Processing method of NM400 steel plate

By adjusting the element ratio and process flow of the NM400 steel plate, using three-stage heating and low-temperature tempering treatment, the problems of high cost and insufficient performance in the production of existing NM400 steel plates are solved, and the high hardness, strength and wear resistance of the steel plate are achieved Improvement.

CN119082592APending Publication Date: 2024-12-06HEBEI PUYANG IRON & STEEL
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411228046.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In the existing production methods of NM400 steel plates, high alloy composition design leads to high finished product costs, and the steel plates prepared by the tissue strengthening method have poor impact toughness and high deformation degree, large energy consumption, and low tensile strength.

Method used

Using low-carbon element design, improve the content of Cr element to refine the grain, add Ti and Cu elements to enhance tempering stability and strength, and optimize the steel plate through three-stage heating and two-stage cooling process, combined with low-temperature tempering treatment. Element proportions and process flow.

Benefits of technology

It improves the comprehensive performance of NM400 steel plate, including hardness, strength and wear resistance, while reducing production costs and energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082592A_ABST
    Figure CN119082592A_ABST
Patent Text Reader

Abstract

The invention provides a processing method of an NM400 steel plate, and belongs to the technical field of steel smelting. The preparation method comprises the following steps: firstly, smelting, refining and continuously casting raw materials to obtain a continuous casting billet, then carrying out heat treatment on the continuous casting billet by adopting a three-section heating method, and then rolling, cooling and tempering at low temperature to obtain the NM400 steel plate. The toughness of the steel plate is improved by adjusting the proportion of elements in the steel plate, adopting a three-stage heating and heat preservation treatment process and a two-stage cooling process, and finally, the hardness, strength and wear resistance of the steel plate are improved by adopting low-temperature tempering and selecting proper temperature and time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steel smelting, and in particular to a processing method of an NM400 steel plate. Background Art

[0002] Wear-resistant steel refers to a type of high-strength steel that is used in environments with severe surface wear. It is mainly used in vehicles or facilities that work in contact with materials such as ore, coal, coal slurry, mud and cement slurry for a long time, such as mining electric wheel dump trucks, coal mine scraper conveyors, cement mixers, bulldozers, excavators, loaders, etc. Among them, NM400 steel is a widely used wear-resistant steel.

[0003] Existing NM400 steel is mainly produced through two methods. One method adopts high alloy composition design to improve the strength, hardness and wear resistance of steel by alloying with higher contents of C, Ni, Cu, Mo, Cr and other elements, but the composition cost of this method is relatively high; the other method utilizes the organizational strengthening effect to obtain the martensitic structure through the offline quenching + tempering production process to improve the strength, hardness and wear resistance of steel, but the wear-resistant steel prepared by this method has poor impact toughness and large deformation degree. A strong quenching machine is required in production, and there are problems such as high energy consumption in the preparation process.

[0004] For example, Chinese patent CN114045444B discloses a NM400 grade DQ type martensitic wear-resistant steel plate and a preparation method thereof. The chemical composition and mass percentage of the steel plate prepared by the method are: C: 0.14-0.16%, Si: 0.25-0.30%, Mn: 1.00-1.40%, Mo: 0.20-0.25%, Cr: 0.20-0.25%, Ti: 0.010-0.015%, Nb: 0.025-0.030%, Ni: 0.20-0.25%, V: 0.0030-0.0040%, B: 0.0014-0.0016%, P≤0.010%, S≤0.003%, N≤0.005%, and the remainder is Fe and inevitable impurities; the wear-resistant steel plate is prepared by a heat treatment process of online quenching + offline tempering. However, the wear-resistant steel plate prepared by this method has low tensile strength.

