Preparation method of polyacrylonitrile-based precursor and polyacrylonitrile-based carbon fiber
By controlling the specific viscosity of the polymerization liquid in the production of carbon fiber, the quality of the polyacrylonitrile-based raw wire is improved, and the tensile strength of carbon fiber is improved, the problem of insufficient strength of carbon fiber is solved, and the product quality and market competitiveness are improved.
Patent Information
- Application Number
- CN202411417987.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-11
- Publication Date
- 2024-12-06
AI Technical Summary
In the process of carbon fiber production, how to improve the tensile strength of carbon fiber has become a key issue affecting the quality and market competitiveness of carbon fibers.
By controlling the specific viscosity of the polymerization liquid in the first polymerization kettle within a preset range, the mass of the polyacrylonitrile-based raw wire is ensured, thereby improving the tensile strength of the prepared polyacrylonitrile-based carbon fiber. The specific steps include mixing and stirring monomers such as acrylonitrile, controlling the reaction temperature, filtration and deselecting the single-staining process, and then coagulation, washing, thermal pulling, drying and steam drawing, and finally setting the polyacrylonitrile-based raw wire. Carbon fibers are prepared by preoxidation, low-temperature carbonization and high-temperature carbonization processes.
It effectively improves the tensile strength of polyacrylonitrile-based carbon fiber, improves product quality, and enhances market competitiveness.
Smart Images

Figure CN119082910A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of carbon fiber, and specifically relates to a method for preparing a polyacrylonitrile-based precursor and a polyacrylonitrile-based carbon fiber. Background Art
[0002] Carbon fiber is a special fiber with a carbon content greater than 90% that is made from polyacrylonitrile (PAN), asphalt, viscose fiber, etc. through a pre-oxidation and carbonization process. Carbon fiber has excellent properties such as high strength, high modulus, low density, high temperature resistance, corrosion resistance, abrasion resistance, electrical conductivity, thermal conductivity, small expansion coefficient, and shock absorption. It is an indispensable engineering material in the aerospace and other industries. It not only has the inherent characteristics of carbon materials, but also has the softness and processability of textile fibers. It is a new generation of reinforcing fiber.
[0003] In the carbon fiber production process, the carbon fiber produced with acrylonitrile as raw material has a simple process, good comprehensive product performance, rapid development, and an output of more than 90%, becoming the most important raw material for carbon fiber production. The production process of polyacrylonitrile-based carbon fiber is as follows: a certain proportion of acrylonitrile, comonomer and solvent are mixed and stirred, an initiator is added, and the reaction temperature is controlled to allow the monomer to undergo solution polymerization. The obtained polymer solution is filtered, de-singled and de-aerated to form a polyacrylonitrile-based spinning solution with suitable viscosity. The spinning solution is then washed, stretched, dried, and shaped to form a polyacrylonitrile-based precursor. The polyacrylonitrile-based precursor is pre-oxidized and carbonized to finally be made into a carbon fiber with a two-dimensional chaotic graphite structure. Polyacrylonitrile-based carbon fiber is mainly used as a composite material reinforcement. Its specific gravity is less than 1 / 4 of that of steel, and its tensile strength is generally above 3500Mpa, which can effectively reduce the weight of the product. The higher the strength, the smaller the weight of the product, and the wider the application prospects. Therefore, in recent years, polyacrylonitrile-based carbon fiber has been widely developed as a raw material in the defense and civilian fields; but in production, how to improve the tensile strength of carbon fiber has become a key point affecting the quality of carbon fiber and improving market competitiveness. Summary of the invention
[0004] In order to solve the above problems existing in the prior art, the present invention provides a method for preparing polyacrylonitrile-based precursor and polyacrylonitrile-based carbon fiber.
[0005] The technical problem to be solved by the present invention is achieved through the following technical solutions:
[0006] The present invention provides a method for preparing polyacrylonitrile-based precursor, comprising:
[0007] S1, adding a plurality of monomers including acrylonitrile into a batching kettle, stirring and mixing, and obtaining a mixed solution;
[0008] S2, adding the mixed solution into a first polymerization kettle, and preparing a first polymerization solution having a specific viscosity within a preset specific viscosity range in the first polymerization kettle;
[0009] S3, continuing to subject the first polymerization liquid to polymerization reaction to obtain a second polymerization liquid;
[0010] S4, filtering and removing the monomers from the second polymerization liquid to obtain a polyacrylonitrile-based polymerization liquid;
[0011] S5. Perform a series of treatments on the polyacrylonitrile-based polymer solution to shape the polyacrylonitrile-based polymer solution and obtain polyacrylonitrile-based precursor fibers; wherein, within the preset specific viscosity range, the mass of the polyacrylonitrile-based precursor fibers is proportional to the specific viscosity of the first polymer solution.
