High-entropy nanorod array electrolyzed water catalyst and preparation method thereof
A high entropy nanorod array catalyst is developed using nickel foam as a substrate to enhance the electrochemical performance.
Patent Information
- Application Number
- CN202411500121.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-09-22
- Filing Date
- 2024-10-25
- Publication Date
- 2024-12-06
AI Technical Summary
The hydrogen evolution reaction (HER) in the field of hydrogen production is hindered by the lack of efficient and durable electrocatalysts, particularly polymetallic sulfides, which suffer from poor stability and performance due to their structural limitations, and the need for improved catalysts to enhance the electrochemical performance.
A high entropy nanorod array catalyst is developed using nickel foam as a substrate, which incorporates a solvothermal method to grow polymetallic sulfides on the surface of nickel foam, which enhances the electrochemical performance.
The catalyst exhibits enhanced electrochemical performance and stability, and the catalyst exhibits enhanced electrochemical performance.
Smart Images

Figure CN119082772A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of hydrogen production by electrolysis of water, and in particular to a high entropy nanorod array water electrolysis catalyst and a preparation method thereof. Background Art
[0002] Hydrogen energy has many advantages, such as high energy density, wide range of sources and uses, and adaptability to large-scale energy storage. Using renewable energy to produce green hydrogen through water electrolysis can achieve zero carbon emissions in hydrogen production, which is of great significance for helping to achieve carbon peak and carbon neutrality goals. However, the hydrogen evolution reaction (HER) is a bottleneck that urgently needs to be broken through in the field of water electrolysis to produce hydrogen, and slow kinetics is still a fatal disadvantage. The most effective electrocatalyst for improving HER performance is Pt / C, but its high price and scarce reserves hinder its industrial application. Therefore, there is an urgent need to develop cheap, efficient and durable HER electrocatalysts to replace precious metal catalysts.
[0003] Polymetallic sulfide catalysts have attracted much attention due to their high entropy effect in thermodynamics, lattice distortion effect in structure, slow diffusion effect in kinetics, and cocktail effect in performance. However, in the process of water electrolysis, polymetallic sulfides are restricted by their structure, and metal dissolution and phase separation will inevitably occur, resulting in poor stability. Therefore, it is urgent to design their structure to effectively improve the electrocatalytic activity and stability of polymetallic sulfides. Summary of the invention
[0004] In order to solve the problems existing in the prior art, the main purpose of the present invention is to propose a high entropy nanorod array water electrolysis catalyst and its preparation method, optimize the electronic structure of polymetallic sulfides, and improve the activity and stability of the catalyst in the HER process
[0005] To solve the above technical problems, according to one aspect of the present invention, the present invention provides the following technical solutions:
[0006] A high entropy nanorod array water electrolysis catalyst is disclosed. The catalyst is a (FeCoNiMo)S / NF water electrolysis catalyst, and its morphology is a rod-shaped array.
[0007] To solve the above technical problem, according to another aspect of the present invention, the present invention provides the following technical solution:
[0008] A preparation method of the above-mentioned high entropy nanorod array electrolytic water catalyst, using nickel foam (NF) as a substrate, using a solvothermal method to in-situ grow an iron source, a cobalt source, a nickel source, and a molybdenum source on the surface of the nickel foam into a (FeCoNiMo)OH / NF material with a nanorod array morphology, and then introducing an S source on the surface of the (FeCoNiMo)OH / NF material through an electrochemical reaction and reacting it with a sulfurization reaction to obtain a high entropy nanorod array (FeCoNiMo)S / NF electrolytic water catalyst.
[0009] As a preferred embodiment of the method for preparing the high entropy nanorod array water electrolysis catalyst of the present invention, the preparation method comprises the following steps:
[0010] S1. Ultrasonic cleaning of NF, drying and vacuum storage for later use;
[0011] S2, dissolving the iron source, cobalt source, nickel source and molybdenum source in a solvent, and ultrasonically mixing until completely dissolved to form a solution A;
[0012] S3, placing solution A and NF in a reactor and ultrasonicating them, and then reacting them at a certain temperature. After the reaction is completed, washing and drying are performed to obtain (FeCoNiMo)OH / NF material;
[0013] S4. Using (FeCoNiMo)OH / NF material as the working electrode and sodium sulfate solution as the electrolyte, after reacting for a period of time in the CV (cyclic voltammetry) mode, a high entropy nanorod array (FeCoNiMo)S / NF water electrolysis catalyst was obtained after washing and drying.
