Packing belt and production method and application thereof
By using iron, manganese and aluminum materials in steel packaging tape and performing blue treatment, combined with water-soluble resin protective film, the flexibility problems brought about by high tensile strength and the high production cost are solved, and the applicable to Complex shapes and frequently packed steel straps have excellent flexibility and corrosion resistance.
Patent Information
- Application Number
- CN202411193825.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-28
AI Technical Summary
The high tensile strength of existing steel packaging belts leads to poor flexibility, making it difficult to adapt to complex shapes and frequent packaging, and has high production costs, which limits its application in light industry and other fields.
The steel strip material mainly includes iron, manganese and aluminum. The oxide film is formed through the blue-blue process, combined with a water-soluble resin protective film, which reduces the tensile strength and improves flexibility and corrosion resistance, and forms a tensile strength of more than 700MPa and an elongation of 12. % or more packing tape.
It achieves the flexibility and corrosion resistance of steel packaging belts, and is suitable for complex shapes and frequent packaging occasions, while reducing production costs and extending service life.
Smart Images

Figure CN119082603A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of strapping tape production, and in particular to a strapping tape and a production method and application thereof. Background Art
[0002] Steel strapping tape has been widely used in the packaging and bundling of steel, metal products, logistics and transportation, building materials, paper rolls (boards), etc. due to its high tensile strength, excellent elongation and excellent corrosion resistance. In practical applications, steel strapping tapes of different strength levels are selected according to the different properties of the goods (such as weight, volume, transportation distance) and the desired bundling effect.
[0003] The tensile strength of existing steel strapping tape is above 830MPa, but strapping tape with higher tensile strength is not flexible and is relatively stiff. For complex strapping shapes and changes, the probability of stress concentration and breakage during the strapping process increases, affecting the strapping efficiency. In addition, high-strength strapping tape often requires the addition of more alloys, and the production and procurement costs are much higher than those of ordinary steel. Therefore, strapping tape with higher tensile strength is not suitable for light industry and other fields. Summary of the invention
[0004] In order to solve the above problems, the present application proposes a strapping tape and a production method and application thereof, wherein the main metals of the steel strap in the strapping tape only include iron, manganese and aluminum, thereby reducing the production cost of the strapping tape; in addition, the tensile strength of the strapping tape is above 700 MPa, and the elongation A is 30mm It is more than 12%.
[0005] This application is implemented through the following technical solutions:
[0006] One of the purposes of the present application is to provide a strapping tape, comprising a steel tape and a protective film, wherein the protective film wraps the steel tape;
[0007] The steel strip includes iron and the following components in mass fraction: 0.17%≤C≤0.20%, Si≤0.30%, 0.15%<Mn≤0.40%, P≤0.035%, S≤0.010%, 0.015%≤Al≤0.035%.
[0008] The strapping tape provided in the present application has a steel tape with the main metal components only containing common iron, manganese and aluminum metals, and a low alloy content, which reduces the production cost of the strapping tape; the protective film makes the strapping tape waterproof, moisture-proof and rust-proof, thereby effectively extending the service life of the strapping tape. The tensile strength of the strapping tape is above 700MPa, and the elongation A is 30mm It is above 12% and has good flexibility, which is suitable for occasions with complex packaging shapes, changes and frequent packaging speeds.
[0009] In some possible implementations, the composition of the steel strip includes iron and also includes the following components in mass fractions: 0.18%≤C≤0.19%, 0.06%≤Si≤0.08%, 0.2%≤Mn≤0.40%, 0.016%≤P≤0.019%, 0.003%≤S≤0.004%, and 0.015%≤Al≤0.035%.
[0010] In some possible implementations, the protective film has a thickness of 3 μm to 5 μm.
[0011] In some possible implementations, the material of the protective film includes a water-soluble resin; the water-soluble resin includes one or more of a water-based acrylic resin, a water-based polyurethane resin, a water-based epoxy-modified acrylic resin, and an acrylic-modified saturated polyester resin.
[0012] In some possible implementations, the strapping tape has a thickness of 0.7 mm to 1.0 mm and a width of 31.75±0.13 mm.
[0013] In some possible implementations, the tensile strength of the strapping tape is greater than 700 MPa, and the elongation A is less than 100 MPa. 30mm It is more than 12%.
[0014] In some preferred implementations, the tensile strength of the strapping tape is 752 MPa to 778 MPa, and the elongation A 30mm It is 12.3% to 13.5%.
[0015] The second object of the present application is to provide a method for producing a strapping tape, comprising the following steps: the stripped steel coil is subjected to the steps of bluing, cooling, waxing and drying to obtain the strapping tape;
[0016] Wherein, in the bluing step, the bluing temperature is 530°C to 600°C, and the bluing time is 90s to 150s.
[0017] In the production method of the strapping tape of the present application, the blueing temperature and time are adopted, and the surface of the steel tape is oxidized to form a uniform and dense oxide film (Fe3O4), which not only improves the corrosion resistance of the steel tape, but also enhances the aesthetics of the strapping tape (with a unique blue-black appearance). In addition, the blueing step can refine the grains, improve the structure and reduce the hardness, and eliminate the internal stress at the same time, thereby effectively reducing the tensile strength of the strapping tape and improving the flexibility of the strapping tape. The prepared strapping tape has excellent elongation, flexibility and corrosion resistance; the excellent elongation improves the tightness and stability of the strapping tape during use; the excellent flexibility enables the strapping tape to adapt to complex packaging shapes, changes and frequent packaging speeds; the excellent corrosion resistance enables the strapping tape to maintain a long service life in a variety of harsh environments, thereby further enhancing its application value.
