B2O3 modified medium-entropy alloy bonded tungsten alloy and preparation method thereof
By introducing trace B2O3 into the tungsten bonded alloy of medium entropy alloy and adopting high-energy ball milling and discharge plasma sintering technology, the problem of improving the mechanical properties of medium entropy alloy is solved, and the "double high" mechanics of high hardness and high strength is achieved performance and reduce preparation costs.
Patent Information
- Application Number
- CN202411290464.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-12-06
AI Technical Summary
There is room for improvement in the mechanical properties of existing medium-entropy alloys, especially in terms of strength, and it is difficult to significantly improve.
By introducing trace amounts of B2O3 as an additive, combined with high-energy ball milling and discharge plasma sintering technology, a B2O3-modified medium-entropy alloy bonded tungsten alloy was prepared, and the superposition effect of various strengthening methods was used to improve the mechanical properties of the alloy.
The hardness and strength of the tungsten alloy are significantly improved, the "double high" mechanical properties are achieved, the preparation cost is reduced, and the sintering temperature is low, the tungsten grains are small, and the relative density is high.
Smart Images

Figure CN119082580A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of tungsten alloy materials, and particularly relates to a B2O3 modified medium entropy alloy bonded tungsten alloy and a preparation method thereof. Background Art
[0002] Tungsten alloy is a two-phase composite material with tungsten as the matrix and low melting point metal as the bonding phase. Due to its high density, high strength, high melting point, good wear resistance and high radiation absorption, tungsten alloy is widely used in different fields such as oil drilling, aerospace, medical and military. For tungsten alloy, the pursuit of higher mechanical properties, especially higher strength, is one of the main research goals in the field of tungsten alloy. Among various tungsten alloy strengthening methods, the use of new bonding phases and the addition of trace additives to modify tungsten alloys have attracted people's attention.
[0003] In recent years, high entropy alloys and medium entropy alloys have attracted much attention due to their excellent mechanical properties and multi-component design. Their emergence has also provided a new choice for the bonding phase of tungsten alloys. High entropy alloys or medium entropy alloys are generally composed of elements in equiatomic ratios or near-equiatomic ratios, and have unique properties such as high strength, good ductility, corrosion resistance, wear resistance and oxidation resistance. Therefore, they are considered to be one of the most promising materials for future applications. Compared with high entropy alloys, medium entropy alloys contain fewer types of metal elements, and their cost is lower than that of high entropy alloys, but their performance is similar to that of high entropy alloys. Therefore, it is more cost-effective to use medium entropy alloys as bonding phases to prepare tungsten alloys with excellent mechanical properties. At present, tungsten alloys with medium entropy alloys as bonding phases often show excellent strength and hardness, but whether the mechanical properties (especially strength) of the alloys can be further significantly improved on this basis remains a question.
[0004] Therefore, it is very important to introduce other trace metal oxides (such as B2O3) as additives into the medium-entropy alloy-bonded tungsten alloy, and then further improve the comprehensive mechanical properties of the medium-entropy alloy-bonded tungsten alloy through the superposition effect of multiple strengthening methods, so as to obtain a "double-high" mechanical property tungsten alloy with higher hardness and higher strength. Summary of the invention
[0005] In view of the shortcomings and deficiencies of the above prior art, the primary purpose of the present invention is to provide a B2O3 modified medium entropy alloy bonded tungsten alloy. In view of the problems existing in medium entropy alloy bonded tungsten alloy, the present invention proposes a technology of oxide modified medium entropy alloy bonded tungsten alloy, that is, by introducing a trace amount of B2O3 as an additive, the comprehensive mechanical properties of the medium entropy alloy bonded tungsten alloy with excellent mechanical properties are improved to a new level, and finally a "double high" mechanical property tungsten alloy with high hardness and high strength is obtained.
[0006] Another object of the present invention is to provide a method for preparing B2O3 modified medium entropy alloy bonded tungsten alloy.
[0007] The purpose of the present invention is achieved through the following technical solutions:
[0008] A B2O3 modified medium entropy alloy bonded tungsten alloy comprises a W matrix, a VCoNi medium entropy alloy bonding phase and a B2O3 modified phase, wherein the content of the W matrix is 85-95wt%, the content of the VCoNi medium entropy alloy bonding phase is 4.5-14.9wt%, the content of the B2O3 modified phase is 0.1-0.5wt%, and the element molar ratio of V, Co and Ni in the VCoNi medium entropy alloy bonding phase is 1:1:1.
