MIL-77 and ZIF-67-PA composite material as well as preparation method and application thereof
Through the preparation of MIL-77 and ZIF-67-PA composite materials and electron beam irradiation technology, the complexity and structural stability of the ZIF-67 electrolytic catalyst synthesis are solved, and the performance optimization and industrial application of the catalyst are achieved, which is significantly improved. Improves electrochemical reaction efficiency.
Patent Information
- Application Number
- CN202410997042.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-12-06
AI Technical Summary
The existing ZIF-67 electrolytic catalyst synthesis method is complex, costly, and easy to aggregate structure, resulting in limited catalytic performance and industrial application, and its structure is unstable under extreme conditions and limited active sites.
Using the preparation method of MIL-77 and ZIF-67-PA composite material, MIL-77 reacts with cobalt salt and dimethylimidazole in a solvent, phytic acid is added to form a hollow structure nanomaterial, and electron beam irradiation is performed. , optimize material morphology and performance.
The specific surface area of the material is increased and the active sites are abundant, which significantly improves the catalytic potential. It shows excellent electrochemical performance in hydrogen evolution and oxygen evolution reactions, reduces overpotential and increases current density, and provides a high-performance electrolytic catalyst. design ideas.
Smart Images

Figure CN119082795A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of novel hydrogen energy conversion, and in particular to a candied haws-shaped hollow composite material of MIL-77 and ZIF-67-PA, a preparation method and application thereof. Background Art
[0002] Faced with the continuous rise in global energy demand and the intensification of environmental pollution problems, it is urgent to seek clean, renewable and sustainable energy alternatives. Hydrogen energy, with its significant advantages of high energy density and zero emissions, has become an ideal candidate for solving future energy crises and environmental pollution problems. Among hydrogen energy production technologies, electrochemical water splitting stands out. It is easy to operate, has high product purity and a sustainable process. It is regarded as a key way to prepare high-purity hydrogen and leads the future development of the hydrogen energy industry.
[0003] In the process of water electrolysis, hydrogen evolution reaction (HER) and oxygen evolution reaction (OER) are the core technologies, which realize the efficient conversion between chemical energy and electrical energy through the electrolysis device. However, the efficiency and economy of this conversion process are highly dependent on efficient water electrolysis catalysts. Therefore, the current research focus in the field of water electrolysis is on the development of low-cost, abundant resource reserves and excellent catalytic performance bifunctional water electrolysis catalyst materials.
[0004] Transition metal-based metal organic frameworks (MOFs) materials have shown great application potential in the field of water electrolysis catalysts due to their unique structural advantages and rich adjustability. Among them, ZIF-67, as a cobalt-based metal organic framework, is particularly eye-catching. The strong synergistic effect between its internal cobalt ions and dimethylimidazole ligands (2-MIM) gives ZIF-67 extremely high chemical stability, which can maintain structural integrity in a variety of solvents while showing good electrical conductivity. Even without high-temperature annealing treatment, it has a certain inherent conductivity.
[0005] However, the current methods for synthesizing ZIF-67, such as hard template method, soft template method and self-template method, generally have the disadvantages of complex operation, high cost and long preparation cycle, which limits its application in large-scale industrial production. In addition, ZIF-67 is easily aggregated into large pieces during the preparation process, resulting in the loss of its unique porous structure, and this aggregation phenomenon greatly reduces the efficiency of its electrochemical catalytic performance and other potential applications. Secondly, although ZIF-67 shows high stability in most cases, its structure may be damaged under certain extreme conditions (such as strong acid environment), affecting the overall performance of the material. In addition, when ZIF-67 is used alone, its function is often limited by its own physicochemical properties. For example, in the field of catalysis, although ZIF-67 has certain catalytic activity, its active sites are limited, resulting in its low catalytic efficiency. Summary of the invention
[0006] In order to overcome the deficiencies of the prior art and realize a simpler, more efficient and cost-controlled ZIF-67 synthesis method, the present invention provides a composite material of MIL-77 and ZIF-67-PA, a preparation method and application thereof.
[0007] The first aspect of the present invention is to provide a method for preparing a composite material of MIL-77 and ZIF-67-PA, the steps comprising:
[0008] Provides MIL-77;
[0009] Mixing MIL-77 and a dispersant in a first solvent to obtain a first solution;
[0010] Cobalt (Co 2+ ) salt and dimethylimidazole are added to the first solution, mixed and reacted to obtain MIL-77@ZIF-67; MIL-77@ZIF-67 and phytic acid (PA, 1,2,3,4,5,6-hexaphosphoric acid) are mixed in the second solvent to obtain MIL-77@ZIF-67-PA, that is, the MIL-77 and ZIF-67-PA composite material.
[0011] Preferably, MIL-77@ZIF-67-PA is also irradiated under electron beam.
[0012] Preferably, the MIL-77 is a nickel-based metal organic framework material.
[0013] Preferably, the structure of the MIL-77 is in the shape of a long strip.
[0014] Preferably, the MIL-77 is in the shape of a nano-scale ribbon, and its length is preferably 1-10 μm, more preferably 2-8 μm, and more preferably 3-6 μm.
[0015] Preferably, the width of the MIL-77 is 0.2-1 μm, more preferably 0.3-0.8 μm, and more preferably 0.5-0.7 μm.
