder, and Ni powder is ≤20μm. The average particle size of Ni3Al powder is ≤40μm.
[0066] 2. Preparation:
[0067] (1) V powder, Co powder, and Ni powder (corresponding mass fractions of 30.22 wt%, 34.96 wt%, and 34.82 wt%, respectively) with an element molar ratio of 1:1:1 were loaded into a ball mill and dry-milled on a high-energy ball mill with a ball-to-material ratio of 10:1, a single running time of 1 h, and an intermittent time of 10 min. After ball milling at a speed of 300 r / min for 24 h, VCoNi medium-entropy alloy powder was obtained.
[0068] (2) The Ni3Al powder was loaded into a ball mill and dry-milled on a high-energy ball mill, wherein the ball-to-material ratio was 10:1, the single operation time was 1 h, the intermittent time was 10 min, and after ball milling at a speed of 300 r / min for 24 h, activated Ni3Al powder was obtained.
[0069] (3) The obtained VCoNi medium entropy alloy powder, activated Ni3Al powder and W powder were mixed in a ball mill according to a certain mass fraction (W powder: 90wt%, VCoNi: 8wt%, Ni3Al: 2wt%), with a ball-to-material ratio of 5:1, a ball mill speed of 300r / min, and a ball milling time of 24h to obtain a uniform tungsten alloy composite powder.
[0070] (4) After the composite powder is loaded into a graphite mold, it is placed in a spark plasma sintering system heating chamber, and after vacuuming, spark plasma one-step liquid phase sintering is performed; the sintering process conditions are: sintering vacuum degree <30Pa, sintering pressure is 40MPa, heating rate is 100℃ / min, sintering temperature is 1250℃, and holding time is 5min; pulse voltage is 4.5V, single power-on time of pulse voltage is 300ms, and single interruption time is 20ms. After the above sintering, a W-VCoNi-Ni3Al alloy with uniform structure is obtained.
[0071] The W-VCoNi-Ni3Al alloy obtained in this embodiment has a relative density greater than 97%, a macroscopic hardness of 76.00HRA, and a bending strength of 1645.5MPa.
[0072] Example 5
[0073] 1. Raw materials:
[0074] The purity of W powder is greater than 99.9%, the purity of V powder is greater than 99.9%, the purity of Co powder is greater than 99.9%, the purity of Ni powder is greater than 99.9%, and the purity of Ni3Al powder is greater than 99.9%. The average particle size of W powder is 3μm. The average particle size of V powder, Co powder, and Ni powder is ≤20μm. The average particle size of Ni3Al powder is ≤40μm.
[0075] 2. Preparation:
[0076] (1) V powder, Co powder, and Ni powder (corresponding mass fractions of 30.22 wt%, 34.96 wt%, and 34.82 wt%, respectively) with an element molar ratio of 1:1:1 were loaded into a ball mill and dry-milled on a high-energy ball mill with a ball-to-material ratio of 10:1, a single running time of 1 h, and an intermittent time of 10 min. After ball milling at a speed of 300 r / min for 24 h, VCoNi medium-entropy alloy powder was obtained.
[0077] (2) The Ni3Al powder was loaded into a ball mill and dry-milled on a high-energy ball mill, wherein the ball-to-material ratio was 10:1, the single operation time was 1 h, the intermittent time was 10 min, and after ball milling at a speed of 300 r / min for 24 h, activated Ni3Al powder was obtained.
[0078] (3) The obtained VCoNi medium entropy alloy powder, activated Ni3Al powder and W powder were mixed in a ball mill according to a certain mass fraction (W powder: 90wt%, VCoNi: 8wt%, Ni3Al: 2wt%), with a ball-to-material ratio of 5:1, a ball mill speed of 300r / min, and a ball milling time of 24h to obtain a uniform tungsten alloy composite powder.
[0079] (4) After the composite powder is loaded into a graphite mold, it is placed in a spark plasma sintering system heating chamber, and after vacuuming, spark plasma one-step liquid phase sintering is performed; the sintering process conditions are: sintering vacuum degree <30Pa, sintering pressure is 40MPa, heating rate is 100℃ / min, sintering temperature is 1300℃, and holding time is 5min; pulse voltage is 4.5V, single power-on time of pulse voltage is 300ms, and single interruption time is 20ms. After the above sintering, a W-VCoNi-Ni3Al alloy with uniform structure is obtained.