[0014] As a preferred embodiment of the method for preparing the high entropy nanorod array water electrolysis catalyst described in the present invention, wherein: in the step S2, the iron source, cobalt source, nickel source, and molybdenum source are respectively derived from ferric nitrate, cobalt nitrate, nickel nitrate, and ammonium molybdate, and the molar ratio of iron, cobalt, nickel, and molybdenum in the iron source, cobalt source, nickel source, and molybdenum source is (2.5-5.5):(2.0-4.5):(1.5-3.5):(1.5-3.0).
[0015] As a preferred embodiment of the method for preparing the high entropy nanorod array water electrolysis catalyst of the present invention, wherein: in the step S3, the reaction temperature is 95 to 125° C., and the reaction time is 18 to 24 hours.
[0016] As a preferred embodiment of the method for preparing the high entropy nanorod array water electrolysis catalyst of the present invention, wherein: in the step S4, the concentration of the sodium sulfate is 1.5 to 4.5 mol / L.
[0017] As a preferred embodiment of the method for preparing the high entropy nanorod array water electrolysis catalyst of the present invention, wherein: in the step S4, the CV voltage window is -0.2 to 1.4 V, the scan rate is 0.005 to 0.1 V / s, and the number of cycles is 1500 to 3000.
[0018] To solve the above technical problem, according to another aspect of the present invention, the present invention provides the following technical solution:
[0019] An application of the above-mentioned high entropy nanorod array water electrolysis catalyst in the field of water electrolysis.
[0020] The beneficial effects of the present invention are as follows:
[0021] The present invention provides a high entropy nanorod array electrolytic water catalyst and a preparation method thereof. With nickel foam (NF) as a substrate, a solvothermal method is used to in-situ grow an iron source, a cobalt source, a nickel source, and a molybdenum source on the surface of the nickel foam into a nanorod array morphology (FeCoNiMo)OH / NF material, and then an S source is introduced on the surface of the (FeCoNiMo)OH / NF material by an electrochemical reaction and undergoes a sulfurization reaction to obtain a high entropy nanorod array (FeCoNiMo)S / NF electrolytic water catalyst. The present invention optimizes the electronic structure of multimetallic sulfides, improves the activity and stability of the catalyst in the HER process, and improves the electrolytic water performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0023] Figure 1 This is a SEM image of the catalyst prepared in Example 1 of the present invention;
[0024] Figure 2 The linear sweep voltammetry curves of the catalysts prepared in the embodiments and comparative examples of the present invention are shown in FIG.
[0025] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0026] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] The main purpose of the present invention is to provide a high entropy nanorod array water electrolysis catalyst and a preparation method thereof, which has at least the following advantages:
[0028] (1) The catalyst prepared by the present invention has low raw material cost, short operation cycle, high repeatability and is easy to mass produce.
[0029] (2) The present invention provides a simple preparation method, that is, using nickel foam with good conductivity and rough surface as the substrate, a solvothermal method is used to make iron source, cobalt source, nickel source and molybdenum source grow in situ on the surface of nickel foam into a nanorod array morphology (FeCoNiMo)OH / NF material. Then, an S source is introduced into the surface of the (FeCoNiMo)OH / NF material through an electrochemical reaction and a sulfurization reaction is carried out with it to generate a high entropy nanorod array (FeCoNiMo)S / NF water electrolysis catalytic material. And it is applied to the field of water electrolysis hydrogen production, enriching the synthesis and preparation technology of multi-metal sulfides, and also greatly broadening its commercial application value.
[0030] According to one aspect of the present invention, the present invention provides the following technical solution:
[0031] A high entropy nanorod array water electrolysis catalyst is disclosed. The catalyst is a (FeCoNiMo)S / NF water electrolysis catalyst, and its morphology is a rod-shaped array.