[0016] Preferably, the thickness of the MIL-77 is 0.06-0.35 μm, preferably 0.08-0.25 μm, and more preferably 0.10-0.20 μm.
[0017] In a preferred embodiment, the synthesis method of MIL-77 comprises the following steps:
[0018] Glutaric acid and nickel (Ni 2+ ) salts are mixed and reacted under alkaline conditions to obtain MIL-77.
[0019] Preferably, the glutaric acid and nickel (Ni 2+ ) The reaction temperature of the salt is 100-300°C, preferably 120-280°C, more preferably 150-180°C.
[0020] Preferably, the glutaric acid and nickel (Ni 2+ ) salt reaction time is 3-64h, preferably 12-50h, more preferably 24-48h.
[0021] Preferably, the alkaline condition is provided by an aqueous solution or an alcohol solution containing a base.
[0022] More preferably, the base is selected from one or more of sodium hydroxide (NaOH), potassium hydroxide (KOH), and aqueous ammonia (NH 3 ·H 2 O).
[0023] More preferably, the concentration of the base (in terms of OH - The standard is 0.1-1 mol / L, preferably 0.2-0.8 mol / L, and more preferably 0.4-0.6 mol / L.
[0024] Preferably, the nickel salt may be an inorganic acid salt or an organic acid salt, and is preferably one or more combinations selected from Ni(NO3)2, NiCO3, NiSO4, NiCl2, NiBr2, Ni(CH3COO)2, and Ni(HCOO)2.
[0025] In a preferred embodiment, the MIL-77 is further cleaned, and more preferably, after cleaning, the reaction product is further dried.
[0026] Preferably, the cleaning solvent used for cleaning the MIL-77 is one or more of water, ethanol and methanol.
[0027] Preferably, the drying temperature of MIL-77 is 50-100°C, preferably 55-80°C, more preferably 60-75°C.
[0028] Preferably, the drying time of MIL-77 is 3-48 h, preferably 4-24 h, more preferably 6-12 h.
[0029] Preferably, the first solvent can be one or more of water, alcohol, ether, ester, ketone, halogenated hydrocarbon, aromatic hydrocarbon, and ionic liquid, and is preferably selected from: water, N,N-dimethylformamide, methanol, ethanol, ether, tetrahydrofuran, dichloromethane, carbon tetrachloride, ethyl acetate, acetone, N-methylpyrrolidone, toluene, ionic liquid (such as 1-butyl-3-methylimidazolium hexafluorophosphate) and mixed in one or more combinations of solvents.
[0030] Preferably, the dispersant includes one or more combinations of polyvinyl pyrrolidone (PVP), sodium dodecyl sulfate (SDS), polyethylene glycol (PEG), sodium polystyrene sulfonate (PSS), polyacrylic acid (PAA), and polyethyleneimine (PEI).
[0031] Preferably, in the first solution, the concentration of MIL-77 is 0.1-1 g / L, preferably 0.15-0.4 g / L, and more preferably 0.2-0.3 g / L.
[0032] Preferably, in the first solution, the concentration of the dispersant is 6-20 g / L, preferably 8-15 g / L, more preferably 10-12 g / L.
[0033] In a preferred embodiment, the cobalt (Co 2+ ) salt and dimethylimidazole are added to the first solution. 2+ ) salt and dimethylimidazole are mixed in a third solvent to obtain a second solution.
[0034] Preferably, the first solution and the second solution are mixed and reacted to obtain MIL-77@ZIF-67.
[0035] Preferably, the third solvent can be one or more of water, alcohol, ether, ester, ketone, halogenated hydrocarbon, aromatic hydrocarbon, and ionic liquid, and is preferably selected from: water, N,N-dimethylformamide, methanol, ethanol, ether, tetrahydrofuran, dichloromethane, carbon tetrachloride, ethyl acetate, acetone, N-methylpyrrolidone, toluene, ionic liquid (such as 1-butyl-3-methylimidazolium hexafluorophosphate) and mixed with one or more combinations of solvents.
[0036] In a preferred embodiment, the cobalt (Co 2+ ) salt and dimethylimidazole are added to the first solution, the cobalt (Co 2+ ) salt is added to the third solvent and mixed to obtain a cobalt salt solution;
[0037] Dimethylimidazole is added to the third solvent and mixed to obtain a dimethylimidazole solution.
[0038] Preferably, the cobalt salt solution and the dimethylimidazole solution are added to the first solution, mixed and reacted to obtain MIL-77@ZIF-67.
[0039] Preferably, the cobalt (Co 2+ ) salt can be one or more combinations selected from CoCO3, Co(NO3)2, CoSO4, CoCl2, and CoBr2.
[0040] Preferably, the cobalt salt may be provided in the form of a hydrate, an aqueous solution or an alcohol solution.
[0041] Preferably, the second solvent can be one or more of water, alcohol, ether, ester, ketone, halogenated hydrocarbon, aromatic hydrocarbon, and ionic liquid, and is preferably selected from: water, N,N-dimethylformamide, methanol, ethanol, ether, tetrahydrofuran, dichloromethane, carbon tetrachloride, ethyl acetate, acetone, N-methylpyrrolidone, toluene, ionic liquid (such as 1-butyl-3-methylimidazolium hexafluorophosphate) and mixed in one or more combinations of solvents.