[0009] Preferably, the relative density of the B2O3 modified medium entropy alloy bonded tungsten alloy is greater than 96%, the macroscopic hardness is greater than 71HRA, and the bending strength is greater than or equal to 1500MPa.
[0010] Further preferably, the content of the W matrix is 90wt%, the content of the VCoNi medium entropy alloy bonding phase is 9.7wt%, and the content of the B2O3 modified phase is 0.3wt%; the relative density of the B2O3 modified medium entropy alloy bonding tungsten alloy is >98%, the macro hardness is >73HRA, and the bending strength is >2200MPa.
[0011] A method for preparing a B2O3 modified medium entropy alloy bonded tungsten alloy comprises the following preparation steps:
[0012] (1) high-energy ball milling V, Co, and Ni single-element powders to obtain VCoNi medium-entropy alloy powder;
[0013] (2) ball milling the VCoNi medium entropy alloy powder, B2O3 powder and W powder to obtain a composite powder;
[0014] (3) The obtained composite powder is subjected to spark plasma sintering to obtain B2O3 modified medium entropy alloy bonded tungsten alloy.
[0015] Furthermore, the average particle size of the V, Co, and Ni single-element powders in step (1) is ≤20 μm; the average particle size of the VCoNi entropy alloy powder is ≤30 μm; the average particle size of the B2O3 powder in step (2) is ≤5 μm; and the average particle size of the W powder in step (3) is ≤5 μm.
[0016] Furthermore, in step (1), the molar ratio of the added V, Co and Ni single substance powders is 1:1:1.
[0017] Furthermore, in the composite powder in step (3), the content of the VCoNi entropy alloy powder is 4.5-14.9wt%, the content of the B2O3 powder is 0.1-0.5wt%, and the content of the W powder is 85-95wt%.
[0018] Furthermore, the high-energy ball milling in step (1) is dry ball milling; the ball-to-material ratio of the high-energy ball milling is 10 to 20:1, the ball mill speed is 200 to 500 r / min, and the ball milling time is 20 to 30 h.
[0019] Further preferably, the high-energy ball milling in step (1) is intermittent ball milling, wherein a single operation time is 30 to 60 minutes and a stop time is 5 to 20 minutes.
[0020] Furthermore, the ball milling mixing in step (2) is carried out with or without adding grinding balls; the mixing method with adding grinding balls is specifically as follows: VCoNi medium entropy alloy powder, B2O3 powder, W powder and grinding balls are placed in a ball mill, and mixed for 10 to 30 hours at a ball-to-material ratio not exceeding 10:1 and a ball mill speed not exceeding 400 r / min; the mixing method without adding grinding balls is specifically as follows: VCoNi medium entropy alloy powder, B2O3 powder and W powder are placed in a ball mill, and mixed for 10 to 30 hours at a ball mill speed not exceeding 400 r / min.
[0021] Furthermore, the spark plasma sintering in step (3) is a one-step sintering method; the air pressure in the furnace of the one-step sintering method is 10-50 Pa, the temperature is 1100-1300° C., the sintering pressure is 30-100 MPa, the heating rate is 100-400° C. / min, and the holding time is 1-30 min.
[0022] The principle of the present invention is: first, the single powders of vanadium, cobalt and nickel are converted into VCoNi medium entropy alloy powder by high-energy ball milling, and then the powder is evenly mixed with tungsten powder and B2O3 powder, and finally a high-performance W-VCoNi-B2O3 alloy is obtained by spark plasma sintering. The present invention adopts a specific VCoNi medium entropy alloy powder as a bonding phase, which has a low melting point, good fluidity in the molten state, and good compatibility with tungsten powder, and can achieve low-temperature sintering and promote low-temperature densification of the alloy. In addition, the introduction of B2O3 powder as a modified phase can produce more strengthening mechanisms. Through the superposition effect of multiple strengthening methods, a fine-grained tungsten alloy with better comprehensive mechanical properties than a single medium entropy alloy bonded tungsten alloy can be prepared.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] (1) The present invention selects VCoNi medium entropy alloy with good mechanical properties and relatively low price as the bonding phase, which can reduce the preparation cost of high entropy alloy bonding tungsten alloy, and has the same effect as high entropy alloy bonding tungsten alloy. The obtained B2O3 modified medium entropy alloy bonding tungsten alloy has the characteristics of low sintering temperature, fine tungsten grains, high relative density, high hardness / strength, etc., and the comprehensive mechanical properties have been significantly improved compared with previous studies.