[0018] In some embodiments, in the drying step, the drying temperature is 180° C. to 220° C., the drying speed is 15 m / min to 18 m / min, and the drying time is 5 s to 10 s.
[0019] The third purpose of the present application is to provide a strapping tape of the present application or a strapping tape produced by the strapping tape production method of the present application for use in the field of packaging of steel, metal products or logistics transportation. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the embodiments of the present drawings or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present drawings. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying any creative work.
[0021] Figure 1 Schematic diagram of the steel strip of the steel coil unwinding and striping in the embodiment of the present application;
[0022] Figure 2 A schematic diagram of the structure of a strapping tape after being rolled up, obtained by a strapping tape production method in an embodiment of the present application;
[0023] Figure 3 This is a schematic diagram of the application of the strapping tape in the embodiment of the present application in the field of steel pipe materials.
[0024] The purpose, features and advantages of this figure will be further described in conjunction with the embodiments with reference to the accompanying drawings. DETAILED DESCRIPTION
[0025] In order to make the purpose, technical solutions and advantages of the present application clearer, the present application is described and illustrated below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not intended to limit the present application. Based on the embodiments provided in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present application.
[0026] Obviously, the following descriptions are only some examples or embodiments of the present application. For ordinary technicians in this field, the present application can also be applied to other similar scenarios without creative work. In addition, it can also be understood that although the efforts made in this development process may be complicated and lengthy, for ordinary technicians in the field related to the content disclosed in this application, some changes in design, manufacturing or production based on the technical content disclosed in this application are just conventional technical means, and should not be understood as insufficient content disclosed in this application.
[0027] However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repeated descriptions of substantially the same structures may be omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate understanding by those skilled in the art. In addition, the following description is provided for those skilled in the art to fully understand the present application and is not intended to limit the subject matter described in the claims.
[0028] If not otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution, and all technical features and optional technical features of the present application can be combined with each other to form a new technical solution.
[0029] Tensile strength refers to the maximum force that a steel strapping tape can withstand when subjected to tensile force, and is one of the important indicators for measuring its mechanical properties. The tensile strength of existing steel strapping tapes is above 830MPa. Steel strapping tapes with high tensile strength usually have better load-bearing capacity and anti-destruction ability, and can ensure effective fixation and protection of the packaged objects during transportation and storage.
[0030] However, too high a tensile strength will reduce the flexibility of the steel strapping tape (the ability of the strapping tape to deform to a certain extent without breaking when subjected to force). This is because if the tensile strength is too high, the strapping tape will be too rigid and difficult to adapt to complex packaging shapes and changes, and may even cause stress concentration and breakage during the packaging process.
[0031] In addition, high-tensile strength steel strapping is usually more expensive and is not suitable for use in light industrial fields or occasions where frequent strapping operations are required.
[0032] In order to take into account the tensile strength, flexibility and production cost of the strapping tape, the present application embodiment proposes a strapping tape and a production method thereof. The main metal materials of the steel strap in the strapping tape only include iron, manganese and aluminum, which effectively reduces the production cost of the strapping tape; and the tensile strength of the strapping tape is above 700MPa, and the elongation A is 30mm It is more than 12%, has excellent tensile strength and flexibility, and is suitable for complex packaging shapes, changes and frequent packaging speeds.
[0033] The following is an explanation of a strapping tape and a production method thereof according to an embodiment of the present application.
[0034]
Packaging tape
[0035] One of the purposes of the embodiments of the present application is to provide a packing tape, comprising a steel tape and a protective film, wherein the protective film wraps the steel tape;
[0036] The components of the steel strip include iron and the following components in mass fractions: 0.17%≤C≤0.20%, Si≤0.30%, 0.15%<Mn≤0.40%, P≤0.035%, S≤0.010%, 0.015%≤Al≤0.035%.
[0037] The strapping tape provided in the embodiment of the present application has a steel tape whose main metal components only include common iron, manganese and aluminum metals, and a low alloy content, thereby reducing the production cost of the strapping tape; the protective film makes the strapping tape waterproof, moisture-proof and rust-proof, thereby effectively extending the service life of the strapping tape. The tensile strength of the strapping tape is above 700MPa, and the elongation A 30mm It is above 12% and has good flexibility, which is suitable for occasions with complex packaging shapes, changes and frequent packaging speeds.
[0038] In some embodiments, the steel strip consists of the following components in mass fractions: 0.17%≤C≤0.20%, Si≤0.30%, 0.15%<Mn≤0.40%, P≤0.035%, S≤0.010%, 0.015%≤Al≤0.035%, and the remainder is iron and unavoidable impurities.
[0039] In some embodiments, the composition of the steel strip includes iron and further includes the following components in mass fractions: 0.18%≤C≤0.19%, 0.06%≤Si≤0.08%, 0.2%≤Mn≤0.40%, 0.016%≤P≤0.019%, 0.003%≤S≤0.004%, and 0.015%≤Al≤0.035%.