[0080] The W-VCoNi-Ni3Al alloy obtained in this embodiment has a relative density greater than 97%, a macroscopic hardness of 72.40HRA, and a bending strength of 1931.69MPa.
[0081] Example 6
[0082] 1. Raw materials:
[0083] The purity of W powder is greater than 99.9%, the purity of V powder is greater than 99.9%, the purity of Co powder is greater than 99.9%, the purity of Ni powder is greater than 99.9%, and the purity of Ni3Al powder is greater than 99.9%. The average particle size of W powder is 3μm. The average particle size of V powder, Co powder, and Ni powder is ≤20μm. The average particle size of Ni3Al powder is ≤40μm.
[0084] 2. Preparation:
[0085] (1) V powder, Co powder, and Ni powder (corresponding mass fractions of 30.22 wt%, 34.96 wt%, and 34.82 wt%, respectively) with an element molar ratio of 1:1:1 were loaded into a ball mill and dry-milled on a high-energy ball mill with a ball-to-material ratio of 10:1, a single running time of 1 h, and an intermittent time of 10 min. After ball milling at a speed of 300 r / min for 24 h, VCoNi medium-entropy alloy powder was obtained.
[0086] (2) The Ni3Al powder was loaded into a ball mill and dry-milled on a high-energy ball mill, wherein the ball-to-material ratio was 10:1, the single operation time was 1 h, the intermittent time was 10 min, and after ball milling at a speed of 300 r / min for 24 h, activated Ni3Al powder was obtained.
[0087] (3) The obtained VCoNi medium entropy alloy powder, activated Ni3Al powder and W powder are mixed in a ball mill according to a certain mass fraction (W powder: 95wt%, VCoNi: 4wt%, Ni3Al: 1wt%), wherein the ball-to-material ratio is 5:1, the ball mill speed is 300r / min, and the ball milling time is 24h to obtain a uniform tungsten alloy composite powder.
[0088] (4) After the composite powder is loaded into a graphite mold, it is placed in a spark plasma sintering system heating chamber, and after vacuuming, spark plasma one-step liquid phase sintering is performed; the sintering process conditions are: sintering vacuum degree <30Pa, sintering pressure is 40MPa, heating rate is 100℃ / min, sintering temperature is 1275℃, and holding time is 5min; pulse voltage is 4.5V, single power-on time of pulse voltage is 300ms, and single interruption time is 20ms. After the above sintering, a W-VCoNi-Ni3Al alloy with uniform structure is obtained.
[0089] The W-VCoNi-Ni3Al alloy obtained in this embodiment has a relative density greater than 98%, a macroscopic hardness of 74.30HRA, and a bending strength of 1874.63MPa.
[0090] Example 7
[0091] 1. Raw materials:
[0092] The purity of W powder is greater than 99.9%, the purity of V powder is greater than 99.9%, the purity of Co powder is greater than 99.9%, the purity of Ni powder is greater than 99.9%, and the purity of Ni3Al powder is greater than 99.9%. The average particle size of W powder is 3μm. The average particle size of V powder, Co powder, and Ni powder is ≤20μm. The average particle size of Ni3Al powder is ≤40μm.
[0093] 2. Preparation:
[0094] (1) V powder, Co powder, and Ni powder (corresponding mass fractions of 30.22 wt%, 34.96 wt%, and 34.82 wt%, respectively) with an element molar ratio of 1:1:1 were loaded into a ball mill and dry-milled on a high-energy ball mill with a ball-to-material ratio of 10:1, a single running time of 1 h, and an intermittent time of 10 min. After ball milling at a speed of 300 r / min for 24 h, VCoNi medium-entropy alloy powder was obtained.
[0095] (2) The Ni3Al powder was loaded into a ball mill and dry-milled on a high-energy ball mill, wherein the ball-to-material ratio was 10:1, the single operation time was 1 h, the intermittent time was 10 min, and after ball milling at a speed of 300 r / min for 24 h, activated Ni3Al powder was obtained.