[0025] (2) The formation of face-centered cubic (Ni, Co) solid solution during the high-energy ball milling process of the present invention and the diffusion of W and V atoms into the solid solution during the sintering process lead to the solid solution strengthening of the bonding phase, which is beneficial to improving the mechanical properties of the alloy. At the same time, during the sintering process, some V, Co, and Ni atoms also diffuse into the W matrix to form a (W, V, Co, Ni) solid solution. The resulting matrix solid solution strengthening is also beneficial to further improving the mechanical properties of the tungsten alloy.
[0026] (3) During the ball milling and sintering process of the present invention, the surface of the metal V powder is oxidized to form a vanadium oxide phase in the tungsten alloy, which can hinder the dissolution-precipitation process of tungsten, thereby inhibiting the growth of tungsten grains and causing fine grain strengthening. It can also pin and hinder dislocation movement and slow down crack propagation, thereby helping to improve the comprehensive mechanical properties of the tungsten alloy.
[0027] (4) The present invention introduces a trace amount of B2O3 into the tungsten alloy composite raw material powder. After ball milling and subsequent sintering, the B2O3 particles are dispersed in the W matrix and bonding phase of the alloy, resulting in dispersion strengthening. Therefore, the W matrix and bonding phase can be further strengthened on the basis of the original solid solution strengthening. The superposition of multiple strengthening methods is conducive to further improving the mechanical properties of the alloy. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 The XRD pattern of the VCoNi medium entropy alloy powder prepared by high energy ball milling in Example 1;
[0029] Figure 2 The DSC graph of the VCoNi medium entropy alloy powder prepared by high energy ball milling in Example 1;
[0030] Figure 3 is the BSE diagram of the W-VCoNi-B2O3 alloy prepared in Example 1;
[0031] Figure 4 TEM image and EDS Mapping image of the W-VCoNi-B2O3 alloy prepared in Example 1. DETAILED DESCRIPTION
[0032] The present invention is further described in detail below in conjunction with embodiments and drawings, but the embodiments of the present invention are not limited thereto.
[0033] Example 1
[0034] 1. Raw materials:
[0035] The purity of W powder is greater than 99.9%, the purity of V powder is greater than 99.9%, the purity of Co powder is greater than 99.9%, the purity of Ni powder is greater than 99.9%, and the purity of B2O3 powder is greater than 99.8%. The average particle size of W powder is 3μm. The average particle size of V powder, Co powder, and Ni powder is ≤20μm. The average particle size of B2O3 powder is ≤5μm.
[0036] 2. Preparation:
[0037] (1) V powder, Co powder, and Ni powder (corresponding mass fractions of 30.22 wt%, 34.96 wt%, and 34.82 wt%, respectively) with an element molar ratio of 1:1:1 were loaded into a ball mill and dry-milled on a high-energy ball mill with a ball-to-material ratio of 10:1, a single running time of 1 h, and an intermittent time of 10 min. After ball milling at a speed of 300 r / min for 24 h, VCoNi medium-entropy alloy powder was obtained.
[0038] (2) The obtained VCoNi medium entropy alloy powder, B2O3 powder and W powder are mixed in a ball mill according to a certain mass fraction (W powder: 90wt%, VCoNi: 9.7wt%, B2O3: 0.3wt%), wherein the ball-to-material ratio is 5:1, the ball mill speed is 300r / min, and the ball milling time is 24h to obtain a uniform tungsten alloy composite powder.
[0039] (3) After the composite powder is loaded into a graphite mold, it is placed in a spark plasma sintering system heating chamber, and after vacuuming, spark plasma one-step liquid phase sintering is performed; the sintering process conditions are: sintering vacuum degree <30Pa, sintering pressure is 40MPa, heating rate is 100℃ / min, sintering temperature is 1275℃, and holding time is 5min; pulse voltage is 4.5V, single pulse voltage power-on time is 300ms, and single interruption time is 20ms. After the above sintering, a W-VCoNi-B2O3 alloy with uniform structure is obtained.
[0040] The W-VCoNi-B2O3 alloy obtained in this embodiment has an average tungsten grain size of less than 1.5 μm, a relative density of greater than 98%, a macroscopic hardness of 73.50 HRA, and a bending strength of 2205.27 MPa.
[0041] The phase analysis of the obtained VCoNi medium entropy alloy powder was carried out using an X-ray diffractometer (XRD, smartlab, RIGAKU, Japan). Figure 1As shown in the figure, after 24 hours of high-energy ball milling, VCoNi medium-entropy alloy powder with face-centered cubic (fcc) (Ni, Co) solid solution and V-σ-rich phase was obtained. Differential scanning calorimetry (TGA / DSC3 + , Mettler Toledo Switzerland) analyzed the thermal effect of VCoNi medium entropy alloy powder during heating. The results are as follows Figure 2 As shown in the figure, the melting point of the medium entropy alloy powder is 1246°C, which is much lower than the melting points of single metals V, Co and Ni.