[0040] In some embodiments, the steel strip consists of the following components in mass fractions: 0.18%≤C≤0.19%, 0.06%≤Si≤0.08%, 0.2%≤Mn≤0.40%, 0.016%≤P≤0.019%, 0.003%≤S≤0.004%, 0.015%≤Al≤0.035%, and the remainder is iron and unavoidable impurities.
[0041] In some embodiments, the steel strip is composed of the following components in mass fractions: 0.1855% C, 0.0623% Si, 0.2405% Mn, 0.0164% P, 0.0037% S, 0.0194% Al, and the remainder is iron and unavoidable impurities.
[0042] In some embodiments, the steel strip is composed of the following components in mass fractions: 0.1894% C, 0.0758% Si, 0.3497% Mn, 0.0186% P, 0.0036% S, 0.0226% Al, and the remainder is iron and unavoidable impurities.
[0043] In some embodiments, the thickness of the protective film is 3 μm to 5 μm. In the exemplary embodiment, it can be a typical but non-limiting thickness such as 3 μm, 4 μm, 5 μm, or a range between any two thicknesses. In this case, the protective film is evenly and firmly attached to the surface of the steel belt, which can improve the waterproof, moisture-proof and rust-proof properties of the steel belt, thereby effectively extending the service life of the steel belt. It should be noted that the thickness of the protective film can be adjusted according to actual production conditions and needs, and is not limited to the scope of the embodiments of the present application.
[0044] In some embodiments, the material of the protective film includes a water-soluble resin; the water-soluble resin includes one or more of a water-based acrylic resin, a water-based polyurethane resin, a water-based epoxy-modified acrylic resin, and an acrylic-modified saturated polyester resin. The relative molecular weight of the water-soluble resin can be adjusted and selected according to the solubility, film-forming properties, mechanical properties, rust prevention, corrosion prevention and other performance requirements in the actual production process, without limitation.
[0045] In some embodiments, the material of the protective film is WEL3000 water-based baking paint with model number 3647C (white) or model number 3607B (black) produced by Weier Environmental Technology (Beijing) Co., Ltd.
[0046] In some embodiments, the tensile strength of the strapping tape is above 700 MPa, and the elongation A 30mm In this case, the strapping tape has good flexibility and can adapt to complex packaging shapes, changes and frequent packaging speeds.
[0047] In some specific embodiments, the tensile strength of the strapping tape is 752 MPa to 778 MPa. In the exemplary embodiment, it can be 752 MPa, 754 MPa, 757 MPa, 764 MPa, 768 MPa, 772 MPa, 776 MPa, 778 MPa, etc., which are typical but non-limiting tensile strengths, or a range between any two tensile strengths; the elongation A 30mm The elongation is 12.3% to 13.5%. In the exemplary embodiment, the elongation may be 12.3%, 12.5%, 13.0%, 13.3%, 13.5%, or other typical but non-limiting elongations or a range between any two elongations.
[0048] In some embodiments, the conditional yield strength (Rp0.2) of the strapping tape is 660 MPa to 730 MPa. In an exemplary embodiment, it can be a typical but non-restrictive strength such as 660 MPa, 700 MPa, 730 MPa, or a range between any two strengths. In this case, the strapping tape is not prone to plastic deformation or fracture during use, thereby improving the safety of the packaged goods.
[0049] In some embodiments, the thickness of the strapping tape is 0.7mm to 1.0mm, and the width is 31.75 ± 0.13mm; in the exemplary embodiment, the thickness of the strapping tape can be a typical but non-restrictive thickness such as 0.7mm, 0.8mm, 0.9mm, 1.0mm, or a range between any two thicknesses; the width of the strapping tape can be a typical but non-restrictive thickness such as 31.62mm, 31.75mm, 31.88mm, or a range between any two thicknesses. In this case, the strapping tape must have high dimensional control accuracy and a smooth surface to ensure that it is easy to feed the tape during use. The dimensional accuracy (i.e., positive and negative tolerances) has a significant impact on the performance of the strapping tape. When the positive tolerance of the width is large, the strapping tape width does not match the caliber of the strapping machine during use, making it difficult to enter and causing tape jams; and when the negative tolerance of the width is too much, the combination with the strapping machine is too poor, and it is easy to deviate during high-speed operation and is difficult to control. It should be noted that the thickness and width of the strapping tape can be adjusted according to actual production conditions and needs, and may not be limited to the scope limited by the embodiments of the present application.
[0050] [Production method of strapping tape]
[0051] The second object of the embodiment of the present application is to provide a method for producing a strapping tape, comprising the following steps: a steel coil is subjected to the steps of bluing, cooling, waxing and drying to obtain a strapping tape;
[0052] Wherein, in the bluing step, the bluing temperature is 530°C to 600°C, and the bluing time is 90s to 150s.