[0042] More preferably, the first solvent and the second solvent may be the same or different.
[0043] In a preferred embodiment, the MIL-77@ZIF-67 is further cleaned, and more preferably, after cleaning, the reaction product is further dried.
[0044] Preferably, the cleaning solvent used for cleaning the MIL-77@ZIF-67 is one or more of water, ethanol and methanol.
[0045] Preferably, the drying temperature of MIL-77@ZIF-67 is 50-100°C, preferably 55-80°C, more preferably 60-75°C.
[0046] Preferably, the drying time of MIL-77@ZIF-67 is 3-48 h, preferably 4-24 h, and more preferably 6-12 h.
[0047] Preferably, the phytic acid may be provided in the form of a solid, an aqueous solution or an alcohol solution.
[0048] More preferably, the alcohol in the alcohol solution of phytic acid is selected from one or more combinations of methanol, ethanol and propanol.
[0049] Preferably, the MIL-77@ZIF-67-PA is a nanomaterial with a hollow structure.
[0050] In a preferred embodiment, MIL-77@ZIF-67-PA is further cleaned, and more preferably, after cleaning, the reaction product is further dried.
[0051] Preferably, the cleaning solvent used for cleaning the MIL-77@ZIF-67-PA is one or more of water, ethanol and methanol.
[0052] Preferably, the drying temperature of MIL-77@ZIF-67-PA is 50-100°C, preferably 55-80°C, and more preferably 60-75°C.
[0053] Preferably, the drying time of MIL-77@ZIF-67-PA is 3-48 h, preferably 4-24 h, and more preferably 6-12 h.
[0054] Preferably, the dose of the electron beam is 50-1500 kGy, preferably 60-1200 kGy, more preferably 70-1000 kGy.
[0055] Specifically, the preset dose of the electron beam is selected from one or more of: 70 kGy, 140 kGy, 280 kGy, 560 kGy, and 840 kGy.
[0056] The second aspect of the present invention is to provide a MIL-77 and ZIF-67-PA composite material.
[0057] In a preferred embodiment, in the MIL-77 and ZIF-67-PA composite material, the mass ratio of MIL-77 to ZIF-67-PA is 1:(5-35), preferably 1:(10-30), and more preferably 1:(15-25).
[0058] In a preferred embodiment, the porosity of the MIL-77 and ZIF-67-PA composite material is 10-40%, preferably 15-35%, and more preferably 20-30%.
[0059] In a preferred embodiment, the pore diameter of the MIL-77 and ZIF-67-PA composite material is 30-100 nm, preferably 40-90 nm, and more preferably 50-80 nm.
[0060] In a preferred embodiment, the particle size of the MIL-77 and ZIF-67-PA composite material is 0.02-0.4 μm, preferably 0.05-0.3 μm, and more preferably 0.1-0.2 μm.
[0061] Preferably, the MIL-77 and ZIF-67-PA are obtained based on the aforementioned preparation method.
[0062] The third aspect of the present invention is to provide an application of a MIL-77 and ZIF-67-PA composite material for use as an electrolytic catalytic material or an electrolytic electrode.
[0063] Preferably, the composite material can be applied in the field of water electrolysis, especially in hydrogen energy production, renewable energy storage, fuel cell technology, environmental protection and water treatment, electrochemical sensors, or detection equipment.
[0064] In this application specification, "MIL-77" is one of the MIL series materials, which is a type of metal organic framework material that has been studied extensively. It forms a three-dimensional framework structure with diamond-shaped channels by coordinating metals (vanadium, iron, aluminum, chromium, nickel, etc.) with terephthalic acid or trimesic acid. MIL-77 has the advantages of large specific surface area, strong chemical activity, fast mass transfer rate, good chemical stability and thermal stability.
[0065] In this application specification, "ZIF-67" is a metal organic framework, which is composed of metal ions and organic ligands (such as 2-methylimidazole Im) connected by coordination bonds to form a three-dimensional network structure.
[0066] In this application specification, "MIL-77@ZIF-67" means that MIL-77 is encapsulated, wrapped or embedded in the pore structure of ZIF-67.
[0067] Compared with the prior art, the beneficial technical effects of the present invention are as follows:
[0068] The invention provides a method for preparing a composite material of MIL-77 and ZIF-67-PA. The method obtains a composite material of MIL-77 and ZIF-67-PA, and achieves dual optimization of material morphology and performance through simple chemical etching and electron beam irradiation technology.
[0069] The present invention uses the strip nickel-based metal organic framework material MIL-77 as the starting template, utilizes phytic acid as an etchant and a phosphorus source, and adopts electron beam irradiation technology to further modify the prepared composite material. By precisely controlling the growth conditions, the ZIF-67 is guided to nucleate uniformly on its surface to form an ordered MIL-77@ZIF-67 composite structure, which not only increases the specific surface area of the material, but also provides abundant active sites, which is beneficial to the penetration of the electrolyte solution and the rapid release of the gas products.
[0070] Moreover, the present invention not only retains the skeleton stability of MIL-77, but also significantly enhances the catalytic potential of the material by introducing phosphorus elements and multi-level structures. In the hydrogen evolution reaction, the overpotential is only 162mV, and the composite material of the present invention can reach 10mAcm -2 In the oxygen evolution reaction test, the overpotential is only 281mV, and the composite material of the present invention can reach 15mAcm -2 of current density.