[0012] The present invention also provides a method for preparing polyacrylonitrile-based carbon fiber, comprising:
[0013] Obtaining polyacrylonitrile-based precursor yarn prepared by the above-mentioned method for preparing polyacrylonitrile-based precursor yarn;
[0014] The polyacrylonitrile-based precursor is processed to obtain polyacrylonitrile-based carbon fibers.
[0015] Compared with the prior art, the present invention has the following beneficial effects:
[0016] When preparing polyacrylonitrile-based precursor fibers, the present invention can improve the quality of the prepared polyacrylonitrile-based precursor fibers by controlling the specific viscosity of the polymerization solution obtained in the first polymerization reactor during the preparation process within a preset specific viscosity range, thereby improving the tensile strength of the polyacrylonitrile-based carbon fibers prepared using the polyacrylonitrile-based precursor fibers.
[0017] The present invention will be further described in detail below with reference to the accompanying drawings and specific implementation methods. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 It is a schematic flow chart of a method for preparing a polyacrylonitrile-based precursor provided by an embodiment of the present invention;
[0019] Figure 2 is a schematic diagram of a method for preparing polyacrylonitrile-based carbon fiber provided in an embodiment of the present invention;
[0020] Figure 3 is a schematic diagram of the relationship between an exemplary solid content in one kettle and the tensile strength of carbon fiber provided in an embodiment of the present invention;
[0021] Figure 4 is a schematic diagram of the relationship between an exemplary one-pot specific viscosity and the tensile strength of carbon fiber provided in an embodiment of the present invention;
[0022] Figure 5is a schematic diagram of the relationship between an exemplary one-pot viscosity and the tensile strength of carbon fiber provided in an embodiment of the present invention;
[0023] Figure 6 is a schematic diagram of the relationship between the solid content of carbon fiber and the tensile strength of carbon fiber provided by an exemplary embodiment of the present invention;
[0024] Figure 7 is a schematic diagram of the relationship between an exemplary stripping viscosity and a tensile strength of a carbon fiber provided in an embodiment of the present invention;
[0025] Figure 8 is a schematic diagram of the relationship between an exemplary single-filament breaking elongation and a carbon fiber tensile strength provided by an embodiment of the present invention;
[0026] Fig. 9 is a schematic diagram of the relationship between the illustrative single filament strength and the tensile strength of the carbon fiber provided in an embodiment of the present invention;
[0027] Fig.10 It is a schematic diagram of the relationship between the illustrative single-filament modulus and the tensile strength of carbon fiber provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0028] The present invention is further described in detail below with reference to specific embodiments, but the embodiments of the present invention are not limited thereto.
[0029] In the production process, the quality of carbon fiber is closely related to the quality of precursor. Whether the tensile strength of carbon fiber is directly related to the process parameters of the precursor and how to control it in production have become the difficult problems that have been overcome in the production process of carbon fiber. The inventor of the present invention has found through his own research that in the production process of carbon fiber, the tensile strength of carbon fiber is closely related to the process parameter of the precursor - the viscosity of one kettle (i.e. the viscosity of the polymer solution prepared in the first polymerization kettle). Based on this discovery, a method for preparing a polyacrylonitrile-based precursor and a polyacrylonitrile-based carbon fiber is provided to improve the tensile strength of the prepared polyacrylonitrile-based carbon fiber.
[0030] Figure 1 is a schematic diagram of a process for preparing a polyacrylonitrile-based precursor provided by an embodiment of the present invention, such as Figure 1 As shown, the method includes:
[0031] S1. Add various monomers including acrylonitrile into a batching kettle, stir and mix, and obtain a mixed solution.
[0032] S2. Add the mixed solution into a first polymerization kettle, and prepare a first polymerization solution having a specific viscosity within a preset specific viscosity range in the first polymerization kettle.
[0033] S3, continuing to subject the first polymerization liquid to polymerization reaction to obtain a second polymerization liquid.
[0034] S4, filtering and removing the monomers from the second polymerization liquid to obtain a polyacrylonitrile-based polymerization liquid.
[0035] S5. Perform a series of treatments on the polyacrylonitrile-based polymer solution to shape the polyacrylonitrile-based polymer solution to obtain polyacrylonitrile-based precursor fibers; wherein, within a preset specific viscosity range, the mass of the polyacrylonitrile-based precursor fibers is proportional to the specific viscosity of the first polymer solution.
[0036] The specific viscosity mentioned in the present invention refers to the ratio of the viscosity of the polymer solution to the viscosity of the solvent, which reflects the internal friction effect between polymers and between pure solvents and polymers; the specific viscosity is related to the concentration of the solution and increases with the increase of the concentration of the solution.