[0053] In the production method of the strapping tape of the embodiment of the present application, the blueing temperature and time are adopted, and the surface of the steel strip is oxidized to form a uniform and dense oxide film (Fe3O4), which not only improves the corrosion resistance of the steel strip, but also enhances the aesthetics of the strapping tape (with a unique blue-black appearance). In addition, the blueing step can refine the grains, improve the structure and reduce the hardness, and eliminate the internal stress at the same time, thereby effectively reducing the tensile strength of the strapping tape and improving the flexibility of the strapping tape. The prepared strapping tape has excellent elongation, flexibility and corrosion resistance; the excellent elongation improves the tightness and stability of the strapping tape during use; the excellent flexibility enables the strapping tape to adapt to complex packaging shapes, changes and frequent packaging speeds; the excellent corrosion resistance enables the strapping tape to maintain a long service life in a variety of harsh environments, thereby further enhancing its application value.
[0054] In the embodiment, the bluing temperature is 530°C to 600°C, and can be typical but non-limiting temperatures such as 530°C, 550°C, 570°C, 590°C, 600°C, or a range between any two temperatures; the bluing time is 90s to 150s, and can be typical but non-limiting times such as 90s, 100s, 120s, 150s, or a range between any two times.
[0055] In some embodiments, the steps of preparing the steel coil include: molten iron smelting, LF refining, CSP (Compact Strip Production) continuous casting and rolling, pickling and cold rolling, and coiling.
[0056] [Hot metal smelting]
[0057] In some embodiments, in the molten iron smelting step, the carbon content of the steel is controlled at 0.100% to 0.155%, the argon station carbon is controlled at 0.100% to 0.160%, and the converter steel tapping temperature is above 1600° C. In this case, it is beneficial to control the temperature and composition of the subsequent smelting process and ensure the production rhythm of smelting molten steel.
[0058] In some specific embodiments, in the molten iron smelting step, the molten iron includes iron and the following components by mass fraction:
[0059] Cu≤0.1%, As≤0.035%, Sn≤0.05%, S≤0.05%, P≤0.150%, S≤0.06%, among which, M (Cu+5As+8Sn) ≤0.35%.
[0060] In some other specific embodiments, in the molten iron smelting step, the molten iron consists of the following components by mass fraction:
[0061] Cu≤0.1%, As≤0.035%, Sn≤0.05%, S≤0.05%, P≤0.150%, S≤0.06%, the rest is iron and unavoidable impurities; among which, M (Cu+5As+8Sn) ≤0.35%.
[0062] In some specific embodiments, the endpoint composition of the converter molten steel includes iron, and also includes the following components in mass fractions: 0.100%≤C≤0.155%, P≤0.025%, S≤0.06%.
[0063] In some specific embodiments, the tapping temperature of the converter is above 1600° C., and the liquidus of the molten steel is 1515° C. In this case, the liquidus temperature of the molten steel determines the temperature control of each process in the steelmaking process. In addition, the continuous casting superheat is also calculated and set based on the liquidus temperature.
[0064] In other specific embodiments, the endpoint composition of the converter molten steel consists of the following components in mass fractions: 0.100%≤C≤0.155%, P≤0.025%, S≤0.06%, and the rest are iron and unavoidable impurities.
[0065] In some embodiments, the composition of the molten steel at the argon station intersection includes iron, and also includes the following components in mass fractions: 0.10%≤C≤0.16%, Si≤0.05%, 0.08%≤Mn≤0.40%, P≤0.03%, S≤0.060%, 0.01%≤Alt≤0.05%.
[0066] In some embodiments, the composition of the molten steel at the argon station junction also includes: Cu≤0.1%, As≤0.035%, Sn≤0.05%, M (Cu+5As+8Sn) ≤0.35%.
[0067] In other embodiments, the composition of the molten steel at the argon station intersection includes iron, and also includes the following components in mass fractions: 0.10%≤C≤0.16%, Si≤0.05%, 0.08%≤Mn≤0.20%, P≤0.03%, S≤0.060%, 0.015%≤Alt≤0.05%.
[0068] [LF Refining]
[0069] In some embodiments, in the LF refining step, the specific contents are steps commonly used in the art, such as desulfurization, deoxidation, etc., and the refining time and the temperature control of each step can be adjusted according to the actual situation. Exemplarily, the refining time is 45min to 120min; the desulfurization temperature is 1560°C to 1580°C. Another exemplary method is to add lime, slag-removing agent, pre-melted slag and calcium carbide according to the slag condition and [S] content for investigation, and the quaternary basicity of the slag is controlled at about 2.0, (FeO) + (MnO) in the slag is less than 1.0%, the slag is slightly thin, and the slag is white. After the molten steel enters the station, the bottom blowing is turned on to facilitate slag removal. Bypass stirring is not allowed throughout the process to prevent serious nitrogen increase. The alloy composition is controlled according to the target. The temperature must be measured before calcium treatment to ensure the outlet temperature. After calcium treatment, power supply, large argon stirring and feeding are prohibited.
[0070] In some embodiments, the molten steel produced in the LF refining step includes iron and the following components in mass fractions: 0.17%≤C≤0.20%, Si≤0.30%, 0.15%≤Mn≤0.40%, P≤0.035%, S≤0.010%, 0.02%≤Alt≤0.07%.