[0071] In addition, the material of the present invention not only has unique structural advantages and excellent electrochemical properties, but also demonstrates the effective regulation of catalytic activity by irradiation dose, providing new ideas and technical support for the design and application of high-performance water electrolysis catalysts, and has important scientific significance and application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0072] Figure 1 Scanning transmission images of samples at different stages obtained in the embodiments of the present invention: (a) MIL-77; (b) MIL-77@ZIF-67; (c, d) MIL-77@ZIF-67-PA hollow composite structure.
[0073] Figure 2 : These are the Fourier infrared curves of the MIL-77@ZIF-67-PA hollow composite structure after different irradiation doses obtained in the embodiments of the present invention (the abscissa is the wavenumber, and the ordinate is the transmittance).
[0074] Figure 3 The electrochemical hydrogen evolution reaction performance of MIL-77@ZIF-67-PA after irradiation with different doses obtained in the embodiments of the present invention: (a) polarization curve (the horizontal axis is potential, the vertical axis is current density); (b) Tafel slope curve (the vertical axis is overpotential); (c) double layer capacitance curve (the horizontal axis is scan rate); (d) electrochemical impedance spectroscopy.
[0075] Figure 4 The electrochemical oxygen evolution reaction performance of MIL-77@ZIF-67-PA after irradiation with different doses obtained in the embodiments of the present invention: (a) polarization curve (the horizontal axis is potential, the vertical axis is current density); (b) Tafel slope curve (the vertical axis is overpotential); (c) double layer capacitance curve (the horizontal axis is scan rate); (d) electrochemical impedance spectroscopy. DETAILED DESCRIPTION
[0076] The embodiments of the present invention provide a MIL-77 and ZIF-67-PA composite material, a preparation method and an application thereof. In order to make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail with reference to the accompanying drawings and examples. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0077] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged under appropriate circumstances. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0078] Example 1
[0079] (1) Synthesis of nickel-based metal organic framework material (MIL-77) nanobelts: 0.39 g glutaric acid (HOOC(CH3)3COOH), 0.23 g potassium hydroxide (KOH), and 0.50 g nickel acetate tetrahydrate were dissolved in a mixed solution of ethanol and water with a volume ratio of 1:1. After mixing evenly, 2 mL of sodium hydroxide aqueous solution (0.4 M) was added and stirred evenly, poured into a 50 mL stainless steel autoclave with Telfon lining and kept in an oven at 180°C for 48 h. After the reaction was completed, the product was collected by centrifugation and washed with ethanol several times, and then placed in a vacuum drying oven at 60°C for 12 h to obtain a green solid product, namely MIL-77.
[0080] (2) Synthesis of MIL-77 and cobalt-based metal organic framework (ZIF-67) composite material (MIL-77@ZIF-67): 15 mg of MIL-77 was dissolved in 50 mL of methanol, and 500 mg of polyvinyl pyrrolidone (PVP) was added and ultrasonically dispersed. 0.40 g of Co(NO3)2·6H2O was dissolved in 50 mL of methanol to prepare solution A, and 5.90 g of dimethylimidazole was dissolved in 100 mL of methanol to prepare solution B. Solutions A and B were added to the dispersion of MIL-77, stirred at room temperature for 2 h, and the purple product was collected by centrifugation and washing, which was MIL-77@ZIF-67.
[0081] (3) Synthesis of MIL-77@ZIF-67-PA (PA: phytic acid) hollow structure composite material: 50 mg of MIL-77@ZIF-67 was dispersed in 50 mL of ethanol, 10 mL of phytic acid ethanol solution was added, stirred for 1 h, centrifuged and washed, and dried in a vacuum drying oven for 12 h to obtain a lavender powder, which is the MIL-77@ZIF-67-PA hollow nanomaterial. The MIL-77@ZIF-67-PA of this example was not irradiated with an electron beam and was recorded as MIL-77@ZIF-67-PA-0 kGy.
[0082] Example 2
[0083] (1) Synthesis of nickel-based metal organic framework material (MIL-77) nanobelts: 0.39 g glutaric acid (HOOC(CH3)3COOH), 0.23 g potassium hydroxide (KOH), and 0.50 g nickel acetate tetrahydrate were dissolved in a mixed solution of ethanol and water with a volume ratio of 1:1. After mixing evenly, 2 mL of sodium hydroxide aqueous solution (0.4 M) was added and stirred evenly, poured into a 50 mL stainless steel autoclave with Telfon lining and kept in an oven at 180°C for 48 h. After the reaction was completed, the product was collected by centrifugation and washed with ethanol several times, and then placed in a vacuum drying oven at 60°C for 12 h to obtain a green solid product, namely MIL-77.
[0084] (2) Synthesis of MIL-77 and cobalt-based metal organic framework (ZIF-67) composite material (MIL-77@ZIF-67): 15 mg of MIL-77 was dissolved in 50 mL of methanol, and 500 mg of polyvinyl pyrrolidone (PVP) was added and ultrasonically dispersed. 0.40 g of Co(NO3)2·6H2O was dissolved in 50 mL of methanol to prepare solution A, and 5.90 g of dimethylimidazole was dissolved in 100 mL of methanol to prepare solution B. Solutions A and B were added to the dispersion of MIL-77, stirred at room temperature for 2 h, and the purple product was collected by centrifugation and washing, which was MIL-77@ZIF-67.