[0096] (3) The obtained VCoNi medium entropy alloy powder, activated Ni3Al powder and W powder were mixed in a ball mill according to a certain mass fraction (W powder: 85wt%, VCoNi: 10wt%, Ni3Al: 5wt%), with a ball-to-material ratio of 5:1, a ball mill speed of 300r / min, and a ball milling time of 24h to obtain a uniform tungsten alloy composite powder.
[0097] (4) After the composite powder is loaded into a graphite mold, it is placed in a spark plasma sintering system heating chamber, and after vacuuming, spark plasma one-step liquid phase sintering is performed; the sintering process conditions are: sintering vacuum degree <30Pa, sintering pressure is 40MPa, heating rate is 100℃ / min, sintering temperature is 1275℃, and holding time is 5min; pulse voltage is 4.5V, single power-on time of pulse voltage is 300ms, and single interruption time is 20ms. After the above sintering, a W-VCoNi-Ni3Al alloy with uniform structure is obtained.
[0098] The W-VCoNi-Ni3Al alloy obtained in this embodiment has a relative density greater than 97%, a macroscopic hardness of 72.59 HRA, and a bending strength of 1726.39 MPa.
[0099] Comparative Example 1
[0100] Compared with Example 1, in this comparative example, after V powder, Co powder and Ni powder are prepared by high-energy ball milling to prepare VCoNi medium entropy alloy powder, a small amount of activated Ni3Al powder is not added, but the tungsten alloy is directly prepared by mixing with W powder. The specific preparation steps are as follows:
[0101] 1. Raw materials:
[0102] The purity of W powder is greater than 99.9%, the purity of V powder is greater than 99.9%, the purity of Co powder is greater than 99.9%, and the purity of Ni powder is greater than 99.9%. The average particle size of W powder is 3μm. The average particle size of V powder, Co powder, and Ni powder is ≤20μm.
[0103] 2. Preparation:
[0104] (1) V powder, Co powder, and Ni powder (corresponding mass fractions of 30.22 wt%, 34.96 wt%, and 34.82 wt%, respectively) in a molar ratio of 1:1:1 were loaded into a ball mill and dry-milled on a high-energy ball mill with a ball-to-material ratio of 10:1, a single running time of 1 h, and an intermittent time of 10 min. After ball milling at a speed of 300 r / min for 24 h, VCoNi medium-entropy alloy powder was obtained.
[0105] (2) The obtained VCoNi medium entropy alloy powder and W powder are mixed in a ball mill according to a certain mass fraction (W powder: 90wt%, VCoNi: 10wt%), wherein the ball-to-material ratio is 10:1, the ball mill speed is 300r / min, and the ball milling time is 24h to obtain a uniform tungsten alloy composite powder.
[0106] (3) After the uniform tungsten alloy composite powder is loaded into a graphite mold, it is placed in a heating chamber of a spark plasma sintering system, and after vacuuming, spark plasma one-step liquid phase sintering is performed; the sintering process conditions are: sintering vacuum degree <30Pa, sintering pressure is 40MPa, heating rate is 100℃ / min, sintering temperature is 1275℃, and holding time is 5min; pulse voltage is 4.5V, single power-on time of pulse voltage is 300ms, and single interruption time is 20ms. After the above sintering, W-VCoNi alloy is obtained.
[0107] The W-VCoNi alloy prepared in this comparative example and not containing a small amount of Ni3Al has a relative density greater than 96%, a macroscopic hardness of 71.30 HRA, and a bending strength of 1883.00 MPa.
[0108] Comparative Example 2
[0109] Compared with Example 1, in this comparative example, V powder, Co powder and Ni powder were not pre-milled by high-energy ball milling to prepare VCoNi medium entropy alloy powder, but were directly mixed with W powder and activated Ni3Al powder to prepare tungsten alloy. The specific preparation steps are as follows:
[0110] 1. Raw materials:
[0111] The purity of W powder is greater than 99.9%, the purity of V powder is greater than 99.9%, the purity of Co powder is greater than 99.9%, the purity of Ni powder is greater than 99.9%, and the purity of Ni3Al powder is greater than 99.9%. The average particle size of W powder is 3μm. The average particle size of V powder, Co powder, and Ni powder is ≤20μm. The average particle size of Ni3Al powder is ≤40μm.