[0071] [CSP continuous casting and rolling]
[0072] In some embodiments, the conditions of CSP continuous casting and rolling are not subject to specific restrictions and can be adjusted and selected according to actual production conditions. As an example, in the CSP continuous casting step, medium carbon steel crystallizer protective slag is used, which can be mixed with medium carbon steel grades such as Q235B and S235JR. Before pouring, each argon sealing system is leak-checked, and the argon blowing in the middle ladle is ≥2 minutes; after the large ladle is poured, the superheat is controlled at 15°C to 35°C; the pulling speed is ≥3.8m / min, and the composition of the middle ladle is controlled to be C at 0.170% to 0.200%, Si at less than 0.300%, Mn at 0.15% to 0.40%, P at less than 0.035%, and S at less than 0.010%.
[0073] As an example, the furnace temperature of the cast slab is 1150℃~1200℃. In this case, the CSP process is compact, and the thin slab has the advantages of high furnace temperature and small temperature difference during rolling. This temperature range can ensure that the steel has good plasticity and is easy to roll. At the same time, under the condition of energy economy, it can also avoid coarse grains caused by excessive temperature, which affects the mechanical properties of the material.
[0074] As an example, in the dephosphorization step of CSP continuous casting and rolling, the inlet pressure is above 20 MPa and the outlet pressure is above 30 MPa. The actual inlet and outlet pressures are based on the descaling effect, and the pressures can be adjusted and are not limited by this example.
[0075] As an example, in the hot rolling step of CSP continuous casting and rolling, the final rolling temperature is 865℃~895℃, the coiling temperature is 602℃~638℃, and the laminar cooling mode is concentrated cooling in the rear section. The thickness range of the steel strip obtained by hot rolling is 1.5mm~6.0mm. The actual thickness range is adjusted according to the actual rolling conditions and is not limited by the example range.
[0076] As an example of the effect, when the thickness of the steel strip obtained by hot rolling is less than 3 mm, the hot rolling convexity C40 is 25μm~55μm, the wedge-shaped |W40| is less than C40, and the head and tail thickness deviation is -0.1mm~0.1mm; when the thickness of the steel strip obtained by hot rolling is more than 3 mm, the hot rolling convexity C40 is 30μm~55μm, the wedge-shaped |W40| is less than C40, and the head and tail thickness deviation is -0.1mm~0.1mm.
[0077] The term "crown C40" refers to the thickness variation of hot-rolled strip in the cross section. When the C40 value is too large, it will cause the appearance of intermediate wave shape defects during cold rolling. The "small crown" rolling strategy, which reduces the control target of hot rolling crown C40 from 50μm to 30μm, can significantly reduce the defect rate of cold rolling intermediate wave.
[0078] The term "wedge shape W40" refers to the difference in thickness of the two edges of the hot-rolled strip in the length direction. If the wedge value is too large, the strip will easily run off the track and be unevenly coiled during subsequent processing, affecting the running stability of the production line and the plate quality of the product. In addition, the wedge shape will also affect the flatness of the strip, resulting in wavy defects on the surface of the product, affecting the appearance quality and market value of the product.
[0079] In some embodiments, during the pickling and cold rolling step,
[0080] In some embodiments, the steel coil needs to go through the steps of uncoiling, slitting and deburring before the blueing step to obtain a steel strip with smooth edges and no sawtooth. The uncoiling, slitting and deburring processes are adjusted according to actual production conditions and are not limited by the exemplary steps. Figure 1 The uncoiling and slitting step includes slitting the cold rolled coil into the required width (generally 31.75±0.13mm) by a disc shear on a slitting line. During the slitting process, the edge of the steel strip is ensured to be smooth and without jagged edges, providing good conditions for subsequent processes. As an example, the deburring step includes removing the tiny burrs and uneven parts that may exist on the edge of the steel strip through a deburring roller, making its edge smoother and preventing scratches or injuries during use.
[0081] In some embodiments, the cooling step includes: cooling the steel strip to room temperature after the bluing step. In this case, when the steel strip cooled to room temperature enters the subsequent waxing step, the wax layer can be evenly and firmly attached to the surface of the steel strip, avoiding the wax layer from falling off or unevenness caused by excessive temperature, thereby improving the quality of waxing. It should be noted that the cooling rate can be adjusted according to the actual production situation, but as an example, the cooling rate can be 5°C / s. The blued steel strip can be cooled by a fan so that its temperature quickly drops to room temperature (fast cooling). Fast cooling is equivalent to a quenching process to ensure the final target strength of the product. Fast cooling can improve production efficiency, and is also beneficial for the oxide film formed in the bluing process to be denser and more stable, which can better protect the surface of the strapping tape. Rapid cooling of the steel strip to room temperature after bluing (such as by a fan) is an important step in the production process, which plays a key role in improving the performance of the strapping tape and extending its service life.
[0082] In some embodiments, the wax coating step includes: placing the steel strip cooled to room temperature in a water-soluble wax tank for wax coating, and the wax liquid is precisely controlled and evenly applied to the surface of the steel strip to form a firm protective film. In this case, the protective film improves the waterproof, moisture-proof and rust-proof properties of the steel strip, and effectively extends the service life of the steel strip. Of course, the wax coating environment and temperature can be adjusted according to the actual production process and environment without restriction.
[0083] In some embodiments, the water-soluble wax is WEL3000 water-based baking paint with model 3647C (white) or model 3607B (black) produced by Weier Environmental Technology (Beijing) Co., Ltd.