[0085] (3) Synthesis of MIL-77@ZIF-67-PA (PA: phytic acid) hollow structure composite material: 50 mg of MIL-77@ZIF-67 was dispersed in 50 mL of ethanol, 10 mL of phytic acid ethanol solution was added, stirred for 1 h, centrifuged and washed, and dried in a vacuum oven for 12 h to obtain a lavender powder, which is the MIL-77@ZIF-67-PA hollow nanomaterial. The synthesized MIL-77@ZIF-67-PA was irradiated in an electron beam accelerator with an irradiation dose of 70 kGy. The irradiated MIL-77@ZIF-67-PA was abbreviated as MIL-77@ZIF-67-PA-70 kGy.
[0086] Example 3
[0087] (1) Synthesis of nickel-based metal organic framework material (MIL-77) nanobelts: 0.39 g glutaric acid (HOOC(CH3)3COOH), 0.23 g potassium hydroxide (KOH), and 0.50 g nickel acetate tetrahydrate were dissolved in a mixed solution of ethanol and water with a volume ratio of 1:1. After mixing evenly, 2 mL of sodium hydroxide aqueous solution (0.4 M) was added and stirred evenly, poured into a 50 mL stainless steel autoclave with Telfon lining and kept in an oven at 180°C for 48 h. After the reaction was completed, the product was collected by centrifugation and washed with ethanol several times, and then placed in a vacuum drying oven at 60°C for 12 h to obtain a green solid product, namely MIL-77.
[0088] (2) Synthesis of MIL-77 and cobalt-based metal organic framework (ZIF-67) composite material (MIL-77@ZIF-67): 15 mg of MIL-77 was dissolved in 50 mL of methanol, and 500 mg of polyvinyl pyrrolidone (PVP) was added and ultrasonically dispersed. 0.40 g of Co(NO3)2·6H2O was dissolved in 50 mL of methanol to prepare solution A, and 5.90 g of dimethylimidazole was dissolved in 100 mL of methanol to prepare solution B. Solutions A and B were added to the dispersion of MIL-77, stirred at room temperature for 2 h, and the purple product was collected by centrifugation and washing, which was MIL-77@ZIF-67.
[0089] (3) Synthesis of MIL-77@ZIF-67-PA (PA: phytic acid) hollow structure composite material: 50 mg of MIL-77@ZIF-67 was dispersed in 50 mL of ethanol, 10 mL of phytic acid ethanol solution was added, stirred for 1 h, centrifuged and washed, and dried in a vacuum oven for 12 h to obtain a lavender powder, which is the MIL-77@ZIF-67-PA hollow nanomaterial. The synthesized MIL-77@ZIF-67-PA was irradiated in an electron beam accelerator with an irradiation dose of 140 kGy. The irradiated MIL-77@ZIF-67-PA is abbreviated as MIL-77@ZIF-67-PA-140 kGy.
[0090] Example 4
[0091] (1) Synthesis of nickel-based metal organic framework material (MIL-77) nanobelts: 0.39 g glutaric acid (HOOC(CH3)3COOH), 0.23 g potassium hydroxide (KOH), and 0.50 g nickel acetate tetrahydrate were dissolved in a mixed solution of ethanol and water with a volume ratio of 1:1. After mixing evenly, 2 mL of sodium hydroxide aqueous solution (0.4 M) was added and stirred evenly, poured into a 50 mL stainless steel autoclave with Telfon lining and kept in an oven at 180°C for 48 h. After the reaction was completed, the product was collected by centrifugation and washed with ethanol several times, and then placed in a vacuum drying oven at 60°C for 12 h to obtain a green solid product, namely MIL-77.
[0092] (2) Synthesis of MIL-77 and cobalt-based metal organic framework (ZIF-67) composite material (MIL-77@ZIF-67): 15 mg of MIL-77 was dissolved in 50 mL of methanol, and 500 mg of polyvinyl pyrrolidone (PVP) was added and ultrasonically dispersed. 0.40 g of Co(NO3)2·6H2O was dissolved in 50 mL of methanol to prepare solution A, and 5.90 g of dimethylimidazole was dissolved in 100 mL of methanol to prepare solution B. Solutions A and B were added to the dispersion of MIL-77, stirred at room temperature for 2 h, and the purple product was collected by centrifugation and washing, which was MIL-77@ZIF-67.
[0093] (3) Synthesis of MIL-77@ZIF-67-PA (PA: phytic acid) hollow structure composite material: 50 mg of MIL-77@ZIF-67 was dispersed in 50 mL of ethanol, 10 mL of phytic acid ethanol solution was added, stirred for 1 h, centrifuged and washed, and dried in a vacuum oven for 12 h to obtain a lavender powder, which is the MIL-77@ZIF-67-PA hollow nanomaterial. The synthesized MIL-77@ZIF-67-PA was irradiated in an electron beam accelerator with an irradiation dose of 280 kGy. The irradiated MIL-77@ZIF-67-PA is abbreviated as MIL-77@ZIF-67-PA-280 kGy.