[0042] The surface of the sintered tungsten alloy was characterized by scanning electron microscopy (FE-SEM, Verios G4 UC, Thermo Scientific, USA). Figure 3 As can be seen from the figure, the W grains in the alloy are small and evenly distributed, and the grains are obviously spheroidized. The fine structure of the tungsten alloy was characterized by transmission electron microscopy (TEM, FEI, Talos, F200X, USA). Figure 4 As shown in the figure, some V, Co, and Ni atoms in the binder phase diffuse into the W matrix to form a (W, V, Co, Ni) solid solution, and at the same time, W and V elements also diffuse into the (Ni, Co) solid solution to form a (Ni, Co, V, W) solid solution. In addition, B2O3 is evenly dispersed in the binder phase and the W matrix.
[0043] Example 2
[0044] 1. Raw materials:
[0045] The purity of W powder is greater than 99.9%, the purity of V powder is greater than 99.9%, the purity of Co powder is greater than 99.9%, the purity of Ni powder is greater than 99.9%, and the purity of B2O3 powder is greater than 99.8%. The average particle size of W powder is 3μm. The average particle size of V powder, Co powder, and Ni powder is ≤20μm. The average particle size of B2O3 powder is ≤5μm.
[0046] 2. Preparation:
[0047] (1) V powder, Co powder, and Ni powder (corresponding mass fractions of 30.22 wt%, 34.96 wt%, and 34.82 wt%, respectively) with an element molar ratio of 1:1:1 were loaded into a ball mill and dry-milled on a high-energy ball mill with a ball-to-material ratio of 10:1, a single running time of 1 h, and an intermittent time of 10 min. After ball milling at a speed of 300 r / min for 24 h, VCoNi medium-entropy alloy powder was obtained.
[0048] (2) The obtained VCoNi medium entropy alloy powder, B2O3 powder and W powder are mixed in a ball mill according to a certain mass fraction (W powder: 90wt%, VCoNi: 9.7wt%, B2O3: 0.3wt%), wherein the ball-to-material ratio is 5:1, the ball mill speed is 300r / min, and the ball milling time is 24h to obtain a uniform tungsten alloy composite powder.
[0049] (3) After the composite powder is loaded into a graphite mold, it is placed in a spark plasma sintering system heating chamber, and after vacuuming, spark plasma one-step liquid phase sintering is performed; the sintering process conditions are: sintering vacuum degree <30Pa, sintering pressure is 40MPa, heating rate is 100℃ / min, sintering temperature is 1150℃, and holding time is 5min; pulse voltage is 4.5V, single pulse voltage power-on time is 300ms, and single interruption time is 20ms. After the above sintering, a W-VCoNi-B2O3 alloy with uniform structure is obtained.
[0050] The W-VCoNi-B2O3 alloy obtained in this embodiment has a relative density greater than 96%, a macroscopic hardness of 78.25 HRA, and a bending strength of 1241.00 MPa.
[0051] Example 3
[0052] 1. Raw materials:
[0053] The purity of W powder is greater than 99.9%, the purity of V powder is greater than 99.9%, the purity of Co powder is greater than 99.9%, the purity of Ni powder is greater than 99.9%, and the purity of B2O3 powder is greater than 99.8%. The average particle size of W powder is 3μm. The average particle size of V powder, Co powder, and Ni powder is ≤20μm. The average particle size of B2O3 powder is ≤5μm.
[0054] 2. Preparation:
[0055] (1) V powder, Co powder, and Ni powder (corresponding mass fractions of 30.22 wt%, 34.96 wt%, and 34.82 wt%, respectively) with an element molar ratio of 1:1:1 were loaded into a ball mill and dry-milled on a high-energy ball mill with a ball-to-material ratio of 10:1, a single running time of 1 h, and an intermittent time of 10 min. After ball milling at a speed of 300 r / min for 24 h, VCoNi medium-entropy alloy powder was obtained.
[0056] (2) The obtained VCoNi medium entropy alloy powder, B2O3 powder and W powder are mixed in a ball mill according to a certain mass fraction (W powder: 90wt%, VCoNi: 9.7wt%, B2O3: 0.3wt%), wherein the ball-to-material ratio is 5:1, the ball mill speed is 300r / min, and the ball milling time is 24h to obtain a uniform tungsten alloy composite powder.