[0037] Different from the specific viscosity described in the present invention, the intrinsic viscosity refers to the ratio of the viscosity of a polymer solution to the concentration of the solution. It reflects the internal friction between the polymer and the solvent molecules. The intrinsic viscosity has nothing to do with the concentration of the solution, but is only related to the properties of the polymer itself.
[0038] Here, the polyacrylonitrile-based precursor is an intermediate product in the production process. The quality of the precursor is closely related to the quality of the carbon fiber. Within the above-mentioned preset specific viscosity range, the performance parameters of the precursor do not change much, but the micropore morphology of the fiber cross section has changed, the micropores inside the precursor have all disappeared, and the structure is relatively dense; after the precursor is carbonized, the tensile strength of the polyacrylonitrile-based carbon fiber obtained is relatively high. Therefore, the density of the polyacrylonitrile-based precursor is proportional to the specific viscosity of the first polymerization solution prepared in the first polymerization kettle.
[0039] In some embodiments, S1 specifically includes: adding monomers acrylonitrile, itaconic acid, azobisisobutyronitrile, dimethyl sulfoxide, 2-acrylamide 2-methylpropanesulfonic acid and ammonia water into a batching kettle whose temperature is within a first temperature range, stirring and mixing to obtain a mixed solution.
[0040] Here, in the mixed solution, the weight ratio of the monomers acrylonitrile, itaconic acid, azobisisobutyronitrile, dimethyl sulfoxide, 2-acrylamide 2-methylpropanesulfonic acid, and ammonia water is: 451-461: 6-8: 4-6: 1598-1608: 2-4: 0.5-1.5.
[0041] For example, in the mixed solution, the weight ratio of the monomers acrylonitrile, itaconic acid, azobisisobutyronitrile, dimethyl sulfoxide, 2-acrylamide 2-methylpropanesulfonic acid, and ammonia water is: 456:7:5:1603:3:1. For example, the mass percentage of AN to the total weight is 22%.
[0042] Here, the purpose of setting the temperature of the batching kettle to the first temperature range is to prevent the monomers in the batching kettle from undergoing polymerization reaction. Exemplarily, the first temperature range is 0-15°C.
[0043] Here, the batching kettle has a jacket, and the temperature in the batching kettle can be adjusted to the first temperature range by introducing a liquid at a certain temperature into the jacket of the batching kettle. For example, water at 7° C. can be introduced into the jacket of the batching kettle.
[0044] In some embodiments, S2 specifically includes: adding the mixed liquid into a first polymerization kettle, controlling the reaction temperature in the first polymerization kettle, and controlling the reaction rate between the monomers in the first polymerization kettle to prepare a first polymerization liquid with a specific viscosity within a preset specific viscosity range in the first polymerization kettle.
[0045] Similarly, the first polymerization kettle is provided with a jacket, and the temperature in the first polymerization kettle can be controlled by introducing a liquid of a certain temperature and a certain flow rate into the jacket of the first polymerization kettle.
[0046] Exemplarily, the reaction temperature in the first polymerization reactor is 60-65°C.
[0047] In some embodiments, the preset specific viscosity range is 1.1 to 1.3 nsp. Exemplarily, the preset specific viscosity range can also be 1.20 to 1.25 nsp, so that the quality of the prepared polyacrylonitrile-based precursor is higher, so that the tensile strength of the finally prepared polyacrylonitrile-based carbon fiber is higher. nsp represents the specific viscosity, which is used to reflect the internal friction effect between polymer molecules and solvent molecules and between polymer molecules.
[0048] In some embodiments, S3 specifically includes:
[0049] S31, adding the first polymerization liquid into a second polymerization kettle whose temperature is within a second temperature range, so that the monomers in the first polymerization liquid continue to undergo polymerization reaction in the second polymerization kettle to obtain an intermediate polymerization liquid.
[0050] S32, adding the intermediate polymerization liquid into a third polymerization kettle whose temperature is within a third temperature range, so that the monomers in the intermediate polymerization liquid continue to undergo polymerization reaction in the third polymerization kettle to obtain a second polymerization liquid.
[0051] Similarly, the second and third polymerization kettles are both provided with jackets, and the temperatures in the second and third polymerization kettles can be controlled respectively by introducing a liquid of a certain temperature and a certain flow rate into the jackets of the second and third polymerization kettles.
[0052] Exemplarily, the second temperature range may be: (59.0±1.0)°C.
[0053] Exemplarily, the third temperature range may be: (59.0±1.0)°C.
[0054] In some embodiments, S4 specifically includes: filtering and degassing the second polymerization liquid in sequence to remove impurities and unreacted monomers in the polymerization liquid to obtain a polyacrylonitrile-based polymerization liquid.