[0094] Example 5
[0095] (1) Synthesis of nickel-based metal organic framework material (MIL-77) nanobelts: 0.39 g glutaric acid (HOOC(CH3)3COOH), 0.23 g potassium hydroxide (KOH), and 0.50 g nickel acetate tetrahydrate were dissolved in a mixed solution of ethanol and water with a volume ratio of 1:1. After mixing evenly, 2 mL of sodium hydroxide aqueous solution (0.4 M) was added and stirred evenly, poured into a 50 mL stainless steel autoclave with Telfon lining and kept in an oven at 180°C for 48 h. After the reaction was completed, the product was collected by centrifugation and washed with ethanol several times, and then placed in a vacuum drying oven at 60°C for 12 h to obtain a green solid product, namely MIL-77.
[0096] (2) Synthesis of MIL-77 and cobalt-based metal organic framework (ZIF-67) composite material (MIL-77@ZIF-67): 15 mg of MIL-77 was dissolved in 50 mL of methanol, and 500 mg of polyvinyl pyrrolidone (PVP) was added and ultrasonically dispersed. 0.40 g of Co(NO3)2·6H2O was dissolved in 50 mL of methanol to prepare solution A, and 5.90 g of dimethylimidazole was dissolved in 100 mL of methanol to prepare solution B. Solutions A and B were added to the dispersion of MIL-77, stirred at room temperature for 2 h, and the purple product was collected by centrifugation and washing, which was MIL-77@ZIF-67.
[0097] (3) Synthesis of MIL-77@ZIF-67-PA (PA: phytic acid) hollow structure composite material: 50 mg of MIL-77@ZIF-67 was dispersed in 50 mL of ethanol, 10 mL of phytic acid ethanol solution was added, stirred for 1 h, centrifuged and washed, and dried in a vacuum oven for 12 h to obtain a lavender powder, which is the MIL-77@ZIF-67-PA hollow nanomaterial. The synthesized MIL-77@ZIF-67-PA was irradiated in an electron beam accelerator with an irradiation dose of 560 kGy. The irradiated MIL-77@ZIF-67-PA is abbreviated as MIL-77@ZIF-67-PA-560 kGy.
[0098] Example 6
[0099] (1) Synthesis of nickel-based metal organic framework material (MIL-77) nanobelts: 0.39 g glutaric acid (HOOC(CH3)3COOH), 0.23 g potassium hydroxide (KOH), and 0.50 g nickel acetate tetrahydrate were dissolved in a mixed solution of ethanol and water with a volume ratio of 1:1. After mixing evenly, 2 mL of sodium hydroxide aqueous solution (0.4 M) was added and stirred evenly, poured into a 50 mL stainless steel autoclave with Telfon lining and kept in an oven at 180°C for 48 h. After the reaction was completed, the product was collected by centrifugation and washed with ethanol several times, and then placed in a vacuum drying oven at 60°C for 12 h to obtain a green solid product, namely MIL-77.
[0100] (2) Synthesis of MIL-77 and cobalt-based metal organic framework (ZIF-67) composite material (MIL-77@ZIF-67): 15 mg of MIL-77 was dissolved in 50 mL of methanol, and 500 mg of polyvinyl pyrrolidone (PVP) was added and ultrasonically dispersed. 0.40 g of Co(NO3)2·6H2O was dissolved in 50 mL of methanol to prepare solution A, and 5.90 g of dimethylimidazole was dissolved in 100 mL of methanol to prepare solution B. Solutions A and B were added to the dispersion of MIL-77, stirred at room temperature for 2 h, and the purple product was collected by centrifugation and washing, which was MIL-77@ZIF-67.
[0101] (3) Synthesis of MIL-77@ZIF-67-PA (PA: phytic acid) hollow structure composite material: 50 mg of MIL-77@ZIF-67 was dispersed in 50 mL of ethanol, 10 mL of phytic acid ethanol solution was added, stirred for 1 h, centrifuged and washed, and dried in a vacuum oven for 12 h to obtain a lavender powder, which is the MIL-77@ZIF-67-PA hollow nanomaterial. The synthesized MIL-77@ZIF-67-PA was irradiated in an electron beam accelerator with an irradiation dose of 840 kGy. The irradiated MIL-77@ZIF-67-PA is abbreviated as MIL-77@ZIF-67-PA-840 kGy.
[0102] Figure 1-4 These are the characterization results of the composite materials of Examples 1-6 of the present invention.
[0103] Figure 1 Scanning transmission images of samples obtained at different stages in Examples 1-6 of the present invention are presented: (a) MIL-77; (b) MIL-77@ZIF-67; (c, d) MIL-77@ZIF-67-PA hollow composite structure. As can be seen from the figure: MIL-77 presents a two-dimensional nanobelt structure (Figure a), with a length of micrometers and a width of nanometers. Using polyvinyl pyrrolidone (PVP) as an adsorbent, Co 2+Ions are adsorbed on the surface of MIL-77, and 2-MIM ligands are added to make ZIF-67 nucleate and grow on the surface of MIL-77. The results show that ZIF-67 presents a dodecahedral morphology, with a smooth and flat surface, uniform size, and an average diameter of about 500nm (Figure b). It can be seen that there is very little exposed MIL-77, which proves the successful preparation of MIL-77@ZIF-67. The scanning and transmission electron microscopy images of MIL-77@ZIF-67-PA obtained after phytic acid (PA) exchange etching are shown in Figures c and d, respectively. It can be seen that the surface of the material changes from smooth to rough, and each face of the dodecahedron shows a certain degree of deformation, but the overall morphology and structure of the composite skeleton remain intact, and the size has basically not changed. During the phytic acid etching process, the composite structure MIL-77@ZIF-67 and phytic acid (C6H 18 O 24 P6,pK a =1.8) the proton H released + Ligand exchange is carried out to generate Ni ions and Co ions. The two cations react with the phytic acid anion (C6H 12 O 24 P6 6- ) cross-linked, and finally formed an organic complex cross-linked by metal ions and phytic acid, namely MIL-77@ZIF-67-PA. By controlling the reaction conditions, phytic acid as an etchant neither destroyed the extremely thin MIL-77 inside, and at the same time the dodecahedral structure of ZIF-67 was basically maintained, forming a hollow structure MIL-77@ZIF-67-PA.