[0005] Chinese patent CN107012396B discloses a microalloyed bainite / martensite multiphase NM400 steel plate and a preparation method thereof, wherein the steel plate is composed of the following chemical components by mass percentage: C: 0.1-0.25%, Si: 0.2-0.6%, Mn: 1.3-1.7%, P: ≤0.02%, S: ≤0.008%, Cr: 0.5-0.7%, Mo: 0.25-0.4%, Ni: 0.1-0.25%, Cu: 0.2-0.4%, V: 0.02-0.05%, Nb: 0.01-0.03%, B: 0.001-0.0025%, and the remainder is Fe and unavoidable impurity elements. This method forms a bainite / martensite complex phase structure after rolling, so the deformation of NM400 steel plate in production is small, the difficulty of later straightening is small, and there is no need for offline quenching treatment, no strong quenching equipment, low equipment cost, and low production difficulty. However, the steel plate prepared by this method has low hardness and low elongation.

[0006] Therefore, it is necessary to provide a processing method for NM400 steel plate to improve its comprehensive performance. Summary of the invention

[0007] Based on the problems existing in the prior art, the purpose of the present invention is to provide a processing method of NM400 steel plate, which has simple process, low production cost and good comprehensive performance of the prepared NM400 steel plate.

[0008] To achieve the above object, the technical solution adopted by the present invention is:

[0009] A method for processing a NM400 steel plate comprises the following steps:

[0010] (1) Smelting, refining and continuous casting: the raw materials are mixed and smelted in a converter, sent to an LF refining furnace for refining and vacuum treatment, and continuously cast to obtain a continuous casting billet;

[0011] (2) Heating of the ingot: The continuous casting ingot is heated to 1200-1300°C by a three-stage heating method and kept at this temperature for 4-5 hours;

[0012] (3) Rolling: The heated continuous casting billet is subjected to rough rolling and finish rolling to obtain a rolled steel plate;

[0013] (4) Cooling: The rolled steel plate is first water-cooled to 200-230°C, and then air-cooled to room temperature;

[0014] (5) Low temperature tempering to obtain the NM400 steel plate.

[0015] Preferably, the smelting temperature in step (1) is 1100-1200° C., and the smelting is carried out after being kept at this temperature for 60-120 minutes.

[0016] Preferably, the element content of the continuous casting billet in step (1) is:

[0017] C: 0.09~0.17%, Si: 0.2~0.6%, Mn: 1.1~1.5%, Cr: 0.3~0.4%, Ti: 0.1~0.45%, Cu: 0.05~0.2%, Al: 0.01~0.025; V: 0.2~0.3%, Nb: 0.01~0.03%, B: 0.001~0.0025%, P: ≤0.02%, S: ≤0.008%, the balance is iron and unavoidable impurities.

[0018] More preferably, the element content of the continuous casting billet in step (1) is:

[0019] C: 0.14%, Si: 0.6%, Mn: 1.29%, Cr: 0.37%, Ti: 0.32%, Cu: 0.13%, Al: 0.019%, V: 0.25%, Nb: 0.02%, B: 0.0017%, P: 0.009%, S: 0.007%, and the remainder is iron and inevitable impurities.

[0020] In the element design of the present invention, a low carbon content is adopted to improve the wear resistance of the alloy; the content of the Cr element is increased to refine the grains and improve the stability of the alloy; the Ti element is added to further refine the grains, increase the tempering stability of the quenched steel, and produce a secondary hardening effect; the Cu element is added to replace a part of the nickel element and improve the strength of the steel; and a small amount of the Al element is added to refine the grains and improve the impact toughness.

[0021] Preferably, the specifications of the continuous casting billet in step (1) are 250-300 mm thick, 1500-1600 mm wide and 2300-1500 mm long.

[0022] Preferably, the specific method for heating the ingot in step (2) is: first, heating to 500-550°C at a rate of 2-3°C / min, and keeping warm for 2-3 hours; then heating to 1000-1150°C at a rate of 1-3°C / min; keeping warm for 2-4 hours; finally, heating to 1200-1300°C, and keeping warm for 4-5 hours.

[0023] Preferably, the starting rolling temperature of the rough rolling in step (3) is 1150-1200° C., the final rolling temperature is 850-900° C., and the rolling is performed in 4-5 passes, with a single pass reduction rate of 30%-40%.

[0024] Preferably, the start rolling temperature of the finishing rolling in step (3) is 950-1000°C, the final rolling temperature is 750-800°C, and the rolling is performed in 3-4 passes, with a single pass reduction rate of 10%-20%.