[0084] In some embodiments, the drying step includes: drying and curing the steel belt coated with the protective film. In this case, through high-temperature drying, the wax layer of the protective film is rapidly solidified to form a uniform and hard protective layer, so that the protective film can be firmly attached to the surface of the steel belt, thereby improving the waterproof, moisture-proof and rust-proof protective properties of the steel belt, and effectively extending the service life of the strapping steel belt (the wax layer is too thick, which will affect the thickness accuracy and strength of the strapping belt, and too thin will weaken its protective effect). Similarly, the temperature and drying time of the drying step are also adjusted according to the actual production process and environment, without restriction; as long as it does not cause problems such as cracking of the protective film. As an example, the drying temperature is 180°C to 220°C, the drying speed is 15m / min to 18m / min, and the drying time is 5s to 10s. The dried steel belt can be further coiled according to actual needs (refer to Figure 2 ), packaging and warehousing; as an example, the dried steel strips can be neatly packaged and stored in a dry and clean warehouse.
[0085] As an example, an embodiment of a method for producing a strapping tape is provided, comprising the following steps:
[0086] S1. Molten steel smelting: the tapping C is controlled at 0.1108% (or 0.1166%), the argon station carbon is controlled at 0.1134% (or 0.1206%), and the converter tapping temperature is 1615°C (or 1618°C).
[0087] S2.LF refining treatment: smelting time 58min (or 46min); desulfurization temperature is 1565℃~1575℃ (or 1568℃~1575℃); LF outgoing composition is controlled at 0.1826% (or 0.1834%) C, Si is controlled at 0.0586% (or 0.0738%), Mn is controlled at 0.2432% (or 0.3437%), P is controlled at 0.0153% (or 0.0186%), S is controlled at 0.0036%, and the soft blowing time is 10min (or 8min).
[0088] S3.CSP continuous casting: argon is blown into the tundish for 2 minutes before pouring; after pouring, the actual superheat is controlled at 18°C ~ 25°C (or 15°C ~ 25°C); the drawing speed is increased to 4.2m / min and kept constant; the composition of the tundish is controlled at C at 0.1855% (or 0.1894%), Si at 0.0623% (or 0.0758%), Mn at 0.2405% (or 0.3497%), P at 0.0164% (or 0.0186%), and S at 0.0037% (or 0.0036%).
[0089] S4.CSP hot rolling: before the slab enters the furnace, check that the furnace rollers and burners are working normally, maintain a weak oxidizing atmosphere in the heating furnace, ensure that the slab is heated evenly, control the temperature of the cast slab out of the furnace within the range of 1060℃~1200℃, and the temperature difference between the head and tail of the slab is ≤20℃; the final rolling temperature is 880±15℃, and the coiling temperature is 680±18℃.
[0090] S5. Pickling: The acid tank concentration and acid solution temperature selected in this step are the commonly used processes for low-carbon steel pickling in this field. The steel strip after pickling is required to have no acid, no water, no parking spots, no foreign pollution, no mechanical damage on the upper and lower surfaces, and no under-pickling or over-pickling on the surface of the steel strip.
[0091] S6. Cold rolling: The pickled steel strip is cold rolled to obtain a cold rolled coil. The cold rolling step uses the F4 stand working roll in a rough roll mode, the rolling mileage is controlled according to the current process system, and the surface quality is controlled according to the S3 grade.
[0092] S7. Uncoiling and slitting: The cold rolled coil is slitting into the required width of 32±0.3mm by a disc shear on the slitting production line. During the slitting process, the edge of the steel strip is ensured to be smooth and without serrations, providing good conditions for subsequent processes.
[0093] S8. Deburring: Use the deburring roller to remove the tiny burrs and uneven parts that may exist on the edge of the steel strip, making its edge smoother and preventing scratches or injuries during use.
[0094] S9. Bluing: After the above process, the steel strip is finely treated and then put into the induction resistance furnace for bluing. The bluing temperature is 530℃~600℃ and the bluing time is 90s~150s. In this process, the surface of the steel strip undergoes a specific oxidation treatment to form a uniform and dense oxide film (Fe3O4). This oxide film not only improves the corrosion resistance of the steel strip, but also gives it a unique blue-black appearance, enhancing the beauty of the product.
[0095] S10. Cooling: After the bluing treatment is completed, the steel strip enters the cooling zone and is cooled by the self-blower to quickly reduce its temperature to room temperature. This step is crucial to ensure the stable performance of the steel strip in the subsequent wax coating process.
[0096] S11. Waxing: Entering the water-soluble wax tank for waxing, coating the steel strip with a uniform wax protective layer, is a key step to improve the product's waterproof, moisture-proof and rust-proof properties. During the waxing process, the wax liquid is precisely controlled and evenly applied to the steel strip surface, forming a firm protective film, which effectively extends the service life of the steel strip.
[0097] S12. Drying: To ensure that the wax layer can be firmly attached to the surface of the steel strip, the steel strip after wax coating needs to be dried and solidified. Through high-temperature drying, the wax layer solidifies quickly to form a hard protective layer, which further enhances the protective performance of the steel strip.