[0057] (3) After the composite powder is loaded into a graphite mold, it is placed in a spark plasma sintering system heating chamber, and after vacuuming, spark plasma one-step liquid phase sintering is performed; the sintering process conditions are: sintering vacuum degree <30Pa, sintering pressure is 40MPa, heating rate is 100℃ / min, sintering temperature is 1200℃, and holding time is 5min; pulse voltage is 4.5V, single pulse voltage power-on time is 300ms, and single interruption time is 20ms. After the above sintering, a W-VCoNi-B2O3 alloy with uniform structure is obtained.
[0058] The W-VCoNi-B2O3 alloy obtained in this embodiment has a relative density greater than 96%, a macroscopic hardness of 76.42 HRA, and a bending strength of 1418.86 MPa.
[0059] Example 4
[0060] 1. Raw materials:
[0061] The purity of W powder is greater than 99.9%, the purity of V powder is greater than 99.9%, the purity of Co powder is greater than 99.9%, the purity of Ni powder is greater than 99.9%, and the purity of B2O3 powder is greater than 99.8%. The average particle size of W powder is 3μm. The average particle size of V powder, Co powder, and Ni powder is ≤20μm. The average particle size of B2O3 powder is ≤5μm.
[0062] 2. Preparation:
[0063] (1) V powder, Co powder, and Ni powder (corresponding mass fractions of 30.22 wt%, 34.96 wt%, and 34.82 wt%, respectively) with an element molar ratio of 1:1:1 were loaded into a ball mill and dry-milled on a high-energy ball mill with a ball-to-material ratio of 10:1, a single running time of 1 h, and an intermittent time of 10 min. After ball milling at a speed of 300 r / min for 24 h, VCoNi medium-entropy alloy powder was obtained.
[0064] (2) The obtained VCoNi medium entropy alloy powder, B2O3 powder and W powder are mixed in a ball mill according to a certain mass fraction (W powder: 90wt%, VCoNi: 9.7wt%, B2O3: 0.3wt%), wherein the ball-to-material ratio is 5:1, the ball mill speed is 300r / min, and the ball milling time is 24h to obtain a uniform tungsten alloy composite powder.
[0065] (3) After the composite powder is loaded into a graphite mold, it is placed in a spark plasma sintering system heating chamber, and after vacuuming, spark plasma one-step liquid phase sintering is performed; the sintering process conditions are: sintering vacuum degree <30Pa, sintering pressure is 40MPa, heating rate is 100℃ / min, sintering temperature is 1250℃, and holding time is 5min; pulse voltage is 4.5V, single pulse voltage power-on time is 300ms, and single interruption time is 20ms. After the above sintering, a W-VCoNi-B2O3 alloy with uniform structure is obtained.
[0066] The W-VCoNi-B2O3 alloy obtained in this embodiment has a relative density of 97%, a macroscopic hardness of 75.67HRA, and a bending strength of 1462.05MPa.
[0067] Example 5
[0068] 1. Raw materials:
[0069] The purity of W powder is greater than 99.9%, the purity of V powder is greater than 99.9%, the purity of Co powder is greater than 99.9%, the purity of Ni powder is greater than 99.9%, and the purity of B2O3 powder is greater than 99.8%. The average particle size of W powder is 3μm. The average particle size of V powder, Co powder, and Ni powder is ≤20μm. The average particle size of B2O3 powder is ≤5μm.
[0070] 2. Preparation:
[0071] (1) V powder, Co powder, and Ni powder (corresponding mass fractions of 30.22 wt%, 34.96 wt%, and 34.82 wt%, respectively) with an element molar ratio of 1:1:1 were loaded into a ball mill and dry-milled on a high-energy ball mill with a ball-to-material ratio of 10:1, a single running time of 1 h, and an intermittent time of 10 min. After ball milling at a speed of 300 r / min for 24 h, VCoNi medium-entropy alloy powder was obtained.
[0072] (2) The obtained VCoNi medium entropy alloy powder, B2O3 and W powder are mixed in a ball mill according to a certain mass fraction (W powder: 90wt%, VCoNi: 9.7wt%, B2O3: 0.3wt%), wherein the ball-to-material ratio is 5:1, the ball mill speed is 300r / min, and the ball milling time is 24h to obtain a uniform tungsten alloy composite powder.
[0073] (3) After the composite powder is loaded into a graphite mold, it is placed in a spark plasma sintering system heating chamber, and after vacuuming, spark plasma one-step liquid phase sintering is performed; the sintering process conditions are: sintering vacuum degree <30Pa, sintering pressure is 40MPa, heating rate is 100℃ / min, sintering temperature is 1300℃, and holding time is 5min; pulse voltage is 4.5V, single pulse voltage power-on time is 300ms, and single interruption time is 20ms. After the above sintering, a W-VCoNi-B2O3 alloy with uniform structure is obtained.