[0104] Figure 2 Fourier transform infrared images of the MIL-77@ZIF-67-PA hollow composite structure obtained by the present invention after different irradiation doses. After electron beam irradiation, the OH bond position shifts to 3400 cm -1 Nearby, indicating that the sample is easy to absorb water in the air after electron beam irradiation. -1 Nearby, small peaks appeared at the positions of R-CH2OH and CH2=CH, 530cm -1 Nearby, the Co-O / Ni-O bond gradually shifts to the left at a small angle as the irradiation dose increases, indicating that electron beam irradiation can change the arrangement of the surface electronic state, and the positive charge on the surface of the material increases after irradiation. -1 The C=O bond peaks and positions on the left and right sides change slightly, which may be due to the change in particle size caused by electron beam irradiation. Therefore, the irradiation dose will change the electronic structure and arrangement of active sites on the surface of the material. After electron beam irradiation, the increase in positive charge on the surface of the material is conducive to the adsorption of OH during the electrocatalytic decomposition of water and oxygen evolution reaction (OER). -, improving the HER (hydrogen evolution reaction) catalytic activity; at the same time, the change in electronic structure will cause the atoms on the surface of the material to rearrange, increasing the degree of material defects and the number of catalytic active sites.
[0105] Figure 3 The electrochemical hydrogen evolution reaction performance of MIL-77@ZIF-67-PA after irradiation at different doses obtained by the implementation of the present invention is presented: (a) polarization curve; (b) Tafel slope curve; (c) double layer capacitance curve; (d) electrochemical impedance spectrum. It can be seen from the figure that the catalytic activity of the hydrogen evolution reaction obtained after different irradiation doses were tested in an alkaline environment of 1M KOH. It can be seen from the linear sweep voltammetric curve of Figure a that the irradiated MIL-77@ZIF-67-PA does not necessarily improve the catalytic performance. On the contrary, it shows a change pattern that the overpotential first increases and then gradually decreases during the gradual increase in the dose, that is, the catalytic activity of the hydrogen evolution reaction first deteriorates and then gradually improves. When the irradiation dose is 70kGy, the overpotential of the material is 210mV, which is much higher than that of the unirradiated MIL-77@ZIF-67-PA (0kGy). Compared with other irradiation doses of 70kGy, 140kGy, 280kGy and 840kGy, the material under the irradiation dose of 560kGy has the lowest overpotential of 162mV, which is significantly lower than the material with 0kGy. Because the unirradiated (0kGy) material may be in an amorphous organic complex state, when the irradiation dose is small, the light element atoms first move their positions, forming a defect repair phenomenon, which reduces the efficiency of electron transfer. When the irradiation dose is gradually increased, the probability and number of defects generated by electron beam irradiation gradually increase, and the new electron distribution structure begins to be reconstructed. The corresponding Tafel curve is shown in Figure b. It can be seen that the material irradiated at 560kGy has a good Tafel slope of 86.13mVdec -1 Compared with materials irradiated at other doses, it has better reaction kinetics and hydrogen evolution catalytic activity. Figure c shows its double layer capacitance curve, which shows that the irradiated material has a larger C than the unirradiated material. dl value. Because C dl The value is linearly proportional to the electrochemical active area. It can be seen that the irradiated material has a larger catalytic active area and more exposed electrochemical active sites. This electron irradiation modification has both advantages and disadvantages. It can increase the number of catalytic active sites, increase the active specific surface area, and change the electronic structure to improve the HER catalytic activity. However, it may also affect the optical or electrical properties of the material. Figure d shows its electrochemical impedance spectrum, and it can be seen that irradiation affects the charge transfer resistance (R ct ) size. After irradiation with a dose of 70 kGy, the material's R ctThe maximum value also proves that this is the process of defect repair and the electron transfer efficiency becomes low. After 560kGy irradiation, the material has the smallest charge transfer resistance. This shows that under alkaline conditions, the charge transfer efficiency between the MIL-77@ZIF-67-PA-560kGy catalyst and the electrolyte solution is the highest, and the electrocatalytic decomposition of water to produce hydrogen is the best.