[0112] 2. Preparation:
[0113] (1) Ni3Al powder was loaded into a ball mill with a ball-to-material ratio of 10:1, and dry-milled on a high-energy ball mill with a ball-to-material ratio of 10:1, a single operation time of 1 h, and an intermittent time of 10 min. After ball milling at a speed of 300 r / min for 24 h, activated Ni3Al powder was obtained.
[0114] (2) W powder, V powder, Co powder, Ni powder and activated Ni3Al powder were loaded into a ball mill according to a certain mass fraction (W powder: 90wt%, V: 2.42wt%, Co: 2.80wt%, Ni: 2.78wt%, Ni3Al: 2wt%) and a ball-to-material ratio of 5:1. Intermittent mixing was performed on a ball mill at a speed of 300r / min for 24h, wherein the single running time was 1h and the stop time was 10min, thereby obtaining a tungsten alloy composite powder.
[0115] (3) After the composite powder is loaded into a graphite mold, it is placed in a spark plasma sintering system heating chamber, and after vacuuming, spark plasma one-step liquid phase sintering is performed; the sintering process conditions are: sintering vacuum degree <30Pa, sintering pressure is 40MPa, heating rate is 100℃ / min, sintering temperature is 1275℃, and holding time is 5min; pulse voltage is 4.5V, single pulse voltage power-on time is 300ms, and single interruption time is 20ms. After the above sintering, W-(V-Co-Ni)-Ni3Al alloy is obtained.
[0116] The W-(V-Co-Ni)-Ni3Al alloy obtained in this comparative example has a macroscopic hardness of 70.80HRA, but there are a large number of pores on the bending fracture surface of the alloy, the relative density is low (92%), and the bending strength is greatly reduced (1356.21MPa).
[0117] Comparative Example 3
[0118] Compared with Example 1, V powder, Co powder, Ni powder and Ni3Al powder in this comparative example are not pre-milled by high-energy ball milling to prepare VCoNi medium entropy alloy powder and activated Ni3Al powder, but are directly mixed with W powder to prepare tungsten alloy. The specific preparation steps are as follows: 1. Raw materials:
[0119] The purity of W powder is greater than 99.9%, the purity of V powder is greater than 99.9%, the purity of Co powder is greater than 99.9%, the purity of Ni powder is greater than 99.9%, and the purity of Ni3Al powder is greater than 99.9%. The average particle size of W powder is 3μm. The average particle size of V powder, Co powder, and Ni powder is ≤20μm. The average particle size of Ni3Al powder is ≤40μm.
[0120] 2. Preparation:
[0121] (1) W powder, V powder, Co powder, Ni powder and Ni3Al powder were loaded into a ball mill according to a certain mass fraction (W powder: 90wt%, V: 2.42wt%, Co: 2.80wt%, Ni: 2.78wt%, Ni3Al: 2wt%) and a ball-to-material ratio of 5:1. Intermittent mixing was performed on a ball mill at a speed of 300r / min for 24h, wherein the single running time was 1h and the stop time was 10min, thereby obtaining a composite powder.
[0122] (2) After the composite powder is loaded into a graphite mold, it is placed in a spark plasma sintering system heating chamber, and after vacuuming, spark plasma one-step liquid phase sintering is performed; the sintering process conditions are: sintering vacuum degree <30Pa, sintering pressure is 40MPa, heating rate is 100℃ / min, sintering temperature is 1275℃, and holding time is 5min; pulse voltage is 4.5V, single pulse voltage power-on time is 300ms, and single interruption time is 20ms. After the above sintering, W-(V-Co-Ni)-Ni3Al alloy is obtained.
[0123] The W-(V-Co-Ni)-Ni3Al alloy obtained in this comparative example has a macroscopic hardness of 68.53 HRA, but the relative density of the alloy is low (90%), and the bending strength is significantly reduced (1127.45 MPa).
[0124] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A Ni3Al reinforced medium entropy alloy bonded tungsten alloy, characterized in that: The invention comprises a W matrix, a VCoNi medium entropy alloy bonding phase and a Ni3Al reinforcement phase, wherein the content of the W matrix is 85-95wt%, the content of the VCoNi medium entropy alloy bonding phase is 4-10wt%, the content of the Ni3Al reinforcement phase is 1-5wt%, and the molar ratio of V, Co and Ni in the VCoNi medium entropy alloy bonding phase is 1:1:
1.