[0055] Specifically, the specific steps of S4 are: the polymerization liquid coming out of the third polymerization kettle is pumped into the first plate-frame filter by a diaphragm pump for filtration, the temperature of the first plate-frame filter is controlled at (58.0±1.0)°C, and 53 filter cloths with a filtration accuracy of 2um are installed in the filter to remove impurities in the polymerization liquid and gel generated during the reaction; the polymerization liquid after the first filtration is pumped into a thin film evaporator by a diaphragm pump, the temperature of the thin film evaporator is controlled at (55.0±3.0)°C, the frequency of the liquid ring vacuum pump is controlled at (50-60)Hz, and the gas and unreacted monomers in the polymerization liquid are removed under vacuum; the polymerization liquid after degassing and deaeration is pumped into the second plate-frame filter by a pump for filtration, the temperature of the second plate-frame filter is controlled at (58.0±1.0)°C, and 51 filter cloths with a filtration accuracy of 2um are installed in the filter to remove impurities in the polymerization liquid and gel generated during the reaction again. After degassing, deaeration and filtration, a polyacrylonitrile-based polymerization liquid with a high viscosity is obtained.
[0056] In some embodiments, S5 specifically includes: subjecting the polyacrylonitrile-based polymer solution to coagulation, water washing, hot drawing, drying, steam drawing, and steam setting steps in sequence to obtain the polyacrylonitrile-based raw yarn.
[0057] Specifically, the specific steps of S5 are: the polyacrylonitrile-based polymer solution is ejected through spinnerets of different specifications, and then through two coagulation processes, double diffusion is carried out with solutions of different concentrations in the coagulation bath, and physical changes such as mass transfer, heat transfer and phase separation occur, thereby forming primary fibers with a gel structure; the primary fibers are subjected to ten water washing processes, and double diffusion is carried out with pure water again to wash away the residual DMSO in the fibers and eliminate the destructive effect of DMSO on the fibers; after a hot water drawing process, the molecular segments of the PAN-based fibers are moved, so that the macromolecular chains are oriented along the fiber axis; after a drying process, the moisture in the fibers is removed, the holes are closed to achieve a densification effect, thereby eliminating the structural unevenness caused by double diffusion during the spinning and coagulation process, as well as the holes and crack structures generated, and eliminating the fiber devitrification phenomenon; after a steam drawing process, the orientation degree, density and mechanical properties of the fibers are improved, and finally after a steam setting process, the residual stress formed inside the fibers during the stretching process is eliminated, the fiber shape is maintained, and finally the polyacrylonitrile-based precursor is obtained.
[0058] The present invention also provides a method for preparing polyacrylonitrile-based carbon fiber, such as Figure 2 As shown, the method includes:
[0059] S201, obtaining polyacrylonitrile-based precursor fibers; wherein, during the process of preparing the polyacrylonitrile-based precursor fibers, the specific viscosity of the first polymerization liquid in the first polymerization kettle is within a preset specific viscosity range.
[0060] Here, the polyacrylonitrile-based precursor is prepared by the above-mentioned method for preparing the polyacrylonitrile-based precursor. In some embodiments, the preset specific viscosity range is 1.1 to 1.3 nsp. Exemplarily, the preset specific viscosity range can also be 1.20 to 1.25 nsp, so that the quality of the prepared polyacrylonitrile-based precursor is higher, so that the tensile strength of the finally prepared polyacrylonitrile-based carbon fiber is higher.
[0061] S202, processing the polyacrylonitrile-based precursor to obtain polyacrylonitrile-based carbon fiber.
[0062] Specifically, the polyacrylonitrile-based polymer solution may be subjected to pre-oxidation, low-temperature carbonization, high-temperature carbonization, and post-treatment steps in sequence to obtain the polyacrylonitrile-based carbon fiber.
[0063] Here, within the preset specific viscosity range, the specific viscosity is proportional to the tensile strength of the polyacrylonitrile-based carbon fiber.
[0064] In order to further verify the technical effect of the present invention, several experiments are provided below:
[0065] Experiment 1:
[0066] 1) Add monomers acrylonitrile, itaconic acid, azobisisobutyronitrile, dimethyl sulfoxide, and 2-acrylamide 2-methylpropanesulfonic acid into a batching kettle in a certain proportion and stir and mix. Pass 7°C chilled water into the jacket of the batching kettle to ensure that the temperature in the batching kettle is ≤15°C to prevent polymerization reaction between various monomers.