[0025] Preferably, the temperature of the low-temperature tempering in step (5) is 180-230° C., and the time is 2-3 hours.

[0026] Compared with the prior art, the present invention has the following beneficial effects: the present invention provides a processing method for NM400 steel plate, which improves the toughness of the steel plate by adjusting the ratio of elements in the steel plate, adopting a three-stage heating and heat preservation treatment process, and a two-stage cooling process. Finally, low-temperature tempering is adopted, and the appropriate temperature and time are selected to improve the hardness, strength and wear resistance of the steel plate. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 The figure is a process flow chart of the NM400 steel plate processing method of the present invention. DETAILED DESCRIPTION

[0028] The present invention will be further described below in conjunction with the embodiments.

[0029] Example 1

[0030] A method for processing NM400 steel plate, the steps are as follows:

[0031] (1) Smelting, refining and continuous casting: The raw materials were mixed and smelted in a converter at a smelting temperature of 1120°C. The raw materials were kept warm for 100 min before being taken out of the converter. The raw materials were then sent to an LF refining furnace for refining and vacuum treatment, and then continuously cast (refining and continuous casting were both performed using conventional processes) to obtain a continuous casting billet with a thickness of 250 mm, a width of 1500 mm and a length of 2300 mm. The element contents of the continuous casting billet are as follows:

[0032] C: 0.14%, Si: 0.6%, Mn: 1.29%, Cr: 0.37%, Ti: 0.32%, Cu: 0.13%, Al: 0.019%, V: 0.25%, Nb: 0.02%, B: 0.0017%, P: 0.009%, S: 0.007%, the balance is iron and unavoidable impurities;

[0033] (2) Heating of the casting: First, heat the continuous casting to 550°C at a rate of 3°C / min and keep it at that temperature for 2.5 hours; then heat it to 1100°C at a rate of 2°C / min and keep it at that temperature for 3 hours; finally, heat it to 1250°C and keep it at that temperature for 4.5 hours;

[0034] (3) Rough rolling: the starting rolling temperature is 1180°C, the final rolling temperature is 880°C, and the rolling is performed in 5 passes, with a single pass reduction rate of 30% to 40%;

[0035] (4) Finish rolling: the starting rolling temperature is 970°C, the final rolling temperature is 780°C, and the rolling is performed in three passes, with a single pass reduction rate of 10% to 20% to obtain a steel plate with a thickness of 10 mm;

[0036] (5) Cooling: The rolled steel plate is water-cooled to 210°C and then air-cooled to room temperature;

[0037] (6) The steel plate is heated to 190° C. for low temperature tempering, kept at this temperature for 3 hours, and air-cooled to obtain the NM400 steel plate.

[0038] Example 2

[0039] A processing method of NM400 steel plate, the steps are as follows:

[0040] (1) Smelting, refining and continuous casting: The raw materials were mixed and smelted in a converter at a smelting temperature of 1120°C. The raw materials were kept warm for 100 min before being taken out of the converter. The raw materials were then sent to an LF refining furnace for refining and vacuum treatment, and then continuously cast (refining and continuous casting were both processed using conventional processes) to obtain a continuous casting billet with a thickness of 250 mm, a width of 1500 mm and a length of 2300 mm. The element contents of the continuous casting billet are as follows:

[0041] C: 0.12%, Si: 0.45%, Mn: 1.23%, Cr: 0.36%, Ti: 0.37%, Cu: 0.12%, Al: 0.017%, V: 0.24%, Nb: 0.01%, B: 0.0019%, P: 0.012%, S: 0.005%, the balance is iron and unavoidable impurities;

[0042] (2) Heating of the ingot: First, heat the ingot to 550°C at a rate of 3°C / min and keep it at that temperature for 3 h; then heat it to 1100°C at a rate of 2°C / min and keep it at that temperature for 3 h; finally, heat it to 1250°C and keep it at that temperature for 4 h;

[0043] (3) Rough rolling: the starting rolling temperature is 1195°C, the final rolling temperature is 860°C, and the rolling is performed in 4 passes, with a single pass reduction rate of 30% to 40%;

[0044] (4) Finish rolling: the starting rolling temperature is 995°C, the final rolling temperature is 785°C, and the rolling is performed in 4 passes, with a single pass reduction rate of 10% to 20% to obtain a steel plate with a thickness of 10 mm;

[0045] (5) Cooling: The rolled steel plate is water-cooled to 220°C and then air-cooled to room temperature;

[0046] (6) The steel plate is heated to 200° C. for low temperature tempering, kept at this temperature for 2 to 3 hours, and cooled to obtain the NM400 steel plate.