[0032] According to another aspect of the present invention, the present invention provides the following technical solution:
[0033] A preparation method of the above-mentioned high entropy nanorod array electrolytic water catalyst, using nickel foam (NF) as a substrate, using a solvothermal method to in-situ grow an iron source, a cobalt source, a nickel source, and a molybdenum source on the surface of the nickel foam into a (FeCoNiMo)OH / NF material with a nanorod array morphology, and then introducing an S source on the surface of the (FeCoNiMo)OH / NF material through an electrochemical reaction and reacting it with a sulfurization reaction to obtain a high entropy nanorod array (FeCoNiMo)S / NF electrolytic water catalyst.
[0034] Preferably, the preparation method comprises the following steps:
[0035] S1. Cut the NF into 20 mm × 20 mm × 1.5 mm in size, clean them ultrasonically in acid solution, anhydrous ethanol and deionized water in sequence, dry them and store them in vacuum for later use;
[0036] S2, dissolving the iron source, cobalt source, nickel source and molybdenum source in a solvent, and ultrasonically mixing until completely dissolved to form a solution A;
[0037] S3, placing solution A together with a piece of unused NF in a reactor with a capacity of 100 mL for ultrasonication, and then reacting at a certain temperature. After the reaction is completed, the (FeCoNiMo)OH / NF material is obtained after washing and drying;
[0038] S4. Using (FeCoNiMo)OH / NF material as the working electrode and sodium sulfate solution as the electrolyte, after reacting for a period of time in the CV (cyclic voltammetry) mode, a high entropy nanorod array (FeCoNiMo)S / NF water electrolysis catalyst was obtained after washing and drying.
[0039] Preferably, in step S1, the acid solution is hydrochloric acid, and the concentration is 1.5 to 4.5 mol / L.
[0040] Preferably, in step S1, the ultrasonic cleaning time is 0.5 to 1.5 hours.
[0041] Preferably, in step S2, the iron source, cobalt source, nickel source and molybdenum source are respectively derived from ferric nitrate, cobalt nitrate, nickel nitrate and ammonium molybdate, and the molar ratio of iron, cobalt, nickel and molybdenum in the iron source, cobalt source, nickel source and molybdenum source is (2.5-5.5):(2.0-4.5):(1.5-3.5):(1.5-3.0).
[0042] Preferably, in step S3, the reaction temperature is 95-125° C. and the reaction time is 18-24 h.
[0043] Preferably, in step S4, the concentration of sodium sulfate is 1.5 to 4.5 mol / L.
[0044] Preferably, in step S4, the CV voltage window is -0.2 to 1.4 V, the scan rate is 0.005 to 0.1 V / s, and the number of turns is 1500 to 3000 turns.
[0045] According to another aspect of the present invention, the present invention provides the following technical solution:
[0046] An application of the above-mentioned high entropy nanorod array water electrolysis catalyst in the field of water electrolysis.
[0047] The technical solution of the present invention is further described below in conjunction with specific embodiments.
[0048] Example 1
[0049] A preparation method of a high entropy nanorod array water electrolysis catalyst comprises: cutting the NF into a size of 20 mm×20 mm×1.5 mm, ultrasonically cleaning in a 3.0 mol / L HCl solution, anhydrous ethanol, and deionized water for 1 h, and vacuum storing the mixture after drying for later use; weighing 1.01 g Fe(NO3)3·6H2O, 1.451 g Co(NO3)2·6H2O, 1.566 g Ni(NO3)2·6H2O, 1.328 g (NH4)6Mo7O 24Place in deionized water, ultrasonically mix until completely dissolved to form solution A; put the above solution A together with a piece of NF to be used into a reactor with a capacity of 100 mL, ultrasonically mix for a period of time, react at 100°C for 20 hours, and after the reaction is completed, wash and dry to obtain (FeCoNiMo)OH / NF material; use the above (FeCoNiMo)OH / NF material as the working electrode, 1.5 mol / L sodium sulfate solution as the electrolyte, react in the CV (cyclic voltammetry) mode at a voltage window of -0.2 to 1.4 V and a scan rate of 0.005 V / s for 1500 cycles, and then wash and dry to obtain a high entropy nanorod array (FeCoNiMo)S / NF water electrolysis catalyst, the SEM image of which is shown in the figure Figure 1 As shown, the catalyst morphology is a rod-shaped array.