[0074] The W-VCoNi-B2O3 alloy obtained in this embodiment has a relative density greater than 100%, a macroscopic hardness of 71.85 HRA, and a bending strength of 1757.38 MPa.
[0075] Example 6
[0076] 1. Raw materials:
[0077] The purity of W powder is greater than 99.9%, the purity of V powder is greater than 99.9%, the purity of Co powder is greater than 99.9%, the purity of Ni powder is greater than 99.9%, and the purity of B2O3 powder is greater than 99.8%. The average particle size of W powder is 3μm. The average particle size of V powder, Co powder, and Ni powder is ≤20μm. The average particle size of B2O3 powder is ≤5μm.
[0078] 2. Preparation:
[0079] (1) V powder, Co powder, and Ni powder (corresponding mass fractions of 30.22 wt%, 34.96 wt%, and 34.82 wt%, respectively) with an element molar ratio of 1:1:1 were loaded into a ball mill and dry-milled on a high-energy ball mill with a ball-to-material ratio of 10:1, a single running time of 1 h, and an intermittent time of 10 min. After ball milling at a speed of 300 r / min for 24 h, VCoNi medium-entropy alloy powder was obtained.
[0080] (2) The obtained VCoNi medium entropy alloy powder, B2O3 and W powder are mixed in a ball mill according to a certain mass fraction (W powder: 95wt%, VCoNi: 4.5wt%, B2O3: 0.5wt%), wherein the ball-to-material ratio is 5:1, the ball mill speed is 300r / min, and the ball milling time is 24h to obtain a uniform tungsten alloy composite powder.
[0081] (3) After the composite powder is loaded into a graphite mold, it is placed in a spark plasma sintering system heating chamber, and after vacuuming, spark plasma one-step liquid phase sintering is performed; the sintering process conditions are: sintering vacuum degree <30Pa, sintering pressure is 40MPa, heating rate is 100℃ / min, sintering temperature is 1275℃, and holding time is 5min; pulse voltage is 4.5V, single pulse voltage power-on time is 300ms, and single interruption time is 20ms. After the above sintering, a W-VCoNi-B2O3 alloy with uniform structure is obtained.
[0082] The W-VCoNi-B2O3 alloy obtained in this embodiment has a relative density greater than 98%, a macroscopic hardness of 74.35 HRA, and a bending strength of 2081.76 MPa.
[0083] Example 7
[0084] 1. Raw materials:
[0085] The purity of W powder is greater than 99.9%, the purity of V powder is greater than 99.9%, the purity of Co powder is greater than 99.9%, the purity of Ni powder is greater than 99.9%, and the purity of B2O3 powder is greater than 99.8%. The average particle size of W powder is 3μm. The average particle size of V powder, Co powder, and Ni powder is ≤20μm. The average particle size of B2O3 powder is ≤5μm.
[0086] 2. Preparation:
[0087] (1) V powder, Co powder, and Ni powder (corresponding mass fractions of 30.22 wt%, 34.96 wt%, and 34.82 wt%, respectively) with an element molar ratio of 1:1:1 were loaded into a ball mill and dry-milled on a high-energy ball mill with a ball-to-material ratio of 10:1, a single running time of 1 h, and an intermittent time of 10 min. After ball milling at a speed of 300 r / min for 24 h, VCoNi medium-entropy alloy powder was obtained.
[0088] (2) The obtained VCoNi medium entropy alloy powder, B2O3 and W powder are mixed in a ball mill according to a certain mass fraction (W powder: 85wt%, VCoNi: 14.9wt%, B2O3: 0.1wt%), wherein the ball-to-material ratio is 5:1, the ball mill speed is 300r / min, and the ball milling time is 24h to obtain a uniform tungsten alloy composite powder.
[0089] (3) After the composite powder is loaded into a graphite mold, it is placed in a spark plasma sintering system heating chamber, and after vacuuming, spark plasma one-step liquid phase sintering is performed; the sintering process conditions are: sintering vacuum degree <30Pa, sintering pressure is 40MPa, heating rate is 100℃ / min, sintering temperature is 1275℃, and holding time is 5min; pulse voltage is 4.5V, single pulse voltage power-on time is 300ms, and single interruption time is 20ms. After the above sintering, a W-VCoNi-B2O3 alloy with uniform structure is obtained.
[0090] The W-VCoNi-B2O3 alloy obtained in this embodiment has a relative density greater than 97%, a macroscopic hardness of 72.96 HRA, and a bending strength of 1952.41 MPa.