[0106] Figure 4 The electrochemical oxygen evolution reaction performance of MIL-77@ZIF-67-PA after irradiation with different doses obtained by the present invention is presented: (a) polarization curve; (b) Tafel slope curve; (c) double layer capacitance curve; (d) electrochemical impedance spectrum. In order to explore the electrochemical oxygen evolution performance of the electron beam irradiated modified catalyst under alkaline conditions, the electrochemical performance of the samples irradiated with different irradiation doses and the unirradiated samples were tested in a standard three-electrode system. From the linear voltammetric curve of Figure a, it can be seen that due to Ni 2+ and Ni 3+ Due to the redox reaction, an obvious oxidation peak appears at about 1.4 V vs. RHE. To avoid the influence of the oxidation peak, a current density of 15 mA cm -2 The overpotential (η 15 ) as the standard for comparison of oxygen evolution catalytic performance. Relatively speaking, the material irradiated at 560kGy has better performance, reaching 15mAcm at an overpotential of 281mV. -2 The current density of MIL-77@ZIF-67-PA-0kGy (287mV), 70kGy (294mV), 140kGy (303mV), 280kGy (301mV) and 840kGy (311mV) requires higher overpotentials. The corresponding Tafel slope curve b shows that the Tafel slope of MIL-77@ZIF-67-PA-560kGy is the smallest at 86.56mV dec. -1 , indicating that the material has better oxygen evolution reaction kinetics after 560kGy irradiation. MIL-77@ZIF-67-PA itself has a hollow core-shell structure with a large number of active sites. When the irradiation dose gradually increases, defect sites are generated in the material, increasing the number of exposed active sites and allowing the catalyst to fully contact the electrolyte, which is conducive to the escape of oxygen. The positive charge distributed on its surface increases, and the catalyst material is easy to adsorb OH during the oxygen evolution reaction. - The OER catalytic activity was improved, indicating that MIL-77@ZIF-67-PA-560kGy is an excellent oxygen evolution reaction catalyst with a small overpotential and Tafel slope.
[0107] In summary, in the hydrogen evolution reaction test in 1 M KOH solution, MIL-77@ZIF-67-PA-560kGy can reach 10 mA cm with an overpotential of only 162 mV. -2 In the oxygen evolution reaction test, MIL-77@ZIF-67-PA-560kGy can reach 15mA cm with an overpotential of only 281mV. -2 The current density of 560 kGy irradiation proves that the material has excellent electrocatalytic activity and stability. This provides a new idea for the design and modification of electrocatalyst materials in the future.
[0108] The specific embodiments of the present invention are described in detail above, but they are only examples, and the present invention is not limited to the specific embodiments described above. For those skilled in the art, any equivalent modifications and substitutions made to the present invention are also within the scope of the present invention. Therefore, the equalization changes and modifications made without departing from the spirit and scope of the present invention should be included in the scope of the present invention.
Claims
1. A method for preparing a composite material of MIL-77 and ZIF-67-PA, characterized in that the steps include: Provides MIL-77; Mixing MIL-77 and a dispersant in a first solvent to obtain a first solution; Adding cobalt salt and dimethylimidazole to the first solution, mixing and reacting, to obtain MIL-77@ZIF-67; MIL-77@ZIF-67 and phytic acid are mixed in a second solvent to obtain MIL-77@ZIF-67-PA, that is, the composite material of MIL-77 and ZIF-67-PA.
2. The preparation method according to claim 1, characterized in that: MIL-77@ZIF-67-PA was also irradiated under electron beam.
3. The preparation method according to claim 2, characterized in that: The dose of the electron beam is 50-1500 kGy, preferably 60-1200 kGy, more preferably 70-1000 kGy; preferably, The preset dose of the electron beam is selected from one or more of 70 kGy, 140 kGy, 280 kGy, 560 kGy, and 840 kGy.
4. The preparation method according to claim 1, characterized in that: The synthesis method of MIL-77 comprises the following steps: Glutaric acid and nickel salt are mixed and reacted under alkaline conditions to obtain MIL-77.
5. The preparation method according to claim 4, characterized in that: The reaction temperature of the glutaric acid and the nickel salt is 100-300°C, preferably 120-280°C, more preferably 150-180°C; and / or The reaction time of the glutaric acid and the nickel salt is 3-64h, preferably 12-50h, and more preferably 24-48h.
6. The preparation method according to claim 1, characterized in that: In the first solution, the concentration of MIL-77 is 0.1-1 g / L, preferably 0.15-0.4 g / L, more preferably 0.2-0.3 g / L; and / or In the first solution, the concentration of the dispersant is 6-20 g / L, preferably 8-15 g / L, and more preferably 10-12 g / L.
7. The preparation method according to claim 1, characterized in that: Before the cobalt salt and dimethylimidazole are added to the first solution, the cobalt salt and dimethylimidazole may be mixed in a third solvent to obtain a second solution; preferably, The first solution and the second solution are mixed and reacted to obtain MIL-77@ZIF-67.
8. The preparation method according to claim 1, characterized in that: Before the cobalt salt and dimethylimidazole are added to the first solution, the cobalt salt can be added to the third solvent and mixed to obtain a cobalt salt solution; adding dimethylimidazole to the third solvent and mixing to obtain a dimethylimidazole solution; The cobalt salt solution and the dimethylimidazole solution are added to the first solution for mixing and reaction to obtain MIL-77@ZIF-67.
9. A MIL-77 and ZIF-67-PA composite material, characterized in that: Obtained based on the preparation method according to any one of claims 1 to 8.
10. An application of a MIL-77 and ZIF-67-PA composite material, characterized in that: The composite material is used as an electrolytic catalytic material or an electrolytic electrode.