[0050] Example 2
[0051] The difference from Example 1 is that the concentration of hydrochloric acid used during ultrasonic cleaning is different:
[0052] The NF was cut into 20 mm × 20 mm × 1.5 mm in size and ultrasonically cleaned in 2.0 mol / L HCl solution, anhydrous ethanol, and deionized water for 1 h, respectively. After drying, it was stored in a vacuum chamber for later use. 1.01 g Fe(NO3)3·6H2O, 1.451 g Co(NO3)2·6H2O, 1.566 g Ni(NO3)2·6H2O, 1.328 g (NH4)6Mo7O 24 Place it in deionized water and mix it ultrasonically until it is completely dissolved to form solution A; put the above solution A together with a piece of NF to be used into a reactor with a capacity of 100 mL, after ultrasonication for a period of time, react at 100°C for 20 hours. After the reaction is completed, wash and dry to obtain (FeCoNiMo)OH / NF material; use the above (FeCoNiMo)OH / NF material as the working electrode and 1.5 mol / L sodium sulfate solution as the electrolyte, react 1500 cycles in the CV (cyclic voltammetry) mode at a voltage window of -0.2 to 1.4 V and a scan rate of 0.005 V / s, and then wash and dry to obtain a high entropy nanorod array (FeCoNiMo)S / NF water electrolysis catalyst.
[0053] Example 3
[0054] The difference from Example 1 is that Fe(NO3)3·6H2O, Co(NO3)2·6H2O, Ni(NO3)2·6H2O, (NH4)6Mo7O 24 The dosage is different:
[0055] The NF was cut into 20 mm × 20 mm × 1.5 mm in size and ultrasonically cleaned in 3.0 mol / L HCl solution, anhydrous ethanol, and deionized water for 1 h, respectively. After drying, it was stored in a vacuum chamber for later use. 1.06 g Fe(NO3)3·6H2O, 1.551 g Co(NO3)2·6H2O, 1.672 g Ni(NO3)2·6H2O, 1.323 g (NH4)6Mo7O 24 Place it in deionized water and mix it ultrasonically until it is completely dissolved to form solution A; put the above solution A together with a piece of NF to be used into a reactor with a capacity of 100 mL, after ultrasonication for a period of time, react at 100°C for 20 hours. After the reaction is completed, wash and dry to obtain (FeCoNiMo)OH / NF material; use the above (FeCoNiMo)OH / NF material as the working electrode and 1.5 mol / L sodium sulfate solution as the electrolyte, react 1500 cycles in the CV (cyclic voltammetry) mode at a voltage window of -0.2 to 1.4 V and a scan rate of 0.005 V / s, and then wash and dry to obtain a high entropy nanorod array (FeCoNiMo)S / NF water electrolysis catalyst.
[0056] Example 4
[0057] The difference from Example 1 is that the hydrothermal reaction temperature and time are different:
[0058] The NF was cut into 20 mm × 20 mm × 1.5 mm in size and ultrasonically cleaned in 3.0 mol / L HCl solution, anhydrous ethanol, and deionized water for 1 h, respectively. After drying, it was stored in a vacuum chamber for later use. 1.01 g Fe(NO3)3·6H2O, 1.451 g Co(NO3)2·6H2O, 1.566 g Ni(NO3)2·6H2O, 1.328 g (NH4)6Mo7O 24 Place it in deionized water and mix it ultrasonically until it is completely dissolved to form solution A; put the above solution A together with a piece of NF to be used into a reactor with a capacity of 100 mL, after ultrasonication for a period of time, react at 110°C for 22 hours. After the reaction is completed, wash and dry to obtain (FeCoNiMo)OH / NF material; use the above (FeCoNiMo)OH / NF material as the working electrode and 1.5 mol / L sodium sulfate solution as the electrolyte, react 1500 cycles in the CV (cyclic voltammetry) mode at a voltage window of -0.2 to 1.4 V and a scan rate of 0.005 V / s, and then wash and dry to obtain a high entropy nanorod array (FeCoNiMo)S / NF water electrolysis catalyst.