[0067] 2) The uniformly stirred mixed liquid is pumped into the first polymerization kettle, the flow rate of hot water in the polymerization kettle jacket is controlled to be 1500L / h, and the reaction temperature in the polymerization kettle is controlled to be 61.0°C, thereby controlling the reaction rate of the monomer in the first polymerization kettle. Afterwards, the solid content, specific viscosity and viscosity of the polymerization liquid are tested. The test results are: the average solid content is 16.77%, the average specific viscosity (i.e. the average value of all specific viscosity values) is 1.168nsp, and the average viscosity is 120p.
[0068] 3) The polymerization liquid was passed through the second and third polymerization kettles in sequence, the flow rate of circulating water in the jacket of the polymerization kettle was controlled to be 100 L / h, and the reaction temperature in the polymerization kettle was controlled to be 59.0 L / h.
[0069] 4) The polymer solution is filtered, degassed and demonstrated to remove impurities and unreacted monomers. After that, the solid content and viscosity of the polymer solution after demonstrating are tested. The test results are as follows: the average solid content is 21.61%, and the average specific viscosity is 472p.
[0070] 5) The polyacrylonitrile-based polymer solution is sequentially subjected to coagulation, water washing, hot drawing, drying, steam drawing, and steam setting processes to obtain polyacrylonitrile-based precursor yarn. Thereafter, the mechanical properties of the precursor yarn are tested, and the test results are as follows: the average elongation at break of the single yarn is 13.6%, the average strength of the single yarn is 6.5 cN / dtex, and the average modulus of the single yarn is 118.9 cN / dtex.
[0071] 6) The polyacrylonitrile-based precursor is subjected to pre-oxidation, low-temperature carbonization, high-temperature carbonization, and post-treatment steps in sequence to obtain polyacrylonitrile-based carbon fibers. The pre-oxidation temperature is set as follows: 1A, 1B: 215°C, 2A, 2B: 236°C, 3A, 3B: 253°C, 4A, 4B: 269°C;
[0072] 7) The tensile strength of carbon fiber was tested, and the average tensile strength of carbon fiber was 3852 MPa.
[0073] Experiment 2:
[0074] 1) Add monomers acrylonitrile, itaconic acid, azobisisobutyronitrile, dimethyl sulfoxide, and 2-acrylamide 2-methylpropanesulfonic acid into a batching kettle in a certain proportion and stir and mix. Pass 7°C chilled water into the jacket of the batching kettle to ensure that the temperature in the batching kettle is ≤15°C to prevent polymerization reaction between various monomers.
[0075] 2) The uniformly stirred mixed liquid is pumped into the first polymerization kettle, the flow rate of hot water in the polymerization kettle jacket is controlled to 1400L / h, and the reaction temperature in the polymerization kettle is controlled to 61.5°C, thereby controlling the reaction rate of the monomer in the first polymerization kettle. Afterwards, the solid content, specific viscosity and viscosity of the polymerization liquid are tested. The test results are: the average solid content is 16.95%, the average specific viscosity is 1.259nsp, and the average viscosity is 105p.
[0076] 3) The polymerization liquid was passed through the second and third polymerization kettles in sequence, the flow rate of circulating water in the jacket of the polymerization kettle was controlled to be 100 L / h, and the reaction temperature in the polymerization kettle was controlled to be 59.5 L / h.
[0077] 4) The polymer solution is filtered, degassed and demonstrated to remove impurities and unreacted monomers. After that, the solid content and viscosity of the polymer solution after demonstrating are tested. The test results are as follows: the average solid content is 21.50%, and the average viscosity is 441p.
[0078] 5) The polyacrylonitrile-based polymer solution is sequentially subjected to coagulation, water washing, hot drawing, drying, steam drawing, and steam setting processes to obtain polyacrylonitrile-based precursor yarn. Thereafter, the mechanical properties of the precursor yarn are tested, and the test results are as follows: the average elongation at break of the single yarn is 12.5%, the average strength of the single yarn is 6.3 cN / dtex, and the average modulus of the single yarn is 107.8 cN / dtex.
[0079] 6) The polyacrylonitrile-based precursor is sequentially subjected to pre-oxidation, low-temperature carbonization, high-temperature carbonization, and post-treatment steps to obtain polyacrylonitrile-based carbon fibers.
[0080] 7) The tensile strength of carbon fiber was tested, and the average tensile strength of carbon fiber was 4226 MPa.
[0081] Experiment 3:
[0082] 1) Add monomers acrylonitrile, itaconic acid, azobisisobutyronitrile, dimethyl sulfoxide, and 2-acrylamide 2-methylpropanesulfonic acid into a batching kettle in a certain proportion and stir and mix. Pass 7°C chilled water into the jacket of the batching kettle to ensure that the temperature in the batching kettle is ≤15°C to prevent polymerization reaction between various monomers.