[0047] Example 3

[0048] A method for processing NM400 steel plate, the steps are as follows:

[0049] (1) Smelting, refining and continuous casting: The raw materials were mixed and smelted in a converter at a smelting temperature of 1120°C. The raw materials were kept warm for 100 min before being taken out of the converter. The raw materials were then sent to an LF refining furnace for refining and vacuum treatment, and then continuously cast (refining and continuous casting were both performed using conventional processes) to obtain a continuous casting billet with a thickness of 250 mm, a width of 1500 mm and a length of 2300 mm. The element contents of the continuous casting billet are as follows:

[0050] C: 0.15%, Si: 0.41%, Mn: 1.37%, Cr: 0.31%, Ti: 0.43%, Cu: 0.18%, Al: 0.023%, V: 0.27%, Nb: 0.02%, B: 0.0024%, P: 0.009%, S: 0.003%, the balance is iron and unavoidable impurities;

[0051] (2) Heating of the ingot: First, heat the ingot to 550°C at a rate of 3°C / min and keep it at that temperature for 3 h; then heat it to 1100°C at a rate of 2°C / min and keep it at that temperature for 4 h; finally, heat it to 1285°C and keep it at that temperature for 4 h;

[0052] (3) Rough rolling: the starting rolling temperature is 1170°C, the final rolling temperature is 880°C, and the rolling is performed in 5 passes, with a single pass reduction rate of 30% to 40%;

[0053] (4) Finish rolling: the starting rolling temperature is 960°C, the final rolling temperature is 790°C, and the rolling is performed in three passes, with a single pass reduction rate of 10% to 20% to obtain a steel plate with a thickness of 10 mm;

[0054] (5) Cooling: The rolled steel plate is water-cooled to 230°C and then air-cooled to room temperature;

[0055] (6) The steel plate is heated to 190° C. for low temperature tempering, kept at this temperature for 3 hours, and cooled to obtain the NM400 steel plate.

[0056] Comparative Example 1

[0057] A method for processing a NM400 steel plate, the steps are the same as those in Example 1, and the specific element contents are as follows:

[0058] C: 0.012%, Si: 0.49%, Mn: 1.25%, Ti: 0.27%, V: 0.25%, Nb: 0.02%, B: 0.0019%, P: 0.014%, S: 0.002%, and the balance is iron and inevitable impurities.

[0059] Comparative Example 2

[0060] A method for processing NM400 steel plate, the steps of heating the ingot are as follows:

[0061] First, the continuous casting billet was heated to 550°C at a rate of 3°C / min, then heated to 1100°C at a rate of 2°C / min and kept at this temperature for 3 hours; finally, it was heated to 1250°C and kept at this temperature for 4.5 hours;

[0062] The remaining steps are the same as those in Example 1, and the specific element composition is the same as that in Example 1.

[0063] Comparative Example 3

[0064] A method for processing NM400 steel plate, the steps of heating the ingot are as follows:

[0065] First, the continuous casting billet was heated to 550°C at a rate of 33°C / min and kept at this temperature for 2.5 hours; then, it was heated to 1250°C at a rate of 2°C / min and kept at this temperature for 4.5 hours;

[0066] The remaining steps are the same as those in Example 1, and the specific element composition is the same as that in Example 1.

[0067] Comparative Example 4

[0068] A method for processing NM400 steel plate, the cooling steps are as follows:

[0069] After rolling, the steel plate is water-cooled to room temperature;

[0070] The remaining steps are the same as those in Example 1, and the specific element composition is the same as that in Example 1.