[0059] Example 5
[0060] The difference from Example 1 is that the concentration of electrolyte sodium sulfate used in the electrochemical reaction is different:
[0061] The NF was cut into 20 mm × 20 mm × 1.5 mm in size and ultrasonically cleaned in 3.0 mol / L HCl solution, anhydrous ethanol, and deionized water for 1 h, respectively. After drying, it was stored in a vacuum chamber for later use. 1.01 g Fe(NO3)3·6H2O, 1.451 g Co(NO3)2·6H2O, 1.566 g Ni(NO3)2·6H2O, 1.328 g (NH4)6Mo7O 24 Place it in deionized water and mix it ultrasonically until it is completely dissolved to form solution A; put the above solution A together with a piece of NF to be used into a reactor with a capacity of 100 mL, after ultrasonication for a period of time, react at 100°C for 20 hours. After the reaction is completed, wash and dry to obtain (FeCoNiMo)OH / NF material; use the above (FeCoNiMo)OH / NF material as the working electrode and 2.0 mol / L sodium sulfate solution as the electrolyte, react 1500 cycles in the CV (cyclic voltammetry) mode at a voltage window of -0.2 to 1.4 V and a scan rate of 0.005 V / s, and then wash and dry to obtain a high entropy nanorod array (FeCoNiMo)S / NF water electrolysis catalyst.
[0062] Example 6
[0063] The difference from Example 1 is that the number of cycles during the electrochemical reaction is different:
[0064] The NF was cut into 20 mm × 20 mm × 1.5 mm in size and ultrasonically cleaned in 3.0 mol / L HCl solution, anhydrous ethanol, and deionized water for 1 h, respectively. After drying, it was stored in a vacuum chamber for later use. 1.01 g Fe(NO3)3·6H2O, 1.451 g Co(NO3)2·6H2O, 1.566 g Ni(NO3)2·6H2O, 1.328 g (NH4)6Mo7O 24 Place it in deionized water and mix it ultrasonically until it is completely dissolved to form solution A; put the above solution A together with a piece of NF to be used into a reactor with a capacity of 100 mL, after ultrasonication for a period of time, react at 100°C for 20 hours. After the reaction is completed, wash and dry to obtain (FeCoNiMo)OH / NF material; use the above (FeCoNiMo)OH / NF material as the working electrode and 1.5 mol / L sodium sulfate solution as the electrolyte, react for 2000 cycles in the CV (cyclic voltammetry) mode at a voltage window of -0.2 to 1.4 V and a scan rate of 0.005 V / s, and then wash and dry to obtain a high entropy nanorod array (FeCoNiMo)S / NF water electrolysis catalyst.
[0065] Comparative Example 1
[0066] The difference from Example 1 is that Fe(NO3)3·6H2O, Co(NO3)2·6H2O, Ni(NO3)2·6H2O, (NH4)6Mo7O 24 The dosage is different:
[0067] The NF was cut into 20 mm × 20 mm × 1.5 mm in size and ultrasonically cleaned in 3.0 mol / L HCl solution, anhydrous ethanol, and deionized water for 1 h, respectively. After drying, it was stored in a vacuum chamber for later use. 5.06 g Fe(NO3)3·6H2O, 6.551 g Co(NO3)2·6H2O, 6.672 g Ni(NO3)2·6H2O, and 7.323 g (NH4)6Mo7O were weighed. 24 Place in deionized water, mix ultrasonically until completely dissolved to form solution A; put the above solution A together with a piece of NF to be used into a reactor with a capacity of 100 mL, after ultrasonication for a period of time, react at 100°C for 20 hours, after the reaction is completed, wash and dry to obtain (FeCoNiMo)OH / NF material; use the above (FeCoNiMo)OH / NF material as the working electrode, 1.5 mol / L sodium sulfate solution as the electrolyte, in the voltage window of -0.2 to 1.4 V, at a scan rate of 0.005 V / s, react for 1500 cycles in CV (cyclic voltammetry) mode, and then wash and dry to obtain the product.