[0083] 2) The uniformly stirred mixed liquid was pumped into the first polymerization kettle, the flow rate of hot water in the polymerization kettle jacket was controlled to 1300 L / h, and the reaction temperature in the polymerization kettle was controlled to 61.7°C, thereby controlling the reaction rate of the monomers in the first polymerization kettle, and testing the solid content, specific viscosity and viscosity of the polymerization liquid. The test results were: the average solid content was 16.60%, the average specific viscosity was 1.148 nsp, and the average viscosity was 101p.
[0084] 3) The polymerization liquid was passed through the second and third polymerization kettles in sequence, the flow rate of circulating water in the jacket of the polymerization kettle was controlled to be 100 L / h, and the reaction temperature in the polymerization kettle was controlled to be 60.0 L / h.
[0085] 4) The polymer solution was filtered, degassed and demonstrated to remove impurities and unreacted monomers in the polymer solution. The solid content and viscosity of the polymer solution after demonstrating were tested. The test results were as follows: the average solid content was 21.45%, and the average viscosity was 427p.
[0086] 5) The polyacrylonitrile-based polymer solution is sequentially subjected to coagulation, water washing, hot drawing, drying, steam drawing, and steam setting processes to obtain polyacrylonitrile-based precursor yarn. Thereafter, the mechanical properties of the precursor yarn are tested, and the test results are as follows: the average elongation at break of the single yarn is 13.7%, the average strength of the single yarn is 6.4 cN / dtex, and the average modulus of the single yarn is 113.9 cN / dtex.
[0087] 6) The polyacrylonitrile-based precursor is sequentially subjected to the processes of pre-oxidation, low-temperature carbonization, high-temperature carbonization, and post-treatment to obtain polyacrylonitrile-based carbon fibers.
[0088] 7) The tensile strength of carbon fiber was tested and the average tensile strength of carbon fiber was found to be 3723 MPa.
[0089] Experiment 4:
[0090] 1) Add monomers acrylonitrile, itaconic acid, azobisisobutyronitrile, dimethyl sulfoxide, and 2-acrylamide 2-methylpropanesulfonic acid into a batching kettle in a certain proportion and stir and mix. Pass 7°C chilled water into the jacket of the batching kettle to ensure that the temperature in the batching kettle is ≤15°C to prevent polymerization reaction between various monomers.
[0091] 2) The uniformly stirred mixed liquid was pumped into the first polymerization kettle, the flow rate of hot water in the polymerization kettle jacket was controlled to 1600 L / h, and the reaction temperature in the polymerization kettle was controlled to 62.0°C, thereby controlling the reaction rate of the monomers in the first polymerization kettle. Afterwards, the solid content, specific viscosity and viscosity of the polymerization liquid were tested. The test results were: the average solid content was 15.73%, the average specific viscosity was 1.178 nsp, and the average viscosity was 99p.
[0092] 3) The polymerization liquid was passed through the second and third polymerization kettles in sequence, the flow rate of circulating water in the jacket of the polymerization kettle was controlled to be 100 L / h, and the reaction temperature in the polymerization kettle was controlled to be 60.5 L / h.
[0093] 4) The polymer solution was filtered, degassed and demonstrated to remove impurities and unreacted monomers in the polymer solution. The solid content and viscosity of the polymer solution after demonstrating were tested. The test results were as follows: the average solid content was 21.76%, and the average viscosity was 402p.
[0094] 5) The polyacrylonitrile-based polymer solution is sequentially subjected to coagulation, water washing, hot drawing, drying, steam drawing, and steam setting processes to obtain polyacrylonitrile-based precursor yarn. Thereafter, the mechanical properties of the precursor yarn single yarn are tested, and the test results are as follows: the average single yarn breaking elongation is 13.2%, the average single yarn strength is 6.2 cN / dtex, and the average single yarn modulus is 116.1 cN / dtex.
[0095] 6) The polyacrylonitrile-based precursor is sequentially subjected to the processes of pre-oxidation, low-temperature carbonization, high-temperature carbonization, and post-treatment to obtain polyacrylonitrile-based carbon fibers.
[0096] 7) The tensile strength of carbon fiber was tested and the average tensile strength of carbon fiber was 3960 MPa.
[0097] Experiment 5:
[0098] 1) Add monomers acrylonitrile, itaconic acid, azobisisobutyronitrile, dimethyl sulfoxide, and 2-acrylamide 2-methylpropanesulfonic acid into a batching kettle in a certain proportion and stir and mix. Pass 7°C chilled water into the jacket of the batching kettle to ensure that the temperature in the batching kettle is ≤15°C to prevent polymerization reaction between various monomers.