[0098] S13. Coiling, packaging and warehousing: The dried steel strips are neatly packaged and stored in a dry and clean warehouse.
[0099] refer to Figure 3 The third purpose of the embodiments of the present application is to provide a strapping tape according to the embodiments of the present application or a strapping tape produced by the production method of the strapping tape according to the embodiments of the present application for use in the field of packaging of steel, metal products or logistics transportation.
[0100] The strapping tape and production method of the present application are further described below in conjunction with specific embodiments.
[0101] Example 1
[0102] Embodiment 1 provides a packing tape, comprising a steel tape and a protective film, wherein the protective film wraps the steel tape;
[0103] The steel strip is composed of the following components by mass fraction: 0.1855% C, 0.0623% Si, 0.2405% Mn, 0.0164% P, 0.0037% S, 0.0194% Al, and the rest is Fe and unavoidable impurities;
[0104] The thickness of the protective film is 4 μm.
[0105] Embodiment 1 also proposes a method for producing a strapping tape of the present embodiment, comprising the following steps:
[0106] 1) Obtain the steel coil to be processed. The specifications (thickness*width) of the steel coil to be processed are 0.898mm*1300mm, the conditional yield strength (Rp0.2) is 880MPa, the tensile strength is 950MPa, and the elongation A 30mm It is 12.1%.
[0107] 2) Uncoiling and slitting: The steel coil to be processed is placed on the longitudinal slitting production line and is longitudinally slid into steel strips with a width of 31.7±0.3mm by a circular shear; during the slitting process, ensure that the edge of the steel strip is smooth and has no serrations ≥0.5mm deep.
[0108] 3) Deburring of steel strip: The steel strip is passed through a deburring roller to remove the tiny burrs and uneven parts that may exist on the edge of the steel strip, making its edge smoother.
[0109] 4) Bluing: The deburred steel strip is placed in an induction resistance furnace for bluing. The bluing temperature is 570°C and the bluing time is 120s.
[0110] 5) Cooling: Place the blued steel strip in the cooling zone and cool it with a natural fan at a cooling rate of -5°C / S.
[0111] 6) Waxing: After bluing and cooling, the steel strip is placed in a water-soluble wax tank for waxing, and a wax protective layer with a thickness of 4 μm is dip-coated on the surface of the steel strip. The wax protective layer material is a water-based acrylic resin. Among them, the water-soluble wax is the WEL3000 water-based baking paint with model 3647C (white) produced by Weier Environmental Technology (Beijing) Co., Ltd.
[0112] 7) Drying: The waxed steel strip is dried at a temperature of 180°C to 220°C for 5s to 10s to obtain a packing tape.
[0113] 8) The strapping tape is subsequently rolled up, packaged and stored.
[0114] Example 2
[0115] Embodiment 2 provides a packing tape, comprising a steel tape and a protective film, wherein the protective film wraps the steel tape;
[0116] The steel strip is composed of the following components in mass fractions: 0.1894% C, 0.0758% Si, 0.3497% Mn, 0.0186% P, 0.0036% S, 0.0226% Al, and the rest is Fe and unavoidable impurities.
[0117] Example 2 also proposes a method for producing a strapping tape of this embodiment, the steps are basically the same as those of Example 1, except that: the conditional yield strength (Rp0.2) of the steel coil to be processed is 832MPa, the tensile strength is 936MPa, and the elongation A is 30mm It is 10.7%.
[0118] Example 3
[0119] Example 3 proposes a strapping tape and a production method thereof. The structural composition of the strapping tape is the same as that of Example 1, and the steps of the production method are basically the same as those of Example 1, except that in the bluing step, the bluing temperature is 530°C and the bluing time is 150s.
[0120] Example 4
[0121] Example 4 proposes a strapping tape and a production method thereof. The structural composition of the strapping tape is the same as that of Example 1, and the steps of the production method are basically the same as those of Example 1, except that in the bluing step, the bluing temperature is 600°C and the bluing time is 90s.
[0122] Example 5
[0123] Example 5 proposes a strapping tape and a production method thereof. The structural composition of the strapping tape is the same as that of Example 1, and the steps of the production method are basically the same as those of Example 1, except that the thickness of the protective film in the wax coating step is 3 μm.
[0124] Example 6
[0125] Example 6 proposes a strapping tape and a production method thereof. The structural composition of the strapping tape is the same as that of Example 1, and the steps of the production method are basically the same as those of Example 1, except that the thickness of the protective film in the wax coating step is 5 μm.
[0126] Comparative Example 1
[0127] Comparative Example 1 proposes a strapping tape and a production method thereof. The structure and composition of the strapping tape are the same as those in Example 1, and the steps of the production method are basically the same as those in Example 1, except that the conditional yield strength (Rp0.2) of the steel coil to be processed is 950 MPa, the tensile strength is 1048 MPa, and the elongation A is 30mm It is 4.5%.
[0128] Comparative Example 2
[0129] Comparative Example 2 proposes a strapping tape and a production method thereof. The structural composition of the strapping tape is the same as that of Example 1, and the steps of the production method are basically the same as those of Example 1, except that in the bluing step, the bluing temperature is 520°C and the bluing time is 160s.