[0068] Comparative Example 2
[0069] The difference from Example 1 is that the hydrothermal reaction temperature and time are different:
[0070] The NF was cut into 20 mm × 20 mm × 1.5 mm in size and ultrasonically cleaned in 3.0 mol / L HCl solution, anhydrous ethanol, and deionized water for 1 h, respectively. After drying, it was stored in a vacuum chamber for later use. 1.01 g Fe(NO3)3·6H2O, 1.451 g Co(NO3)2·6H2O, 1.566 g Ni(NO3)2·6H2O, 1.328 g (NH4)6Mo7O 24 Place in deionized water, mix ultrasonically until completely dissolved to form solution A; put the above solution A together with a piece of NF to be used into a reactor with a capacity of 100 mL, after ultrasonication for a period of time, react at 50°C for 15 hours, after the reaction is completed, wash and dry to obtain (FeCoNiMo)OH / NF material; use the above (FeCoNiMo)OH / NF material as the working electrode, 1.5 mol / L sodium sulfate solution as the electrolyte, in the voltage window of -0.2 to 1.4 V, at a scan rate of 0.005 V / s, react for 1500 cycles in CV (cyclic voltammetry) mode, and then wash and dry to obtain the product.
[0071] Comparative Example 3
[0072] The difference from Example 1 is that the concentration of electrolyte sodium sulfate used in the electrochemical reaction is different:
[0073] The NF was cut into 20 mm × 20 mm × 1.5 mm in size and ultrasonically cleaned in 3.0 mol / L HCl solution, anhydrous ethanol, and deionized water for 1 h, respectively. After drying, it was stored in a vacuum chamber for later use. 1.01 g Fe(NO3)3·6H2O, 1.451 g Co(NO3)2·6H2O, 1.566 g Ni(NO3)2·6H2O, 1.328 g (NH4)6Mo7O 24 Place in deionized water, mix ultrasonically until completely dissolved to form solution A; put the above solution A together with a piece of NF to be used into a reactor with a capacity of 100 mL, after ultrasonication for a period of time, react at 100°C for 20 hours, after the reaction is completed, wash and dry to obtain (FeCoNiMo)OH / NF material; use the above (FeCoNiMo)OH / NF material as the working electrode, 6.5 mol / L sodium sulfate solution as the electrolyte, in the voltage window of -0.2 to 1.4 V, at a scan rate of 0.005 V / s, react for 1500 cycles in CV (cyclic voltammetry) mode, and then wash and dry to obtain the product.
[0074] Comparative Example 4
[0075] The difference from Example 1 is that the number of cycles during the electrochemical reaction is different:
[0076] The NF was cut into 20 mm × 20 mm × 1.5 mm in size and ultrasonically cleaned in 3.0 mol / L HCl solution, anhydrous ethanol, and deionized water for 1 h, respectively. After drying, it was stored in a vacuum chamber for later use. 1.01 g Fe(NO3)3·6H2O, 1.451 g Co(NO3)2·6H2O, 1.566 g Ni(NO3)2·6H2O, 1.328 g (NH4)6Mo7O 24 Place in deionized water, mix ultrasonically until completely dissolved to form solution A; put the above solution A together with a piece of NF to be used into a reactor with a capacity of 100 mL, after ultrasonication for a period of time, react at 100°C for 20 hours, after the reaction is completed, wash and dry to obtain (FeCoNiMo)OH / NF material; use the above (FeCoNiMo)OH / NF material as the working electrode, 1.5 mol / L sodium sulfate solution as the electrolyte, in the voltage window of -0.2 to 1.4 V, at a scan rate of 0.005 V / s, react for 6500 cycles in CV (cyclic voltammetry) mode, and then wash and dry to obtain the product.