[0071] The steel plates prepared in Examples 1 to 3 and Comparative Examples 1 to 4 were subjected to performance tests, wherein the strength was tested according to the room temperature tensile test method for metal materials in GB / T228-2002, the low temperature impact toughness was tested according to the metal Charpy impact test method in GB / T229-2007, and the hardness was tested according to the method in GB / T231.1-2009. The results are shown in Table 1.

[0072] Table 1

[0073]

[0074]

[0075] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for processing NM400 steel plate, characterized in that: The following steps are involved: (1) Smelting, refining and continuous casting: The raw materials are mixed and smelted in a converter, sent to an LF refining furnace for refining and vacuum treatment, and continuously cast to obtain a continuous casting billet; (2) Heating of the ingot: The continuous casting ingot is heated to 1200-1300°C by a three-stage heating method and kept at this temperature for 4-5 hours; (3) Rolling: The heated continuous casting billet is subjected to rough rolling and finish rolling to obtain a rolled steel plate; (4) Cooling: The rolled steel plate is first water-cooled to 200-230°C, and then air-cooled to room temperature; (5) Low temperature tempering to obtain the NM400 steel plate.

2. The processing method of NM400 steel plate according to claim 1, characterized in that: The smelting temperature in step (1) is 1100-1200° C. and the smelting temperature is kept for 60-120 minutes before being taken out of the furnace.

3. The processing method of NM400 steel plate according to claim 1, characterized in that: The element content of the continuous casting billet in step (1) is: C: 0.09~0.17%, Si: 0.2~0.6%, Mn: 1.1~1.5%, Cr: 0.3~0.4%, Ti: 0.1~0.45%, Cu: 0.05~0.2%, Al: 0.01~0.025; V: 0.2-0.3%, Nb: 0.01-0.03%, B: 0.001-0.0025%, P: ≤0.02%, S: ≤0.008%, and the balance is iron and inevitable impurities.

4. The processing method of NM400 steel plate according to claim 1, characterized in that: The element content of the continuous casting billet in step (1) is: C: 0.14%, Si: 0.6%, Mn: 1.29%, Cr: 0.37%, Ti: 0.32%, Cu: 0.13%, Al: 0.019%, V: 0.25%, Nb: 0.02%, B: 0.0017%, P: 0.009%, S: 0.007%, and the remainder is iron and inevitable impurities.

5. The method for processing the NM400 steel plate according to claim 1, characterized in that: The specifications of the continuous casting billet in step (1) are 250-300 mm thick, 1500-1600 mm wide and 2300-1500 mm long.

6. The method for processing the NM400 steel plate according to claim 1, characterized in that: The specific method for heating the ingot in step (2) is as follows: first, heating to 500-550°C at a rate of 2-3°C / min, and keeping warm for 2-3 hours; then heating to 1000-1150°C at a rate of 1-3°C / min; keeping warm for 2-4 hours; and finally heating to 1200-1300°C, and keeping warm for 4-5 hours.

7. The method for processing the NM400 steel plate according to claim 1, characterized in that: The starting rolling temperature of the rough rolling in step (3) is 1150-1200° C., the final rolling temperature is 850-900° C., and the rolling is performed in 4-5 passes, with a single pass reduction rate of 30%-40%.

8. The method for processing the NM400 steel plate according to claim 1, characterized in that: The starting rolling temperature of the finishing rolling in step (3) is 950-1000°C, the final rolling temperature is 750-800°C, and the rolling is performed in 3-4 passes, with a single pass reduction rate of 10%-20%.

9. The method for processing the NM400 steel plate according to claim 1, characterized in that: The thickness of the steel plate after rolling in step (3) is 8 to 15 mm.

10. The method for processing the NM400 steel plate according to claim 1, characterized in that: The temperature of the low-temperature tempering in step (5) is 180-230° C. and the time is 2-3 hours.

Citation Information

Patent Citations

  • Microalloyed bainitic / martensitic multiphase NM400 steel plate and its preparation method

    CN107012396B

  • A type DQ martensitic wear-resistant steel plate of grade NM400 and its preparation method

    CN114045444B