[0130] Comparative Example 3
[0131] Comparative Example 3 proposes a strapping tape and a production method thereof. The structural composition of the strapping tape is the same as that of Example 1, and the steps of the production method are basically the same as those of Example 1, except that in the bluing step, the bluing temperature is 620°C and the bluing time is 80s.
[0132] Comparative Example 4
[0133] Comparative Example 4 proposes a strapping tape and a production method thereof. The structural composition of the strapping tape is the same as that of Example 1, and the steps of the production method are basically the same as those of Example 1, except that the thickness of the protective film in the wax coating step is 6 μm.
[0134] In order to verify the progressiveness of the strapping tape and the production method thereof provided in the embodiments of the present application, the strapping tapes provided in Examples 1 to 6 and Comparative Examples 1 to 4 were subjected to at least conditional yield strength (R p 0.2), tensile strength, elongation A 30mm The results of the thickness test (finished product thickness) are shown in Table 1 below.
[0135] Table 1
[0136]
[0137] From Table 1 above, at least the following conclusions can be drawn:
[0138] ① The production method of strapping provided in the embodiment of the present application combines the characteristics of strapping steel and the use strength level requirements, makes adjustments based on the composition and process of ordinary medium carbon steel, utilizes the work hardening of cold rolled coils to improve the strength of the coils, and combines the optimization of the production process of strapping to produce strapping with low cost, stable tensile strength of more than 700MPa, and elongation A 30mm ≥12%, suitable for steel strapping with normal strength requirements.
[0139] ② The tensile strength of the strapping tape in the embodiment of the present application is above 700 MPa, and the elongation A 30mmThe thickness of the strapping tape is above 12%, so it has good flexibility and elongation, and can be widely used in packaging and bundling in the fields of steel, metal products, logistics and transportation, and can also be customized to meet the needs of different industries and scenarios. Furthermore, the wide application of the strapping tape of the embodiment of the present application will help improve the overall level of the packaging industry and promote the coordinated development of related industries.
[0140] ③ The production method of the strapping tape in the embodiment of the present application has a tensile strength of less than 830 MPa, filling the gap of 700 MPa-level ordinary strength strapping tape in the prior art. This not only helps to meet the actual needs of related industries, but also provides strong support for the development of related industries.
[0141] ④ The strapping tape of the embodiment of the present application has excellent elongation performance, ensuring the tightness and stability of the strapping tape during use.
[0142] ⑤ The production method of the strapping tape in the embodiment of the present application optimizes the process links such as bluing and dipping (waxing), and the strapping tape produced also has excellent corrosion resistance and can maintain a long service life in a variety of harsh environments, thereby further enhancing its application value.
[0143] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A packing tape, comprising a steel tape and a protective film, wherein the protective film wraps the steel tape; characterized in that: The steel strip comprises iron and the following components in mass fractions: 0.17%≤C≤0.20%, Si≤0.30%, 0.15%<Mn≤0.40%, P≤0.035%, S≤0.010%, 0.015%≤Al≤0.035%.
2. The strapping tape according to claim 1, characterized in that: The steel strip comprises iron and the following components in mass fractions: 0.18%≤C≤0.19%, 0.06%≤Si≤0.08%, 0.2%≤Mn≤0.40%, 0.016%≤P≤0.019%, 0.003%≤S≤0.004%, 0.015%≤Al≤0.035%.
3. The strapping tape according to claim 1, characterized in that: The thickness of the protective film is 3 μm to 5 μm.
4. The strapping tape according to claim 1, characterized in that: The material of the protective film includes water-soluble resin; the water-soluble resin includes one or more of water-based acrylic resin, water-based polyurethane resin, water-based epoxy-modified acrylic resin, and acrylic-modified saturated polyester resin.
5. The strapping tape according to any one of claims 1 to 4, characterized in that: The packing tape has a thickness of 0.7 mm to 1.0 mm and a width of 31.75 ± 0.13 mm.
6. The strapping tape according to claim 5, characterized in that: The tensile strength of the strapping tape is above 700 MPa, and the elongation A 30mm It is more than 12%.
7. The strapping tape according to claim 6, characterized in that: The tensile strength of the strapping tape is 752MPa-778MPa, and the elongation A 30mm It is 12.3% to 13.5%.
8. A method for producing a strapping tape according to any one of claims 1 to 7, characterized in that: The method comprises the following steps: the steel coil is subjected to the steps of bluing, cooling, waxing and drying to obtain a packing tape; Wherein, in the bluing step, the bluing temperature is 530°C to 600°C, and the bluing time is 90s to 150s.
9. The method for producing a strapping tape according to claim 8, characterized in that: In the drying step, the drying temperature is 180° C. to 220° C., and the drying speed is 15 m / min to 18 m / min.
10. Use of the strapping tape as claimed in any one of claims 1 to 7 or the strapping tape produced by the production method of strapping tape as claimed in any one of claims 8 to 9 in the field of strapping of steel, metal products or logistics transportation.
Citation Information
Patent Citations
Manufacturing method of high strength bluing strapping steel
CN102719730A
Production method of low-cost cold-rolled steel strip raw material for packing belt
CN113621887A
High tensile strength cold rolled steel sheet having high corrosion resistance and high workability and its production
JP1994272055A
Manufacturing of high toughness steel band for coilbanding
KR1020010060398A