[0091] Comparative Example 1
[0092] Compared with Example 1, in this comparative example, after V powder, Co powder and Ni powder are prepared by high-energy ball milling to prepare VCoNi medium entropy alloy powder, trace oxide B2O3 powder is not added, but directly mixed with W powder to prepare tungsten alloy. The specific preparation steps are as follows:
[0093] 1. Raw materials:
[0094] The purity of W powder is greater than 99.9%, the purity of V powder is greater than 99.9%, the purity of Co powder is greater than 99.9%, and the purity of Ni powder is greater than 99.9%. The average particle size of W powder is 3μm. The average particle size of V powder, Co powder, and Ni powder is ≤20μm.
[0095] 2. Preparation:
[0096] (1) V powder, Co powder, and Ni powder (corresponding mass fractions of 30.22 wt%, 34.96 wt%, and 34.82 wt%, respectively) in a molar ratio of 1:1:1 were loaded into a ball mill and dry-milled on a high-energy ball mill with a ball-to-material ratio of 10:1, a single running time of 1 h, and an intermittent time of 10 min. After ball milling at a speed of 300 r / min for 24 h, VCoNi medium-entropy alloy powder was obtained.
[0097] (2) The obtained VCoNi medium entropy alloy powder and W powder are mixed in a ball mill according to a certain mass fraction (W powder: 90wt%, VCoNi: 10wt%), wherein the ball-to-material ratio is 10:1, the ball mill speed is 300r / min, and the ball milling time is 24h to obtain a uniform tungsten alloy composite powder.
[0098] (3) After the uniform tungsten alloy composite powder is loaded into a graphite mold, it is placed in a heating chamber of a spark plasma sintering system, and after vacuuming, spark plasma one-step liquid phase sintering is performed; the sintering process conditions are: sintering vacuum degree <30Pa, sintering pressure is 40MPa, heating rate is 100℃ / min, sintering temperature is 1275℃, and holding time is 5min; pulse voltage is 4.5V, single power-on time of pulse voltage is 300ms, and single interruption time is 20ms. After the above sintering, W-VCoNi alloy is obtained.
[0099] The W-VCoNi alloy prepared in this comparative example and free of trace B2O3 has a relative density greater than 96%, a macroscopic hardness of 71.30 HRA, and a bending strength of 1883.00 MPa.
[0100] Comparative Example 2
[0101] Compared with Example 1, in this comparative example, V powder, Co powder and Ni powder are not pre-milled by high-energy ball milling to prepare VCoNi medium entropy alloy powder, but are directly mixed with trace oxide B2O3 powder and W powder to prepare tungsten alloy. The specific preparation steps are as follows:
[0102] 1. Raw materials:
[0103] The purity of W powder is greater than 99.9%, the purity of V powder is greater than 99.9%, the purity of Co powder is greater than 99.9%, the purity of Ni powder is greater than 99.9%, and the purity of B2O3 powder is greater than 99.8%. The average particle size of W powder is 3μm. The average particle size of V powder, Co powder, and Ni powder is ≤20μm. The average particle size of B2O3 powder is ≤5μm.
[0104] 2. Preparation:
[0105] (1) W powder, V powder, Co powder, Ni powder and B2O3 powder were loaded into a ball mill according to a certain mass fraction (W powder: 90wt%, V: 2.93wt%, Co: 3.39wt%, Ni: 3.38wt%, B2O3: 0.3wt%) and a ball-to-material ratio of 5:1. Intermittent mixing was performed on a ball mill at a speed of 300r / min for 24h, wherein the single running time was 1h and the stop time was 10min, thereby obtaining a composite powder.
[0106] (2) After the composite powder is loaded into a graphite mold, it is placed in a spark plasma sintering system heating chamber, and after vacuuming, spark plasma one-step sintering is performed; the sintering process conditions are: sintering vacuum degree <30Pa, sintering pressure is 40MPa, heating rate is 100℃ / min, sintering temperature is 1275℃, and holding time is 5min; pulse voltage is 4.5V, single pulse voltage power-on time is 300ms, and single interruption time is 20ms. After the above sintering, W-(V-Co-Ni)-B2O3 alloy is obtained.
[0107] The W-(V-Co-Ni)-B2O3 alloy obtained in this comparative example has a macroscopic hardness of 70.13 HRA, but the relative density of the alloy is low (91%) and the bending strength is significantly reduced (1254.86 MPa).
[0108] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications made without departing from the spirit and principles of the present invention shall be equivalent replacement methods and shall be included in the protection scope of the present invention.