[0099] 2) The uniformly stirred mixed liquid is pumped into the first polymerization kettle, the flow rate of hot water in the polymerization kettle jacket is controlled to 1500L / h, and the reaction temperature in the polymerization kettle is controlled to 62.5°C, thereby controlling the reaction rate of the monomer in the first polymerization kettle. Afterwards, the solid content, specific viscosity and viscosity of the polymerization liquid are tested. The test results are: the average solid content is 16.55%, the average specific viscosity is 1.125nsp, and the average viscosity is 103p.
[0100] 3) The polymerization liquid was passed through the second and third polymerization kettles in sequence, the flow rate of the circulating water in the jacket of the polymerization kettle was controlled to be 95 L / h, and the reaction temperature in the polymerization kettle was controlled to be 59.5 L / h.
[0101] 4) The polymer solution was filtered, degassed and demonstrated to remove impurities and unreacted monomers in the polymer solution. The solid content and viscosity of the polymer solution after demonstrating were tested. The test results were as follows: the average solid content was 21.89%, and the average viscosity was 396p.
[0102] 5) The polyacrylonitrile-based polymer solution is sequentially subjected to coagulation, water washing, hot drawing, drying, steam drawing, and steam setting processes to obtain polyacrylonitrile-based precursor yarn. Afterwards, the mechanical properties of the precursor yarn are tested, and the test results are as follows: the average elongation at break of the single yarn is 12.6%, the average strength of the single yarn is 5.8 cN / dtex, and the average modulus of the single yarn is 119.6 cN / dtex.
[0103] 6) The polyacrylonitrile-based precursor is sequentially subjected to the processes of pre-oxidation, low-temperature carbonization, high-temperature carbonization, and post-treatment to obtain polyacrylonitrile-based carbon fibers.
[0104] 7) The tensile strength of carbon fiber was tested and the average tensile strength of carbon fiber was found to be 3680 MPa.
[0105] Result analysis:
[0106] The data of Experiments 1 to 5 above were statistically analyzed, as shown in Table 1 and Figures 3 to 10 As shown:
[0107] Table 1 Summary of process parameters of different schemes
[0108]
[0109] In the above Table 1, the solid content of one kettle represents the solid content of the polymerization solution prepared in the first polymerization kettle, the specific viscosity of one kettle represents the specific viscosity of the polymerization solution prepared in the first polymerization kettle, and the viscosity of one kettle represents the viscosity of the polymerization solution prepared in the first polymerization kettle. The debonding viscosity represents the solid content of the polymerization solution obtained after the degassing and debonding process, and the debonding viscosity represents the viscosity of the polymerization solution obtained after the degassing and debonding process. The single-filament breaking elongation represents the single-filament breaking elongation of the prepared polyacrylonitrile-based precursor, the single-filament strength represents the single-filament strength of the prepared polyacrylonitrile-based precursor, and the single-filament modulus represents the single-filament modulus of the prepared polyacrylonitrile-based precursor. The carbon fiber tensile strength represents the tensile strength of the carbon fiber prepared using the prepared polyacrylonitrile-based precursor.
[0110] Figure 3 It is a schematic diagram of the relationship between the solid content of a kettle and the tensile strength of carbon fiber; Figure 3 As shown, there is no direct relationship between the solid content in one pot and the tensile strength of carbon fiber. Figure 4 is a schematic diagram of the relationship between the specific viscosity of a kettle and the tensile strength of carbon fiber; Figure 4 As shown in the figure, the change trend of carbon fiber tensile strength is consistent with that of one-pot specific viscosity. Figure 5 is a schematic diagram of the relationship between the viscosity of a kettle and the tensile strength of carbon fiber; Figure 5 As shown, one-pot viscosity has no direct relationship with carbon fiber tensile strength. Figure 6 It is a schematic diagram of the relationship between the solid content of carbon fiber and the tensile strength of carbon fiber; Figure 6 As shown in the figure, there is no direct relationship between the solid content and the tensile strength of carbon fiber. Figure 7 It is a schematic diagram of the relationship between the stripping viscosity and the tensile strength of carbon fiber; Figure 7 As shown, there is no direct relationship between the debonding viscosity and the tensile strength of carbon fiber. Figure 8 is a schematic diagram of the relationship between the single-filament elongation at break and the tensile strength of carbon fiber; Figure 8 As shown, there is no direct relationship between the single filament elongation at break and the tensile strength of carbon fiber. Fig. 9 is a schematic diagram of the relationship between the single-filament strength and the tensile strength of the carbon fiber. Fig. 9 As shown, there is no direct relationship between the monofilament strength and the tensile strength of the carbon fiber. Fig.10 is a schematic diagram of the relationship between the single fiber modulus and the tensile strength of carbon fiber. Fig.10 As shown, there is no direct relationship between the single filament modulus and the tensile strength of carbon fiber.