[0077] The electrochemical properties of the products prepared in Examples 1-6 and Comparative Examples 1-4 were detected by linear voltammetry to obtain the electrolytic water hydrogen evolution properties, as shown in FIG. Figure 2 As shown. Figure 2 From the linear sweep voltammetric curve, at the same current density, the hydrogen evolution overpotential of Examples 1-6 is much smaller than that of Comparative Examples 1-4. This shows that the present invention uses nickel foam with good conductivity and rough surface as the substrate, and adopts a solvothermal method to make the iron source, cobalt source, nickel source, and molybdenum source grow in situ on the surface of nickel foam into a nanorod array morphology (FeCoNiMo)OH / NF material. Then, an S source is introduced into the surface of the (FeCoNiMo)OH / NF material through an electrochemical reaction and a sulfurization reaction occurs with it to generate a high entropy nanorod array (FeCoNiMo)S / NF water electrolysis catalytic material, thereby achieving low energy consumption and high hydrogen evolution efficiency of the water electrolysis hydrogen production membrane electrode; at the same time, Comparative Examples 1-2 can no longer continue to produce hydrogen by water electrolysis at a higher current density, which shows that the nanorod array (FeCoNiMo)S / NF water electrolysis catalyst of the present invention can achieve high current density water electrolysis hydrogen production.
[0078] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. A high entropy nanorod array water electrolysis catalyst, characterized in that: The catalyst is a (FeCoNiMo)S / NF water electrolysis catalyst, and its morphology is a rod array.
2. A method for preparing the high entropy nanorod array water electrolysis catalyst according to claim 1, characterized in that: Taking NF as the substrate, a solvothermal method was used to in situ grow iron source, cobalt source, nickel source and molybdenum source on the surface of nickel foam to form a nanorod array morphology (FeCoNiMo)OH / NF material. Then, an S source was introduced into the surface of the (FeCoNiMo)OH / NF material through an electrochemical reaction and a sulfurization reaction occurred with it to obtain a high entropy nanorod array (FeCoNiMo)S / NF water electrolysis catalyst.
3. The method for preparing a high entropy nanorod array water electrolysis catalyst according to claim 2, characterized in that: The preparation method comprises the following steps: S1. Ultrasonic cleaning of NF, drying and vacuum storage for later use; S2, dissolving the iron source, cobalt source, nickel source and molybdenum source in a solvent, and ultrasonically mixing until completely dissolved to form a solution A; S3, placing solution A and NF in a reactor and ultrasonicating them, and then reacting them at a certain temperature. After the reaction is completed, washing and drying are performed to obtain (FeCoNiMo)OH / NF material; S4. Using (FeCoNiMo)OH / NF material as the working electrode and sodium sulfate solution as the electrolyte, after reacting in CV mode for a period of time, a high entropy nanorod array (FeCoNiMo)S / NF water electrolysis catalyst was obtained after washing and drying.
4. The method for preparing a high entropy nanorod array water electrolysis catalyst according to claim 3, characterized in that: In step S2, the iron source, cobalt source, nickel source and molybdenum source are respectively derived from ferric nitrate, cobalt nitrate, nickel nitrate and ammonium molybdate, and the molar ratio of iron, cobalt, nickel and molybdenum in the iron source, cobalt source, nickel source and molybdenum source is (2.5-5.5):(2.0-4.5):(1.5-3.5):(1.5-3.0).
5. The method for preparing a high entropy nanorod array water electrolysis catalyst according to claim 3, characterized in that: In step S3, the reaction temperature is 95-125° C., and the reaction time is 18-24 hours.
6. The method for preparing a high entropy nanorod array water electrolysis catalyst according to claim 3, characterized in that: In step S4, the concentration of sodium sulfate is 1.5-4.5 mol / L.
7. The method for preparing a high entropy nanorod array water electrolysis catalyst according to claim 3, characterized in that: In step S4, the CV voltage window is -0.2 to 1.4 V, the scanning speed is 0.005 to 0.1 V / s, and the number of turns is 1500 to 3000 turns.
8. Use of the high entropy nanorod array water electrolysis catalyst according to claim 1 in the field of water electrolysis.
Citation Information
Cited By
Preparation method of high-entropy FeCoNiCuS homojunction electrocatalyst and preparation method and application of high-entropy FeCoNiCuS homojunction electrocatalyst