2. The Ni3Al reinforced medium entropy alloy bonded tungsten alloy according to claim 1, characterized in that: The relative density of the Ni3Al reinforced medium entropy alloy bonded tungsten alloy is greater than 95%, the macroscopic hardness is greater than 72HRA, and the bending strength is greater than or equal to 1500MPa.
3. The Ni3Al reinforced medium entropy alloy bonded tungsten alloy according to claim 1, characterized in that: The content of the W matrix is 90wt%, the content of the VCoNi medium entropy alloy bonding phase is 8wt%, and the content of the Ni3Al reinforcement phase is 2wt%; the relative density of the Ni3Al reinforced medium entropy alloy bonding tungsten alloy is greater than 98%, the macroscopic hardness is greater than 73HRA, and the bending strength is greater than 1900MPa.
4. A method for preparing a Ni3Al reinforced medium entropy alloy bonded tungsten alloy, characterized in that: The method comprises the following preparation steps: (1) high-energy ball milling V, Co, and Ni single-element powders to obtain VCoNi medium-entropy alloy powder; (2) high-energy ball milling the Ni3Al powder to obtain activated Ni3Al powder; (3) ball milling the VCoNi medium entropy alloy powder, activated Ni3Al powder and W powder to obtain a composite powder; (4) The obtained composite powder is subjected to spark plasma sintering to obtain Ni3Al reinforced medium entropy alloy bonded tungsten alloy.
5. The method for preparing a Ni3Al reinforced medium entropy alloy bonded tungsten alloy according to claim 4, characterized in that: The average particle size of the V, Co, and Ni single-substance powders in step (1) is ≤20 μm; the average particle size of the VCoNi entropy alloy powder is ≤30 μm; the average particle size of the Ni3Al powder in step (2) is ≤40 μm; the average particle size of the W powder in step (3) is ≤5 μm.
6. The method for preparing a Ni3Al reinforced medium entropy alloy bonded tungsten alloy according to claim 4, characterized in that: The molar ratio of the elements added to the V, Co and Ni single substance powders in step (1) is 1:1:1; the content of the VCoNi entropy alloy powder in the composite powder in step (3) is 4-10wt%, the content of Ni3Al powder is 1-5wt%, and the content of W powder is 85-95wt%.
7. The method for preparing a Ni3Al reinforced medium entropy alloy bonded tungsten alloy according to claim 4, characterized in that: The high-energy ball milling in step (1) and step (2) is dry ball milling; the ball-to-material ratio of the high-energy ball milling is 10 to 20:1, the ball mill speed is 200 to 500 r / min, and the ball milling time is 20 to 30 h.
8. The method for preparing a Ni3Al reinforced medium entropy alloy bonded tungsten alloy according to claim 4, characterized in that: The high-energy ball milling in step (1) and step (2) is intermittent ball milling, wherein a single operation time is 30 to 60 minutes and a stop time is 5 to 20 minutes.
9. The method for preparing a Ni3Al reinforced medium entropy alloy bonded tungsten alloy according to claim 4, characterized in that: The ball milling mixing in step (3) is carried out with or without adding grinding balls; the mixing method with adding grinding balls is specifically as follows: VCoNi medium entropy alloy powder, Ni3Al powder, W powder and grinding balls are placed in a ball mill, and the mixing is carried out for 10 to 30 hours at a ball-to-material ratio not exceeding 10:1 and a ball mill speed not exceeding 400 r / min; the mixing method without adding grinding balls is specifically as follows: VCoNi medium entropy alloy powder, Ni3Al powder and W powder are placed in a ball mill, and the mixing is carried out for 10 to 30 hours at a ball mill speed not exceeding 400 r / min.
10. The method for preparing a Ni3Al reinforced medium entropy alloy bonded tungsten alloy according to claim 4, characterized in that: The spark plasma sintering in step (4) is a one-step sintering method; the air pressure in the furnace of the one-step sintering method is 10-50 Pa, the temperature is 1100-1300° C., the sintering pressure is 30-100 MPa, the heating rate is 100-400° C. / min, and the insulation time is 1-30 min.