[0111] According to the above experimental results, in the carbon fiber production process, the tensile strength of the carbon fiber is closely related to the raw yarn process parameter one-pot specific viscosity. With the increase of one-pot specific viscosity, the tensile strength of the carbon fiber gradually increases, but the specific viscosity cannot be increased infinitely. If the specific viscosity is too large, gel is likely to occur during the production process, the spinneret is blocked, and spinning is difficult. Moreover, when the one-pot specific viscosity is controlled at 1.20-1.25nsp, the production is stable, spinning is easy, and the raw yarn quality is good, so that the tensile strength performance of the carbon fiber can be high.
[0112] It should be noted that the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0113] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification.
[0114] In the specification, the word "comprising" does not exclude other components or steps, and "a" or "an" does not exclude a plurality of components. Certain measures are recorded in different embodiments, but this does not mean that these measures cannot be combined to produce good effects.
[0115] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the protection scope of the present invention.
Claims
1. A method for preparing polyacrylonitrile-based precursor, It is characterized in that include: S1, adding a plurality of monomers including acrylonitrile into a batching kettle, stirring and mixing, and obtaining a mixed solution; S2, adding the mixed solution into a first polymerization kettle, and preparing a first polymerization solution having a specific viscosity within a preset specific viscosity range in the first polymerization kettle; S3, continuing to subject the first polymerization liquid to polymerization reaction to obtain a second polymerization liquid; S4, filtering and removing the monomers from the second polymerization liquid to obtain a polyacrylonitrile-based polymerization liquid; S5. Perform a series of treatments on the polyacrylonitrile-based polymer solution to shape the polyacrylonitrile-based polymer solution and obtain polyacrylonitrile-based precursor fibers; wherein, within the preset specific viscosity range, the mass of the polyacrylonitrile-based precursor fibers is proportional to the specific viscosity of the first polymer solution.
2. The method for preparing the polyacrylonitrile-based precursor according to claim 1, It is characterized in that The S1 specifically includes: Add monomers of acrylonitrile, itaconic acid, azobisisobutyronitrile, dimethyl sulfoxide, 2-acrylamide 2-methylpropanesulfonic acid and ammonia water into a batching kettle whose temperature is within the first temperature range, stir and mix to obtain a mixed solution.
3. The method for preparing the polyacrylonitrile-based precursor according to claim 2, It is characterized in that The weight ratio of the monomer acrylonitrile, the itaconic acid, the azobisisobutyronitrile, the dimethyl sulfoxide, the 2-acrylamide 2-methylpropanesulfonic acid, and the ammonia water is: 451-461: 6-8: 4-6: 1598-1608: 2-4: 0.5-1.
5.
4. The method for preparing the polyacrylonitrile-based precursor according to claim 2, It is characterized in that The first temperature range is 0-15°C.
5. The method for preparing polyacrylonitrile-based precursor according to claim 1, It is characterized in that The S2 specifically includes: adding the mixed liquid into a first polymerization kettle, controlling the reaction temperature in the first polymerization kettle, and controlling the reaction rate between the monomers in the first polymerization kettle, so as to prepare a first polymerization liquid with a specific viscosity within a preset specific viscosity range in the first polymerization kettle.
6. The method for preparing polyacrylonitrile-based precursor according to claim 1, It is characterized in that The preset specific viscosity range is 1.1 to 1.3 nsp.
7. The method for preparing polyacrylonitrile-based precursor according to claim 5, It is characterized in that The reaction temperature in the first polymerization vessel is between 60 and 65°C.
8. The method for preparing polyacrylonitrile-based precursor according to claim 1, It is characterized in that The S3 specifically includes: S31, adding the first polymerization liquid into a second polymerization kettle whose temperature is within a second temperature range, so that the monomers in the first polymerization liquid continue to undergo polymerization reaction in the second polymerization kettle to obtain an intermediate polymerization liquid; S32, adding the intermediate polymerization liquid into a third polymerization kettle whose temperature is within a third temperature range, so that the monomers in the intermediate polymerization liquid continue to undergo polymerization reaction in the third polymerization kettle to obtain a second polymerization liquid.
9. The method for preparing polyacrylonitrile-based precursor according to claim 1, It is characterized in that The S5 specifically includes: subjecting the polyacrylonitrile-based polymer solution to coagulation, water washing, heat drawing, drying, steam drawing, and steam setting steps in sequence to obtain polyacrylonitrile-based raw fibers.
10. A method for preparing polyacrylonitrile-based carbon fiber, It is characterized in that include: Obtaining polyacrylonitrile-based precursor prepared by the method of any one of claims 1 to 9 above; The polyacrylonitrile-based precursor is processed to obtain polyacrylonitrile-based carbon fibers.