Claims
1. A B 2 O 3 Modified medium entropy alloy bonded tungsten alloy, It is characterized in that It contains W matrix, VCoNi medium entropy alloy binder phase and B 2 O 3 The modified phase has a W matrix content of 85-95wt%, a VCoNi medium entropy alloy binder phase content of 4.5-14.9wt%, and a B 2 O 3 The content of the modified phase is 0.1-0.5wt%, and the molar ratio of V, Co and Ni in the VCoNi medium entropy alloy bonding phase is 1:1:
1.
2. A B according to claim 1 2 O 3 Modified medium entropy alloy bonded tungsten alloy, It is characterized in that B 2 O 3 The relative density of the modified medium entropy alloy bonded tungsten alloy is greater than 96%, the macroscopic hardness is greater than 71HRA, and the bending strength is greater than or equal to 1500MPa.
3. A B according to claim 1 2 O 3 Modified medium entropy alloy bonded tungsten alloy, It is characterized in that The content of the W matrix is 90wt%, the content of the entropy alloy binder phase in VCoNi is 9.7wt%, and the content of B 2 O 3 The modified phase content is 0.3wt%; the B 2 O 3 The relative density of the modified medium entropy alloy bonded tungsten alloy is greater than 98%, the macroscopic hardness is greater than 73HRA, and the bending strength is greater than 2200MPa.
4. A B 2 O 3 Preparation method of modified medium entropy alloy bonded tungsten alloy, It is characterized in that The method comprises the following preparation steps: (1) high-energy ball milling V, Co, and Ni single-element powders to obtain VCoNi medium-entropy alloy powder; (2) the VCoNi medium entropy alloy powder, B 2 O 3 The powder is mixed with W powder by ball milling to obtain composite powder; (3) The obtained composite powder is subjected to spark plasma sintering to obtain B 2 O 3 Modified medium entropy alloy bonded tungsten alloy.
5. A B according to claim 4 2 O 3 Preparation method of modified medium entropy alloy bonded tungsten alloy, It is characterized in that The average particle size of the V, Co, and Ni single-substance powders in step (1) is ≤20 μm; the average particle size of the VCoNi entropy alloy powder is ≤30 μm; the B in step (2) 2 O 3 The average particle size of the powder is ≤5 μm; the average particle size of the W powder in step (3) is ≤5 μm.
6. A B according to claim 4 2 O 3 Preparation method of modified medium entropy alloy bonded tungsten alloy, It is characterized in that The molar ratio of the added V, Co, and Ni single substance powders in step (1) is 1:1:1; the content of the entropy alloy powder in the VCoNi composite powder in step (2) is 4.5-14.9wt%, and B 2 O 3 The content of the powder is 0.1-0.5 wt %, and the content of the W powder is 85-95 wt %.
7. A B according to claim 4 2 O 3 Preparation method of modified medium entropy alloy bonded tungsten alloy, It is characterized in that The high-energy ball milling in step (1) is dry ball milling; the ball-to-material ratio of the high-energy ball milling is 10-20:1, the ball mill speed is 200-500 r / min, and the ball milling time is 20-30 h.
8. A B according to claim 4 2 O 3 Preparation method of modified medium entropy alloy bonded tungsten alloy, It is characterized in that The high-energy ball milling in step (1) is intermittent ball milling, wherein a single operation time is 30 to 60 minutes and a stop time is 5 to 20 minutes.
9. A B according to claim 4 2 O 3 Preparation method of modified medium entropy alloy bonded tungsten alloy, It is characterized in that The ball milling mixing in step (2) is carried out with or without adding grinding balls; the mixing method with adding grinding balls is specifically: VCoNi medium entropy alloy powder, B 2 O 3 The powder, W powder and grinding balls are put into a ball mill, and the materials are mixed for 10 to 30 hours at a ball-to-material ratio of no more than 10:1 and a ball mill speed of no more than 400 r / min; the mixing method without adding grinding balls is specifically as follows: VCoNi medium entropy alloy powder, B 2 O 3 The powder and W powder are put into a ball mill and mixed for 10 to 30 hours at a ball mill speed not exceeding 400 r / min.
10. A B according to claim 4 2 O 3 Preparation method of modified medium entropy alloy bonded tungsten alloy, It is characterized in that The spark plasma sintering in step (3) is a one-step sintering method; the air pressure in the furnace of the one-step sintering method is 10-50 Pa, the temperature is 1100-1300° C., the sintering pressure is 30-100 MPa, the heating rate is 100-400° C. / min, and the insulation time is 1-30 min.